Residue soil curing agent and residue soil curing method
By using a specific proportion of metakaolin, solid alkali and silicate solutions as slag curing agents, the problem of poor curing strength of slag curing bodies is solved, the mechanical properties of slag are improved, and it is suitable as a groove backfiller and can be realized. Resource utilization and cost reduction.
Patent Information
- Application Number
- CN202411093544.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-15
AI Technical Summary
The curing strength of the existing slag curing agent after curing is poor, resulting in slag being unsuitable for use as a groove backfiller.
Metakaolin, solid alkali and silicate solutions with mass ratio of (11.01-12.08):1: (4.06-5.35) were used as slag curing agents. The mechanical properties of the curing body were significantly improved by stirring and mixing and curing molding.
The mechanical properties of the slag cured body are significantly improved, making it suitable for use as a groove backfiller, and resource utilization is realized, reducing engineering costs and environmental pollution.
Smart Images

Figure BDA0004987230290000101 
Figure BDA0004987230290000111
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of soil solidification, and in particular to a slag solidifying agent and a slag solidifying method. Background Art
[0002] At present, rail transit projects generate a large amount of slag, which occupies a large amount of land as receiving sites and landfills, resulting in a serious waste of land resources. Most of the construction slag is in a plastic flow state, and simple and rough landfilling can easily cause safety hazards.
[0003] In order to solve the above problems, the prior art adopts the method of solidification backfilling for reuse. For example, CN111393082A discloses a slag solidifying agent composed of the following components calculated by weight: 20-25 parts of large-particle slag; 10-30 parts of small-particle slag; 25-35 parts of cement; 10-15 parts of mineral waste; 5-8 parts of resin; 1-1.5 parts of water reducing agent; 2-3 parts of resin colloid protective agent; 0.7-1 part of water retaining agent; the mesh size of the large-particle slag is 20-25 parts; the mesh size of the large-particle slag is 20-30 ... The mesh size of the small-particle slag is 900-1200 meshes; the mesh size of the mineral waste is 600-1000 meshes; the resin is a mixture of one or more of the following substances: ternary copolymer rubber powder of ethylene, vinyl chloride and vinyl silicate, ternary copolymer rubber powder of vinyl acetate, ethylene and higher fatty acid vinyl ester, copolymer rubber powder of vinyl acetate and higher fatty acid vinyl ester, ternary copolymer rubber powder of vinyl acetate, acrylate and higher fatty acid vinyl ester.
[0004] CN115806417A discloses a construction slag solidifying agent and a preparation method thereof. The solidifying agent mainly uses silicate cement, desulfurization ash, industrial by-product gypsum, slag powder, dispersant, calcium carbonate doping agent and the like as raw materials. At the same time, solid wastes such as construction slag, desulfurization ash, industrial by-product gypsum, slag powder and the like are utilized on a large scale to improve the resource utilization level of solid wastes such as construction slag, desulfurization ash, industrial by-product gypsum, slag powder and the like.
[0005] However, the existing slag solidifying agent still has the problem of poor solidification strength after solidifying the slag, which is not conducive to using the slag as trench backfill. Summary of the invention
[0006] In view of the problems existing in the prior art, the purpose of the present invention is to provide a slag solidifying agent and a slag solidifying method to solve the problem that the solidified body obtained after the slag solidification still has poor solidification strength, which is not conducive to the use of the slag as trench backfill.
[0007] To achieve this object, the present invention adopts the following technical solutions:
[0008] In a first aspect, the present invention provides a slag solidifying agent, the slag solidifying agent comprising:
[0009] The mass ratio of kaolin, solid alkali and silicate solution is (11.01-12.08):1:(4.06-5.35).
[0010] The slag solidifying agent provided by the present invention can significantly improve the mechanical properties of the solidified body after the slag is solidified through the design of the composition of the slag solidifying agent, which is conducive to the use of the slag as trench backfill.
[0011] As a preferred technical solution of the present invention, the metakaolin includes coal-based metakaolin.
[0012] Preferably, the particle size of the metakaolin is 3-32 μm.
[0013] As a preferred technical solution of the present invention, the solid alkali includes sodium hydroxide and / or potassium hydroxide.
[0014] As a preferred technical solution of the present invention, the silicate solution includes a sodium silicate solution and / or a potassium silicate solution.
[0015] Preferably, the modulus of the silicate solution is 3-4.
[0016] Preferably, the mass concentration of the silicate solution is 34-35%.
[0017] In a second aspect, the present invention provides a method for solidifying slag, the solidification method comprising solidifying and shaping the slag using the slag solidifying agent described in the first aspect.
[0018] As a preferred technical solution of the present invention, the curing method comprises: preparing ingredients according to a mass ratio formula, and then mixing a solid alkali and a silicate solution to obtain a curing intermediate solution;
[0019] Kaolin, solidification intermediate liquid, calcium material and slag are stirred and mixed, and then cured and formed to obtain solidified slag.
[0020] As a preferred technical solution of the present invention, the mass ratio of kaolin and slag is (0.1-0.25):1;
[0021] Preferably, the mass ratio of the slag to the calcium material is (5-10):1.
[0022] As a preferred technical solution of the present invention, the stirring and mixing includes a first stirring and mixing and a second stirring and mixing performed sequentially;
[0023] Preferably, the stirring speed of the first stirring and mixing is less than the stirring speed of the second stirring and mixing.
[0024] As a preferred technical solution of the present invention, the stirring speed of the first stirring and mixing is 62-140r / min;
[0025] Preferably, the stirring time of the first stirring and mixing is 2-5 min.
[0026] As a preferred technical solution of the present invention, the stirring speed of the second stirring and mixing is 125-285r / min;
[0027] Preferably, the stirring time of the second stirring and mixing is 2-5 min.
[0028] Compared with the prior art solutions, the present invention has the following beneficial effects:
[0029] (1) The slag solidifying agent provided by the present invention is added to the slag and produces various chemical reactions under the action of water to generate gel-like hydrates, which surround the slag particles, enhance the bonding strength and stability between the soil particles, and make the distribution of the slag solid in the solidified soil more uniform, thereby improving its modification effect on the solidified soil and significantly improving the mechanical properties of the solidified body.
[0030] (2) During the preparation of solidified soil, a time interval can be set for adding the curing agent and construction waste soil, so that the curing agent and soil materials can be better integrated into the water. Adding and stirring at the same time can make the mixing of the various groups of materials more uniform, thereby improving the quality of the solidified soil and ensuring the construction effect. In this way, not only the resource utilization of construction waste soil is realized, but also the engineering problems of transportation, accumulation and treatment and disposal of waste soil are solved. In addition, the procurement cost of external backfill materials is also reduced.
[0031] (3) The solidified material provided by the present invention can utilize engineering slag. This material not only improves the strength of the solidified slag, but also solves the environmental pollution and resource waste problems caused by engineering slag, which is beneficial to reducing the economic cost of the project and is low-carbon and environmentally friendly. DETAILED DESCRIPTION
[0032] To better illustrate the present invention and facilitate understanding of the technical solution of the present invention, typical but non-limiting embodiments of the present invention are as follows:
[0033] This embodiment provides a slag solidifying agent, which includes:
[0034] The mass ratio of kaolin, solid alkali and silicate solution is (11.01-12.08):1:(4.06-5.35).
[0035] In this embodiment, the mass ratio of the metakaolin, solid alkali and silicate solution is (11.01-12.08):1:(4.06-5.35), for example, it can be 11.01:1:4.06, 11.1:1:4.1, 11.2:1:4.2, 11.3:1:4.5, 11.4:1:4.8, 11.8:1:5, 12:1:5.2 or 12.08:1:4.06, etc., but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0036] Wherein, the metakaolin includes coal-bearing metakaolin.
[0037] Wherein, the particle size of the metakaolin is 3-32 μm.
[0038] In the present invention, the particle size is limited to aggregates of particles of any size within a range or aggregates of all particles within a certain range, such as aggregates of particles with a particle size of 3 μm, aggregates of particles with a particle size of 5 μm, aggregates of particles with a particle size of 10 μm, aggregates of particles with a particle size of 15 μm, aggregates of particles with a particle size of 20 μm, or aggregates of particles with a particle size of 32 μm, etc., or aggregates of all particles within 3-10 μm, aggregates of all particles within 8-15 μm, aggregates of all particles within 12-20 μm, aggregates of all particles within 18-25 μm, or aggregates of all particles within 20-32 μm, etc.
[0039] Wherein, the solid alkali includes sodium hydroxide and / or potassium hydroxide.
[0040] Wherein, the silicate solution includes sodium silicate solution and / or potassium silicate solution.
[0041] The modulus of the silicate solution is 3-4, for example, 3, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9 or 4, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0042] Among them, the mass concentration of the silicate solution is 34-35%, for example, it can be 34%, 34.1%, 34.2%, 34.3%, 34.4%, 34.5%, 34.6%, 34.7%, 34.8%, 34.9% or 35%, etc., but is not limited to the listed values, and other unlisted values within this range also meet the requirements.
[0043] Furthermore, the present invention provides a method for solidifying slag, which comprises solidifying and shaping the slag using the slag solidifying agent as described above.
[0044] Specifically, the curing method comprises: preparing ingredients according to a mass ratio formula, and then mixing a solid alkali and a silicate solution to obtain a curing intermediate solution;
[0045] Kaolin, solidification intermediate liquid, calcium material and slag are stirred and mixed, and then cured and formed to obtain solidified slag.
[0046] Among them, the mass ratio of kaolin and slag is (0.1-0.25):1, for example, it can be 0.1:1, 0.11:1, 0.12:1, 0.13:1, 0.14:1, 0.15:1, 0.16:1, 0.17:1, 0.18:1, 0.19:1, 0.2:1, 0.21:1, 0.22:1, 0.23:1, 0.1:24 or 0.1:25, etc., but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0047] Among them, the mass ratio of the slag and calcium material is (5-10):1, for example, it can be 5:1, 5.5:1, 6:1, 6.5:1, 7:1, 7.5:1, 8:1, 8.5:1, 9:1, 9.5:1 or 10:1, but is not limited to the listed values, and other unlisted values within this range also meet the requirements.
[0048] Wherein, the stirring and mixing includes a first stirring and mixing and a second stirring and mixing performed sequentially.
[0049] Wherein, the stirring speed of the first stirring and mixing is less than the stirring speed of the second stirring and mixing.
[0050] Wherein, the stirring speed of the first stirring and mixing is 62-140r / min, for example, it can be 62r / min, 65r / min, 70r / min, 75r / min, 80r / min, 85r / min, 90r / min, 95r / min, 100r / min, 105r / min, 110r / min, 115r / min, 120r / min, 125r / min, 130r / min, 135r / min or 140r / min, but is not limited to the listed values, and other values not listed in this range also meet the requirements.
[0051] Among them, the stirring time of the first stirring and mixing is 2-5min, for example, it can be 2min, 2.2min, 2.4min, 2.6min, 2.8min, 3min, 3.2min, 3.4min, 3.6min, 3.8min, 4min, 4.2min, 4.4min, 4.6min, 4.8min or 5min, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0052] Wherein, the stirring speed of the second stirring and mixing is 125-285r / min, for example, it can be 125r / min, 125r / min, 130r / min, 140r / min, 150r / min, 160r / min, 170r / min, 180r / min, 190r / min, 200r / min, 210r / min, 220r / min, 240r / min, 260r / min or 285r / min, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0053] Among them, the stirring time of the second stirring and mixing is 2-5min, for example, it can be 2min, 2.2min, 2.4min, 2.6min, 2.8min, 3min, 3.2min, 3.4min, 3.6min, 3.8min, 4min, 4.2min, 4.4min, 4.6min, 4.8min or 5min, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0054] Furthermore, in order to illustrate the curing effect that can be achieved by the slag curing agent provided by the present invention, an actual example is used for exemplary description, as follows:
[0055] Example 1
[0056] This embodiment provides a slag solidifying agent, the slag solidifying agent comprising:
[0057] Metakaolin, solid alkali and silicate solution in a mass ratio of 11.5:1:4.4;
[0058] The metakaolin is coal-based metakaolin; the particle size of the metakaolin is 3-10 μm;
[0059] The solid alkali is sodium hydroxide;
[0060] The silicate solution is a sodium silicate solution; the modulus of the silicate solution is 3.26; the mass concentration of the silicate solution is 34.5%;
[0061] The exploit process is as follows:
[0062] The ingredients are formulated according to a mass ratio, and then the solid alkali and the silicate solution are mixed to obtain a solidified intermediate solution;
[0063] The kaolin, solidification intermediate liquid, calcium material and slag are stirred and mixed, and then cured and formed to obtain solidified slag;
[0064] The mass ratio of kaolin to slag is 0.13:1; the mass ratio of slag to calcium material is 10:1;
[0065] The stirring and mixing includes a first stirring and mixing and a second stirring and mixing performed sequentially; the stirring speed of the first stirring and mixing is less than the stirring speed of the second stirring and mixing; the stirring speed of the first stirring and mixing is 62 r / min; the stirring time of the first stirring and mixing is 3 min; the stirring speed of the second stirring and mixing is 125 r / min; and the stirring time of the second stirring and mixing is 3 min.
[0066] The unconfined compressive strength of the solidified soil was tested, and the results are shown in Table 1.
[0067] Example 2
[0068] This embodiment provides a slag solidifying agent, the slag solidifying agent comprising:
[0069] Metakaolin, solid alkali and silicate solution in a mass ratio of 11.7:1:4.8;
[0070] The metakaolin is coal-based metakaolin; the particle size of the metakaolin is 8-15 μm;
[0071] The solid alkali is potassium hydroxide;
[0072] The silicate solution is a sodium silicate solution; the modulus of the silicate solution is 3.58; the mass concentration of the silicate solution is 34.8%;
[0073] The exploit process is as follows:
[0074] The ingredients are formulated according to a mass ratio, and then the solid alkali and the silicate solution are mixed to obtain a solidified intermediate solution;
[0075] The kaolin, solidification intermediate liquid, calcium material and slag are stirred and mixed, and then cured and formed to obtain solidified slag;
[0076] The mass ratio of kaolin to slag is 0.2:1; the mass ratio of slag to calcium material is 10:1;
[0077] The stirring and mixing includes a first stirring and mixing and a second stirring and mixing performed sequentially; the stirring speed of the first stirring and mixing is less than the stirring speed of the second stirring and mixing; the stirring speed of the first stirring and mixing is 62 r / min; the stirring time of the first stirring and mixing is 4 min; the stirring speed of the second stirring and mixing is 125 r / min; and the stirring time of the second stirring and mixing is 4 min.
[0078] The unconfined compressive strength of the solidified soil was tested, and the results are shown in Table 1.
[0079] Example 3
[0080] This embodiment provides a slag solidifying agent, the slag solidifying agent comprising:
[0081] Metakaolin, solid alkali and silicate solution in a mass ratio of 12.08):1:4.06;
[0082] The metakaolin is coal-based metakaolin; the particle size of the metakaolin is 12-20 μm;
[0083] The solid alkali is sodium hydroxide;
[0084] The silicate solution is a sodium silicate solution; the modulus of the silicate solution is 3; the mass concentration of the silicate solution is 35%;
[0085] The exploit process is as follows:
[0086] The ingredients are formulated according to a mass ratio, and then the solid alkali and the silicate solution are mixed to obtain a solidified intermediate solution;
[0087] The kaolin, solidification intermediate liquid, calcium material and slag are stirred and mixed, and then cured and formed to obtain solidified slag;
[0088] The mass ratio of kaolin to slag is 0.13:1; the mass ratio of slag to calcium material is 5:1;
[0089] The stirring and mixing includes a first stirring and mixing and a second stirring and mixing performed sequentially; the stirring speed of the first stirring and mixing is less than the stirring speed of the second stirring and mixing; the stirring speed of the first stirring and mixing is 140 r / min; the stirring time of the first stirring and mixing is 2 min; the stirring speed of the second stirring and mixing is 285 r / min; and the stirring time of the second stirring and mixing is 5 min.
[0090] The unconfined compressive strength of the solidified soil was tested, and the results are shown in Table 1.
[0091] Example 4
[0092] This embodiment provides a slag solidifying agent, the slag solidifying agent comprising:
[0093] Metakaolin, solid alkali and silicate solution in a mass ratio of 11.01:1:5.35;
[0094] The metakaolin is coal-based metakaolin; the particle size of the metakaolin is 18-32 μm;
[0095] The solid alkali is sodium hydroxide;
[0096] The silicate solution is a sodium silicate solution; the modulus of the silicate solution is 4; the mass concentration of the silicate solution is 34%;
[0097] The exploit process is as follows:
[0098] The ingredients are formulated according to a mass ratio, and then the solid alkali and the silicate solution are mixed to obtain a solidified intermediate solution;
[0099] The kaolin, solidification intermediate liquid, calcium material and slag are stirred and mixed, and then cured and formed to obtain solidified slag;
[0100] The mass ratio of kaolin to slag is 0.2:1; the mass ratio of slag to calcium material is 5:1;
[0101] The stirring and mixing includes a first stirring and mixing and a second stirring and mixing performed in sequence; the stirring speed of the first stirring and mixing is less than the stirring speed of the second stirring and mixing; the stirring speed of the first stirring and mixing is 120 r / min; the stirring time of the first stirring and mixing is 5 min; the stirring speed of the second stirring and mixing is 200 r / min; and the stirring time of the second stirring and mixing is 2 min.
[0102] The unconfined compressive strength of the solidified soil was tested, and the results are shown in Table 1.
[0103] Comparative Example 1
[0104] The only difference from Example 1 is that the mass ratio of metakaolin, solid alkali and silicate solution in the slag solidifying agent is 5:1:4.4.
[0105] Comparative Example 2
[0106] The only difference from Example 1 is that the mass ratio of metakaolin, solid alkali and silicate solution in the slag solidifying agent is 15:1:4.4.
[0107] Comparative Example 3
[0108] The only difference from Example 1 is that the mass ratio of metakaolin, solid alkali and silicate solution in the slag solidifying agent is 11.5:1:3.
[0109] Comparative Example 4
[0110] The only difference from Example 1 is that the mass ratio of metakaolin, solid alkali and silicate solution in the slag solidifying agent is 11.5:1:8.
[0111] Comparative Example 5
[0112] The only difference from Example 1 is that the solid alkali in the slag solidifying agent is replaced by calcium hydroxide.
[0113] Comparative Example 6
[0114] The only difference from Example 1 is that the metakaolin is replaced by an equal amount of calcined kaolin.
[0115] Comparative Example 7
[0116] The only difference from Example 1 is that the metakaolin is replaced by an equal amount of bentonite.
[0117] The solidified slag obtained in the example was sampled according to the test procedure for inorganic binder stabilized materials for highway engineering, and the unconfined compressive strength was tested after curing for 1d, 7d, and 28d.
[0118] Table 1
[0119]
[0120]
[0121] It can be seen from Table 1 that in the scheme provided by the present invention, through the reasonable design of the curing agent formula, after the slag is cured with the curing agent, the obtained solidified body has good compressive strength, the compressive strength after 28 days of curing is ≥53.6MPa, the compressive strength after 7 days of curing is ≥46MPa, and the compressive strength after 1 day of curing is ≥35.5MPa, which is conducive to the use of slag as trench backfill.
[0122] It is stated that the present invention illustrates the detailed structural features of the present invention through the above embodiments, but the present invention is not limited to the above detailed structural features, that is, it does not mean that the present invention must rely on the above detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
[0123] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0124] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0125] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A soil solidifying agent, characterized in that: The slag solidifying agent comprises: The mass ratio of kaolin, solid alkali and silicate solution is (11.01-12.08):1:(4.06-5.35).
2. The soil solidifying agent according to claim 1, characterized in that: The metakaolin includes coal-measure metakaolin; Preferably, the particle size of the metakaolin is 3-32 μm.
3. The soil solidifying agent according to claim 1, characterized in that: The solid base includes sodium hydroxide and / or potassium hydroxide.
4. The soil solidifying agent according to claim 1, characterized in that: The silicate solution includes a sodium silicate solution and / or a potassium silicate solution; Preferably, the modulus of the silicate solution is 3-4; Preferably, the mass concentration of the silicate solution is 34-35%.
5. A method for solidifying slag, characterized in that: The solidification method comprises solidifying and shaping the slag using the slag solidifying agent as described in any one of claims 1 to 4.
6. The curing method according to claim 5, characterized in that: The solidification method comprises: preparing ingredients according to a mass ratio formula, and then mixing a solid alkali and a silicate solution to obtain a solidification intermediate solution; Kaolin, solidification intermediate liquid, calcium material and slag are stirred and mixed, and then cured and formed to obtain solidified slag.
7. The curing method according to claim 6, characterized in that: The mass ratio of kaolin and slag is (0.1-0.25):1; Preferably, the mass ratio of the slag to the calcium material is (5-10):
1.
8. The curing method according to claim 6, characterized in that: The stirring and mixing includes a first stirring and mixing and a second stirring and mixing performed sequentially; Preferably, the stirring speed of the first stirring and mixing is less than the stirring speed of the second stirring and mixing.
9. The curing method according to claim 8, characterized in that: The stirring speed of the first stirring and mixing is 62-140 r / min; Preferably, the stirring time of the first stirring and mixing is 2-5 min.
10. The curing method according to claim 8 or 9, characterized in that: The stirring speed of the second stirring and mixing is 125-285r / min; Preferably, the stirring time of the second stirring and mixing is 2-5 min.
Citation Information
Patent Citations
Muck curing agent
CN111393082A
Engineering muck curing agent and preparation method thereof
CN115806417A