Bentonite salt-isolating material for highway base course in salinized area, salt-isolating base course and construction method
By using a mixture of foam light soil, ceramide and single-grade gravel in the salt-bearing soil area to form a salt-separated base layer, the problems of water and salt migration and freezing are solved, and effective water and salt isolation and discharge are achieved, which improves the Highway life and safety.
Patent Information
- Application Number
- CN202411034067.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
AI Technical Summary
When building roads in salt-damaged soil areas, water and salt migration and freezing caused by changes in external temperature and humidity will cause damage to the pavement base structure, affecting the service life and safety of the highway. The existing technology partition treatment has water and gas accumulation and Poor water discharge problem.
Use a mixture of foam light soil, ceratops and single-grade gravel as salt separator materials to prepare foam light soil by modifying bentonite and composite plant foaming agent, combining ceratops and gravel to form a salt separator base layer to block Water and salt migration and have anti-freeze and insulation properties.
Effectively block the upward migration of water and salt in the roadbed, prevent salt from destroying the pavement base structure, have good mechanical properties and moisture discharge ability, and improve the durability and safety of the highway.
Smart Images

Figure CN118955028A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of highway construction, and in particular to a bentonite salt-isolating material for a highway base in a saline area, a salt-isolating base and a construction method. Background Art
[0002] Saline soil refers to saline soil, alkaline soil, and soils of varying degrees of salinization and alkalization that are formed under natural or artificial conditions due to the effects of saline and alkali components. When building roads in saline soil areas, the capillary water rises continuously due to changes in external temperature and humidity, which will drive the salt to migrate upward, causing changes in the water-salt environment at the junction of the road base and the soil subgrade, thereby causing damage to the road base structure, which seriously affects the road performance and service life. At the same time, under certain circumstances such as rainwater infiltration, the roadbed and pavement structure will also be damaged by frost heave and other damages in severe cold climates due to excessive water, reducing the safety of the road.
[0003] Prior art, such as the construction method for treating saline soil roadbed with a barrier layer disclosed in publication number "CN102140771B", adopts a structural form of arranging a fine silt cushion layer, an impermeable composite geotextile and a crushed stone cushion layer in sequence from bottom to top. This invention mainly utilizes the barrier performance of the impermeable composite geotextile to achieve the purpose of salt isolation. However, in the process of water vapor migrating upward in the roadbed, it is easy to accumulate under the membrane, which may cause the mechanical properties of the roadbed soil under the membrane to decrease; at the same time, the geomembrane will also block the water and salt that infiltrates from the upper structure of the roadbed, and cannot be discharged in time. Summary of the invention
[0004] In view of the problems existing in the prior art, the present invention provides a bentonite salt-isolating material, a salt-isolating base and a construction method for a highway base in a saline area. The salt-isolating structure can block the upward migration of water and salt in the roadbed, thereby preventing the damage of the road base structure by salt; it can discharge the water and salt that seep into the road base structure under specific conditions such as rainfall; and it also has certain antifreeze and thermal insulation properties.
[0005] The present invention is achieved through the following technical solutions:
[0006] A bentonite salt-isolating material for a highway base in a saline area, comprising foamed lightweight soil, ceramsite and single-graded crushed stone, with a volume ratio of (3-4):1:(5-6);
[0007] The foamed lightweight soil comprises slurry and foam;
[0008] The slurry comprises 30-50 parts of cement, 10-20 parts of fly ash, 5-8 parts of modified bentonite and 25-40 parts of water.
[0009] Preferably, the foam comprises 2 parts of a composite plant foaming agent, 0.1 parts of a foam stabilizer and 60 parts of water.
[0010] Preferably, the foam stabilizer is dodecanol.
[0011] Preferably, the composite plant foaming agent is HTW-1.
[0012] A method for preparing a salt-isolating material comprises the following steps:
[0013] Step 1, preparing foamed lightweight soil;
[0014] Cement, fly ash and modified bentonite are mixed with water to obtain a mixed slurry, and a composite plant foaming agent and a stabilizer are added to the mixed slurry and mixed to obtain foamed lightweight soil;
[0015] Step 2, preparing salt isolation material;
[0016] The foamed lightweight soil, expanded clay and single-graded crushed stone are uniformly mixed in a volume ratio of (3-4):1:(5-6) to obtain a salt-isolating material.
[0017] Preferably, the preparation method of the foamed lightweight soil in step 1 is as follows:
[0018] Add 30-50 parts of cement, 10-20 parts of fly ash, 5-8 parts of modified bentonite and 25-40 parts of argon to mix and stir evenly to form a mixed slurry;
[0019] Add 2 parts of diluted composite plant foaming agent and 0.1 parts of foam stabilizer to the mixed slurry, stir evenly to obtain foamed lightweight soil.
[0020] Preferably, the dilution ratio of the composite plant foaming agent is 1:30.
[0021] A highway base bentonite salt-isolating base comprises, from top to bottom, a crushed stone layer, a protective cushion layer and a salt-isolating material layer, wherein the salt-isolating material layer is a salt-isolating material of a certain thickness.
[0022] Preferably, the protective cushion layer is a sand layer.
[0023] A construction method for a highway base bentonite salt-isolating base comprises the following steps:
[0024] Step 1: Mix the single-graded crushed stone and ceramsite thoroughly and spread them on the moistened roadbed surface;
[0025] Step 2: pouring the foamed lightweight soil on the single-graded crushed stone and ceramsite, and filling the gaps between the crushed stone and the ceramsite with the foamed lightweight soil, and forming a salt-isolating material layer after solidification;
[0026] Step 3: Laying a protective cushion layer on the salt isolation material layer;
[0027] Step 4: Lay graded crushed stone on the protective cushion layer and compact it to form a salt-isolating base layer.
[0028] Compared with the prior art, the present invention has the following beneficial technical effects:
[0029] The present invention provides a bentonite salt-isolating material for the base of a highway in a saline area, which uses a mixture of foamed lightweight soil, single-graded crushed stone, and ceramsite as a partition material. The modified nano-bentonite in the foamed lightweight soil has good water absorption, and combined with the unique bubble pore structure of the foamed lightweight soil, the salt will be trapped in it as the water rises; an appropriate amount of fly ash can improve the frost resistance of the foamed lightweight soil, and combined with the inherent thermal insulation performance of the foamed lightweight soil, it has good durability; at the same time, ceramsite, as a commonly used salt-isolating material, will further improve the salt storage capacity of the mixture to a certain extent. The single-graded crushed stone serves as a skeleton that bears external loads and is bonded into a whole by the foamed lightweight soil, so that it has good mechanical properties. Under specific circumstances such as rainfall infiltration, most of the water and salt in the upper base structure are discharged into the road structure along with the laid cross slope during the infiltration process, and the remaining water and salt that cannot be discharged in time will be stored in the mixture. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 It is a schematic end view of the bentonite salt-isolating material for the highway base of the present invention;
[0031] Figure 2 The present invention is a construction flow chart of the bentonite salt-isolating base layer of the highway base layer. DETAILED DESCRIPTION
[0032] The present invention will be further described in detail below in conjunction with the accompanying drawings, which are intended to explain the present invention rather than to limit it.
[0033] A bentonite salt-isolating material for highway base in saline soil areas comprises foamed lightweight soil, ceramsite and single-graded crushed stone, wherein the volume ratio is (3-4):1:(5-6).
[0034] The foamed lightweight soil comprises slurry and foam;
[0035] The slurry includes 30-50 parts of cement, 10-20 parts of fly ash, 5-8 parts of modified bentonite, and 25-40 parts of water;
[0036] The modified bentonite is modified nano-bentonite, and the density of fly ash is not less than 2000kg / m 3 , Class F II fly ash is preferred.
[0037] The foam comprises 2 parts of a composite plant foaming agent, 0.1 parts of a foam stabilizer and 60 parts of water.
[0038] The composite plant foaming agent is HTW-1, the optimal dilution ratio is 1:30, and the foam stabilizer is 0.7 g / L dodecanol.
[0039] The cement is 42.5 grade ordinary Portland cement
[0040] The particle size of the expanded clay is 20-25 mm, and the particle size of the single-graded crushed stone is 30-37.5 mm.
[0041] A method for preparing a highway base bentonite salt-isolating material comprises the following steps:
[0042] Step 1, preparing foamed lightweight soil;
[0043] Cement, fly ash and modified bentonite are mixed with water to obtain a mixed slurry, and a composite plant foaming agent and a stabilizer are added to the mixed slurry and mixed to obtain foamed lightweight soil. The specific method is as follows:
[0044] S1.1, add 30-50 parts of cement, 10-20 parts of fly ash, 5-8 parts of modified bentonite and 25-40 parts of argon to mix and stir evenly to form a mixed slurry;
[0045] S1.2. Add 2 parts of the diluted composite plant foaming agent and 0.1 parts of the foam stabilizer to the mixed slurry obtained in step S1.1, and stir evenly to obtain foamed lightweight soil.
[0046] During the preparation process, set the foam density to 45-50kg / m 3 , the density of foam lightweight soil is 450-500KN / m 3 The humidity of the prepared foamed lightweight soil is 500-550KN / m 3 .
[0047] Step 2, preparing salt isolation material;
[0048] The foamed lightweight soil, expanded clay and single-graded crushed stone are uniformly mixed in a volume ratio of (3-4):1:(5-6) to obtain a salt-isolating material.
[0049] The particle size of the ceramsite is 20-25 mm, and the particle size of the single-grade crushed stone is 30-37.5 mm.
[0050] Example 1
[0051] A method for preparing a highway base bentonite salt-isolating material comprises the following steps:
[0052] Step 1, preparing foamed lightweight soil;
[0053] 30 parts of cement, 10 parts of fly ash and 8 parts of modified bentonite are added into a hopper, and after being conveyed to a mixer via a conveyor belt, 30 parts of water are added for rapid stirring to obtain a mixed slurry;
[0054] Dilute 2 parts of composite plant foaming agent with 30 times of water, and add 0.1 parts of foam stabilizer to obtain foaming agent. Set the foam density to 45kg / m 3 , blowing the foaming agent into the foaming slurry mixer for stirring;
[0055] Set the foam lightweight soil density to 450-500KN / m in the control center of the foam mixer. 3 The system automatically adjusts the slurry feeding speed in the hopper to obtain a wet density of 500-550KN / m 3 Foam lightweight soil.
[0056] Step 2, preparing salt isolation material;
[0057] Add 1 part of expanded clay and 5 parts of single-graded crushed stone to 4 parts of foamed lightweight soil and mix well to obtain salt-isolating material.
[0058] Example 2
[0059] A method for preparing a highway base bentonite salt-isolating material comprises the following steps:
[0060] Step 1, preparing foamed lightweight soil;
[0061] 35 parts of cement, 16 parts of fly ash, and 5 parts of modified bentonite are added into a hopper, and after being conveyed to a mixer via a conveyor belt, 25 parts of water are added for rapid stirring to obtain a mixed slurry;
[0062] Dilute 2 parts of composite plant foaming agent with 30 times of water, and add 0.1 parts of foam stabilizer to obtain foaming agent. Set the foam density to 48kg / m 3 , blowing the foaming agent into the foaming slurry mixer for stirring;
[0063] The foam lightweight soil density is set to 480KN / m in the control center of the slurry mixer. 3 The system automatically adjusts the slurry feeding speed in the hopper to obtain a wet density of 520KN / m 3 Foam lightweight soil.
[0064] Step 2, preparing salt isolation material;
[0065] Add 1 part of expanded clay and 6 parts of single-graded crushed stone to 3 parts of foamed lightweight soil and mix well to obtain salt-isolating material.
[0066] Example 3
[0067] A method for preparing a highway base bentonite salt-isolating material comprises the following steps:
[0068] Step 1, preparing foamed lightweight soil;
[0069] 50 parts of cement, 20 parts of fly ash and 7 parts of modified bentonite are added into a hopper, and after being conveyed to a mixer via a conveyor belt, 40 parts of water are added for rapid stirring to obtain a mixed slurry;
[0070] Dilute 2 parts of composite plant foaming agent with 30 times of water, and add 0.1 parts of foam stabilizer to obtain foaming agent. Set the foam density to 50kg / m 3 , blowing the foaming agent into the foaming slurry mixer for stirring;
[0071] The foam lightweight soil density is set to 500KN / m in the control center of the foam mixer. 3 The system automatically adjusts the slurry feeding speed in the hopper to obtain a wet density of 550KN / m 3 Foam lightweight soil.
[0072] Step 2, preparing salt isolation material;
[0073] Add 1 part of expanded clay and 5.6 parts of single-graded crushed stone to 3.5 parts of foamed lightweight soil and mix well to obtain a salt-isolating material.
[0074] See also Figure 1 A highway base bentonite salt-isolating base layer comprises, from top to bottom, a crushed stone layer, a sand layer and a salt-isolating material layer.
[0075] The crushed stone layer is graded crushed stone, and the thickness of the crushed stone layer is 20-25 cm.
[0076] The sand layer serves as a protective cushion layer, and its thickness is 10-20 cm.
[0077] The thickness of the salt isolation material layer is 10-15 cm.
[0078] A method for preparing a highway base bentonite salt-isolating base comprises the following steps:
[0079] Step 1: clean up the debris on the roadbed surface, compact it and make the roadbed surface smooth;
[0080] Step 2: Measure and lay out the lines; set up markers to control the paving thickness and arrange supports on both sides of the paving;
[0081] Step 3: Sprinkle water on the roadbed surface to keep the local contact surface moist;
[0082] Step 4: Mix the single-graded crushed stone and ceramsite thoroughly and spread them on the roadbed surface, and set a 1.5% cross slope on both sides with the center of the roadbed as the boundary;
[0083] Step 5: pour the prepared foamed lightweight soil on top, and use a concrete vibrator to fully fill the gaps between the gravel. After solidification, cover it with straw mats and sprinkle water for curing for no less than 7 days to form a salt-isolating material layer.
[0084] Step 6: Lay 10 cm of fine sand on the salt isolation material layer as a protective cushion;
[0085] Step 7: Lay 20cm of graded crushed stone on the protective cushion layer, and use a roller of more than 12t to perform static pressure treatment and then vibration compaction to form a salt-isolating base layer.
[0086] The present invention provides a salt-protected bentonite salt-isolating material for the base of a highway in a saline area, comprising foamed lightweight soil, ceramsite and single-graded crushed stone; the foamed lightweight soil is formed by mixing slurry and foam components, the slurry components include cement, fly ash, modified bentonite and water; the foam components include a composite plant foaming agent, a stabilizer and water; the ceramsite particle size is 20-25 mm, and the single-graded crushed stone particle size is 30-37.5 mm. The salt-isolating material can effectively prevent the migration of water and salt in the roadbed due to changes in external temperature and humidity, thereby destroying the road base structure; at the same time, it can discharge the water that seeps into the upper structure of the road, effectively prevent the road structure from being damaged, and increase the service life of the road.
[0087] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A bentonite salt-isolating material for highway base in saline areas, characterized in that: It includes foamed lightweight soil, ceramsite and single-graded crushed stone, with the volume ratio of (3-4):1:(5-6); The foamed lightweight soil comprises slurry and foam; The slurry comprises 30-50 parts of cement, 10-20 parts of fly ash, 5-8 parts of modified bentonite and 25-40 parts of water.
2. The bentonite salt-isolating material for road base in saline areas according to claim 1, characterized in that: The foam comprises 2 parts of a composite plant foaming agent, 0.1 parts of a foam stabilizer and 60 parts of water.
3. The bentonite salt-isolating material for road base in saline areas according to claim 2, characterized in that: The foam stabilizer is dodecanol.
4. The bentonite salt-isolating material for road base in saline areas according to claim 2, characterized in that: The composite plant foaming agent is HTW-1.
5. A method for preparing the salt barrier material according to any one of claims 1 to 4, characterized in that: The following steps are involved: Step 1, preparing foamed lightweight soil; Cement, fly ash and modified bentonite are mixed with water to obtain a mixed slurry, and a composite plant foaming agent and a stabilizer are added to the mixed slurry and mixed to obtain foamed lightweight soil; Step 2, preparing salt isolation material; The foamed lightweight soil, expanded clay and single-graded crushed stone are uniformly mixed in a volume ratio of (3-4):1:(5-6) to obtain a salt-isolating material.
6. The method for preparing the salt-isolating material according to claim 5, characterized in that: The preparation method of the foamed lightweight soil in step 1 is as follows: Add 30-50 parts of cement, 10-20 parts of fly ash, 5-8 parts of modified bentonite and 25-40 parts of argon to mix and stir evenly to form a mixed slurry; Add 2 parts of diluted composite plant foaming agent and 0.1 parts of foam stabilizer to the mixed slurry, stir evenly to obtain foamed lightweight soil.
7. The method for preparing the salt-isolating material according to claim 5, characterized in that: The dilution ratio of the composite plant foaming agent is 1:
30.
8. A bentonite salt-isolating base for a highway base, characterized in that: The method comprises, from top to bottom, a crushed stone layer, a protective cushion layer and a salt-isolating material layer, wherein the salt-isolating material layer is the salt-isolating material according to any one of claims 1 to 4 with a certain thickness.
9. A highway base bentonite salt-isolating base according to claim 8, characterized in that: The protective cushion layer is a sand layer.
10. A construction method for a highway base bentonite salt-isolating base as claimed in claim 8 or 9, characterized in that: The following steps are involved: Step 1: Mix the single-graded crushed stone and ceramsite thoroughly and spread them on the moistened roadbed surface; Step 2: pouring the foamed lightweight soil on the single-graded crushed stone and ceramsite, and filling the gaps between the crushed stone and the ceramsite with the foamed lightweight soil, and forming a salt-isolating material layer after solidification; Step 3: Laying a protective cushion layer on the salt isolation material layer; Step 4: Lay graded crushed stone on the protective cushion layer and compact it to form a salt-isolating base layer.
Citation Information
Cited By
Salinized soil roadbed soluble salt adsorption material, preparation method and roadbed building method
CN121550955A