Permanent magnetic ferrite material as well as preparation method and application thereof
By using permanent magnet ferrite powder as crystallization seeds in the preparation of permanent magnet ferrite materials, the prefiring temperature is reduced, and the problem of limited improvement in magnetic performance in the prior art is solved, and the preparation of high-performance permanent magnet ferrite materials is realized, reducing the reduction of energy consumption and cost.
Patent Information
- Application Number
- CN202411043864.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-31
AI Technical Summary
In the prior art, under the condition of no lanthanum cobalt addition, the magnetic performance improvement of permanent magnet ferrite materials is limited, and the process flow is extended and energy consumption is increased, making it difficult to meet higher application prospects.
By adding a small amount of permanent magnet ferrite powder as crystal seeds for the solid phase reaction of ferrite in the preparation of permanent magnet ferrite materials, the prefiring temperature is reduced, energy consumption is reduced, and the process formula is optimized to improve magnetic performance.
It is achieved without adding lanthanum cobalt to obtain high-performance permanent magnet ferrite materials, significantly improve magnetic performance, reduce preburning temperature, reduce energy consumption, and improve cost-effectiveness.
Smart Images

Figure BDA0004973003430000101 
Figure BDA0004973003430000111 
Figure BDA0004973003430000121
Abstract
Description
Technical Field
[0001] The invention belongs to the field of magnetic materials and relates to a permanent magnetic ferrite material and a preparation method and application thereof. Background Art
[0002] Permanent ferrite is one of the basic functional materials of permanent magnet DC motors. It can meet the use requirements of motors in various environments. It has high sensitivity and stability and can be widely used in various types of high-power, high-speed, and high-torque motors, such as high-end automotive motors (ABS motors, starter motors, etc.), motorcycle starter motors, household appliances, and power tool motors.
[0003] There are two most important parameters that determine the magnetic properties of permanent ferrite, namely the residual flux density (B r ) and intrinsic coercivity (H cj ). The original permanent ferrite materials were mainly strontium ferrite (SrO·6Fe2O3) and barium ferrite (BaO·6Fe2O3) with a hexagonal structure of magnetoplumbite. In order to further improve the magnetic properties, since this century, ion replacement formula technology represented by La-Co replacement has been developed and applied, which has greatly improved the performance of permanent ferrites. Relevant researchers at home and abroad have successively developed permanent ferrite materials with a remanence of about 4500Gs and an intrinsic coercive force of 5000Oe.
[0004] However, as the lowest-cost permanent magnetic material, the permanent magnetic ferrite prepared by La-Co ion exchange technology has a relatively limited application range due to the addition of expensive rare earth and rare metal oxides, which leads to a significant increase in cost and a significant decrease in cost-performance. In recent years, the preparation technology of high-performance permanent magnetic ferrite without lanthanum and cobalt addition has been significantly developed. This technology takes into account the requirements of magnetic properties and low cost, has excellent cost-performance, and has a very broad market application prospect.
[0005] CN104003704B discloses a method for preparing a lanthanum-free cobalt permanent magnet ferrite. The method uses molten salt as a medium for solid-phase reaction, adjusts the type and ratio of the molten salt, and controls the sintering process to obtain a permanent magnet ferrite material with higher magnetic properties than the traditional process without adding lanthanum and cobalt.
[0006] CN101209920B discloses a sintered permanent magnet ferrite and a preparation method thereof, and CN104496444B discloses a low-cost sintered permanent magnet ferrite material and a preparation method thereof. Both use relatively low-cost Al2O3 or Cr2O3 to replace the expensive Co oxide, and at the same time greatly reduce or even completely avoid adding rare earth elements, thereby greatly reducing direct material costs. The prepared sintered permanent magnet ferrite can obtain higher magnetic induction intensity and better intrinsic coercive force, meeting the application requirements of medium and high-end magnets.
[0007] CN109836148B discloses a permanent magnet ferrite material without La and Co elements and a preparation method thereof. The material composition is optimized, the uniformity of ferrite grains is improved, the pre-firing temperature is reduced, the intrinsic coercivity of the material is effectively improved, and a sintered ferrite permanent magnet material with high coercivity and high remanence is prepared without adding La and Co elements.
[0008] Although the optimization solutions provided by the above-mentioned existing technologies can improve the material performance to a certain extent without adding lanthanum-cobalt additives, they are mainly achieved by continuing the ion exchange technology to optimize the formula. Some solutions also extend the process flow and improve the energy consumption level. The improvement of magnetic properties by the existing solutions is also relatively limited. Therefore, it is necessary to further develop new technical solutions to achieve higher practical application prospects. Summary of the invention
[0009] In view of the problems existing in the prior art, the purpose of the present invention is to provide a permanent magnet ferrite material and a preparation method and use thereof. The preparation method accelerates the solid phase reaction, reduces the pre-firing temperature, and reduces the energy consumption during the pre-firing process by adding a small amount of permanent magnet ferrite powder as a crystallization seed for the ferrite solid phase reaction. By improving the preparation method, a permanent magnet ferrite material with excellent magnetic properties is obtained without the addition of lanthanum and cobalt.
[0010] To achieve this object, the present invention adopts the following technical solutions:
[0011] In a first aspect, the present invention provides a method for preparing a permanent magnetic ferrite material, the preparation method comprising:
[0012] A permanent magnet ferrite seed crystal is provided, the permanent magnet ferrite seed crystal is mixed with a permanent magnet ferrite raw material, and pre-sintering and sintering are performed in sequence to obtain a permanent magnet ferrite material.
[0013] The following are preferred technical solutions of the present invention, but are not intended to be limitations of the technical solutions provided by the present invention. Through the following technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.
[0014] As a preferred technical solution of the present invention, the permanent magnet ferrite seed crystals include permanent magnet ferrite pre-sintered powder and / or waste permanent magnet ferrite material powder.
[0015] It should be noted that the permanent magnet ferrite pre-burned powder can be a pre-burned material (hereinafter referred to as permanent magnet ferrite main phase material) powder obtained by the preparation method of the present invention (i.e., using seed crystals). When the pre-burned material obtained by the preparation method of the present invention is used, it means that the preparation method of the present invention needs to use an initial seed crystal at the beginning. The initial seed crystal can be a pre-burned powder obtained by pre-burning the permanent magnet ferrite raw material using the means of the prior art, or a pre-burned powder obtained by pre-burning the permanent magnet ferrite raw material using the process technology other than the seed crystal content in the present invention (such as ingredient mixing, wet grinding, pre-burning and dry crushing, etc.). Compared with the pre-burning temperature in the preparation method of the present invention when the seed crystal process is used, when the seed crystal process of the present invention is not used to prepare the initial seed crystal, its pre-burning temperature is relatively high.
[0016] It should also be noted that the preparation method of the present invention is based on the mechanism of adding a small amount of permanent magnet ferrite powder as a crystal seed for the solid phase reaction of ferrite, and is therefore not limited to the permanent magnet ferrite powder at the stage of pre-burned powder. The process of using pre-burned powder as a seed is simpler, and the energy consumption and cost are lower. However, the finished permanent magnet ferrite material obtained after sintering or the waste powder after appropriate treatment can also be used as the seed and play a role in the preparation method of the present invention. That is, the permanent magnet ferrite seed of the present invention can also be prepared by conventional preparation methods, or waste powder can be selected.
[0017] Preferably, the average particle size of the permanent magnet ferrite seed crystal is 0.8-10 μm, for example, 0.8 μm, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm or 10 μm, etc., preferably 1-5 μm.
[0018] Preferably, the amount of the permanent magnet ferrite seed crystals is 1% to 10% of the total mass of the permanent magnet ferrite raw material, for example, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%, etc., preferably 2% to 5%.
[0019] In the present invention, the main function of adding seed crystals is to make them evenly dispersed in the raw material powder during the subsequent pre-firing process, adsorb various raw material particles around, thereby accelerating the solid phase reaction, promoting the rapid ferritization of the raw materials, and helping to reduce the pre-firing reaction temperature, reduce the number of large ferrite particles crystallized in the pre-firing material, thereby obtaining uniformly crystallized ferrite particles, improving the comprehensive magnetic properties of the material, and at the same time, also helping to reduce the energy consumption level in the pre-firing material production process. If too few seed crystals are added, it is difficult to play a role, and the uniformity of the crystallization of the pre-firing material will also be relatively low, which is not conducive to the improvement of magnetic properties; if too many seed crystals are added, the ferrite seed powder with a relatively large density is difficult to be evenly mixed with the raw material powder during mixing, resulting in uneven crystallization of ferrite particles during the pre-firing process, and relatively more coarse particles will be crystallized, which is not conducive to the improvement of magnetic properties.
[0020] As a preferred technical solution of the present invention, the permanent ferrite theoretically generated from the permanent ferrite raw material and the permanent ferrite seed crystal belong to the same permanent ferrite system.
[0021] Preferably, the permanent magnet ferrite system comprises strontium ferrite without lanthanum and cobalt, barium ferrite without lanthanum and cobalt, or barium strontium ferrite without lanthanum and cobalt, preferably strontium ferrite without lanthanum and cobalt.
[0022] Preferably, the chemical formula of the lanthanum-free cobalt-free strontium ferrite comprises SrFe 2n O 19 , and 5.5≤n≤6.0, for example, n can be 5.5, 5.6, 5.7, 5.8, 5.9 or 6.0, etc.
[0023] Preferably, the permanent magnet ferrite raw material includes an iron source and a strontium source.
[0024] Preferably, the iron source comprises red iron.
[0025] Preferably, the strontium source comprises strontium carbonate.
[0026] As a preferred technical solution of the present invention, the chemical formula of the strontium ferrite without lanthanum and cobalt includes Sr 1-x M x Fe 2n O 19 , M is a doping element, M includes Ca, and 0.05≤x≤0.4, for example, x can be 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35 or 0.4, etc.; 5.5≤n≤6.0, for example, n can be 5.5, 5.6, 5.7, 5.8, 5.9 or 6.0, etc.
[0027] Preferably, the permanent magnet ferrite raw material further includes a dopant containing M.
[0028] Preferably, the dopant containing M includes calcium carbonate.
[0029] As a preferred technical solution of the present invention, the average particle size of the permanent magnet ferrite raw material is less than 2 μm, for example, 1.9 μm, 1.7 μm, 1.5 μm, 1.2 μm, 1 μm, 0.8 μm, etc.
[0030] Preferably, the mixing method includes wet mixing for 3 to 5 hours (1 hr represents 1 hour or 60 minutes), such as 3 hours, 3.5 hours, 4 hours, 4.5 hours or 5 hours, etc., to obtain a first slurry with an average particle size of 0.6 to 1.0 μm, such as 0.90 μm, 0.85 μm, 0.80 μm, 0.75 μm, 0.70 μm, 0.65 μm or 0.60 μm, etc., and then the first slurry is dried and pelletized to obtain a pelletizing material, and the pelletizing material is pre-calcined.
[0031] In the batching process of the preparation method of the present invention, the average particle size of each raw material is preferably at least 2 μm or less. If the slurry is formed by further wet mixing after batching, the average particle size of the slurry is preferably at least not greater than 0.6 to 1 μm. In particular, for the first slurry before pre-firing, if the average particle size of the first slurry is too large, it is easy to cause insufficient pre-firing during the pre-firing process, resulting in too low a content of the generated M-phase ferrite.
[0032] Preferably, the pre-firing is carried out in an oxygen-containing atmosphere, preferably in air.
[0033] Preferably, the pre-calcination temperature is 1100-1300°C, for example, 1100°C, 1120°C, 1130°C, 1140°C, 1150°C, 1160°C, 1170°C, 1180°C, 1190°C, 1200°C, 1220°C, 1240°C, 1260°C, 1280°C or 1300°C, preferably 1120-1250°C, more preferably 1150-1180°C, and the pre-calcination time is 0.5-3hr, for example, 0.5hr, 0.8hr, 1hr, 1.2hr, 1.4hr, 1.6hr, 1.8hr, 2hr, 2.2hr, 2.4hr, 2.6hr, 2.8hr or 3hr, etc.
[0034] In the present invention, during the pre-sintering process, the addition of permanent magnet ferrite seed powder can adsorb the surrounding uniformly mixed raw material particles at a relatively low temperature, accelerate the ferritization process of the raw material composition, and improve the crystallization uniformity, and can achieve pre-sintering at a lower temperature to avoid the generation of coarse crystal particles as much as possible, thereby improving the comprehensive magnetic properties of the material. At the same time, the lower pre-sintering temperature can also reduce the energy consumption of the pre-sintering process accordingly, thereby reducing the manufacturing cost of the pre-sintered material.
[0035] As a preferred technical solution of the present invention, dry pulverization is performed after the pre-sintering to obtain a permanent magnet ferrite main phase material, which is then sintered and / or used as the permanent magnet ferrite seed crystal.
[0036] Preferably, before the sintering, the permanent magnet ferrite main phase material is first mixed with a secondary additive and wet-ground to obtain a second slurry, and the second slurry is molded to obtain a molded body, which is then sintered.
[0037] In the present invention, the permanent magnet ferrite raw material and the crystal seed constitute the main formula to obtain the main phase material; the present invention further ensures the reduction of the pre-firing temperature by optimizing the main formula and the secondary addition formula.
[0038] Preferably, the secondary additive includes at least one of SiO2, CaCO3, Al2O3, Cr2O3, ZnO, SrCO3 or H3BO3.
[0039] Preferably, the total amount of the secondary additives accounts for 1.0% to 5.0% of the mass of the permanent magnet ferrite main phase material, for example, 1%, 1.2%, 1.4%, 1.6%, 1.8%, 2%, 2.2%, 2.4%, 2.6%, 2.8%, 3%, 3.2%, 3.4%, 3.6%, 3.8%, 4%, 4.2%, 4.4%, 4.6%, 4.8% or 5%, etc.
[0040] Preferably, based on the mass of the permanent magnet ferrite main phase material being 100%, the amount of SiO2 is 0.05% to 3%, the amount of CaCO3 is 0.4% to 3%, the amount of Al2O3 is 0 to 3%, the amount of Cr2O3 is 0 to 1.5%, the amount of ZnO is 0 to 0.6%, the amount of SrCO3 is 0.1% to 1%, and the amount of H3BO3 is 0 to 0.8%.
[0041] Preferably, the average particle size of the secondary additive is less than 2 μm, for example, 1.9 μm, 1.7 μm, 1.5 μm, 1.3 μm, 1 μm, 0.8 μm, etc.
[0042] Preferably, the average particle size of the second slurry is 0.6-1 μm, for example, 0.90 μm, 0.85 μm, 0.80 μm, 0.75 μm, 0.70 μm, 0.65 μm or 0.60 μm, and the solid content is 65wt%-80wt%, for example, 65wt%, 68wt%, 70wt%, 72wt%, 74wt%, 76wt%, 78wt% or 80wt%, etc.
[0043] In the present invention, the solid content (water content) of the obtained slurry can be adjusted using pure water.
[0044] Preferably, the forming method comprises magnetic field forming.
[0045] Preferably, the magnetic field strength of the magnetic field forming is greater than 10000 Oe, such as 11000 Oe, 13000 Oe, 15000 Oe or 18000 Oe.
[0046] In the present invention, if the magnetic field intensity of the magnetic field molding is too low, the orientation of magnetic particles in the molded body will be too low, thereby affecting the remanence of the final magnet.
[0047] As a preferred technical solution of the present invention, the sintering method includes firstly performing a first sintering at 100-600°C, such as 100°C, 130°C, 150°C, 180°C, 200°C, 230°C, 250°C, 280°C, 300°C, 320°C, 350°C, 380°C, 400°C, 430°C, 450°C, 480°C, 500°C, 530°C, 550°C, 580°C or 600°C for 0.5-2 hr, such as 0.5 hr, 0.8 hr, 1 hr , 1.2hr, 1.4hr, 1.6hr, 1.8hr or 2hr, and then at 1180-1230°C, for example, 1180°C, 1190°C, 1200°C, 1210°C, 1220°C or 1230°C, preferably 1190-1220°C, for a second sintering for 0.5-3hr, for example, 0.5hr, 0.8hr, 1hr, 1.3hr, 1.5hr, 1.8hr, 2hr, 2.3hr, 2.5hr, 2.8hr or 3hr, etc.
[0048] Preferably, the second sintering is performed in an oxygen-containing atmosphere, preferably in air.
[0049] As a preferred technical solution of the present invention, the preparation method comprises:
[0050] (1) Synthesizing an initial permanent magnet ferrite seed crystal, wherein the initial permanent magnet ferrite seed crystal is a pre-sintered powder of strontium ferrite without lanthanum and cobalt, wherein the chemical formula of the strontium ferrite without lanthanum and cobalt is SrFe 2n O 19 , and 5.5≤n≤6.0, preparing the raw materials of the initial permanent magnet ferrite seed crystals, including iron source iron oxide and strontium source strontium carbonate, and measuring and mixing them according to the chemical formula, and then wet grinding to obtain an initial slurry with an average particle size of 0.6 to 1 μm, and pre-calcining the initial slurry at 1120 to 1200° C. in air for 0.5 to 3 hours, and then dry-crushing until the average particle size is 0.8 to 10 μm, to obtain the pre-calcined powder as the initial permanent magnet ferrite seed crystals;
[0051] (2) Prepare permanent ferrite raw materials, including iron source iron oxide, strontium source strontium carbonate and calcium carbonate containing calcium element dopant, according to the chemical formula Sr1-x Ca x Fe 2n O 19 , and 0.05≤x≤0.4, 5.5≤n≤6.0 are measured and mixed, and at the same time, the initial permanent magnet ferrite seed crystals are added according to 1% to 10% of the total mass of the permanent magnet ferrite raw material, and wet mixing is performed for 3 to 5 hours to obtain a first slurry with an average particle size of 0.6 to 1 μm; the first slurry is dried and then pelletized to obtain a pelletized material;
[0052] (3) pre-calcining the first slurry at 1120-1200° C. in an oxygen-containing atmosphere for 0.5-3 hours and then dry-crushing the slurry to obtain a permanent magnet ferrite main phase material, using a portion of the obtained permanent magnet ferrite main phase material for subsequent sintering, and re-crushing another portion of the obtained permanent magnet ferrite main phase material to an average particle size of 0.8-10 μm to serve as permanent magnet ferrite seed crystals;
[0053] (4) mixing the permanent magnet ferrite main phase material for sintering with a secondary additive, wherein the secondary additive includes at least one of SiO2, CaCO3, Al2O3, Cr2O3, ZnO, SrCO3 or H3BO3, and the total amount of the secondary additive accounts for 1% to 5% of the mass of the permanent magnet ferrite main phase material for sintering, and performing wet grinding to obtain a second slurry with an average particle size of 0.6 to 1 μm and a solid content of 65wt% to 80wt%, and then performing magnetic field molding at a magnetic field strength of >10000Oe to obtain a molded body;
[0054] (5) The obtained molded body is first sintered at 200-400°C for 0.5-2 hours, and then second sintered at 1180-1230°C in air for 0.5-3 hours to obtain a permanent magnet ferrite material.
[0055] In a second aspect, the present invention provides a permanent magnet ferrite material obtained according to the preparation method described in the first aspect.
[0056] In a third aspect, the present invention provides a use of the permanent magnet ferrite material described in the second aspect, and the use includes a motor.
[0057] Compared with the prior art solutions, the present invention has at least the following beneficial effects:
[0058] The present invention adds a small amount of ferrite powder as a crystal seed to the permanent magnet ferrite raw material, thereby accelerating the solid phase reaction and reducing the pre-sintering temperature, thereby preparing a high-performance permanent magnet ferrite material without the need to add lanthanum and cobalt; the ferrite crystal particles in the obtained permanent magnet ferrite material are more uniform, and because the generation of coarse crystal particles is effectively avoided, the comprehensive magnetic properties of the material are significantly better than those of similar materials prepared by traditional processes;
[0059] The present invention further ensures that the pre-firing temperature is reduced by optimizing the main formula and the secondary addition formula. The pre-firing temperature is relatively lower, and the energy consumption level in the preparation process of the pre-firing material is effectively reduced, thereby further improving the cost performance of the material. DETAILED DESCRIPTION
[0060] The technical solution of the present invention is further illustrated below through specific implementation methods.
[0061] It should be clear to those skilled in the art that the embodiments are only intended to help understand the present invention and should not be considered as specific limitations of the present invention.
[0062] Example 1
[0063] This embodiment provides a method for preparing a permanent magnetic ferrite, comprising:
[0064] (1) Synthesizing an initial permanent magnet ferrite seed crystal, wherein the initial permanent magnet ferrite seed crystal is a pre-sintered powder of strontium ferrite without lanthanum and cobalt, wherein the chemical formula of the strontium ferrite without lanthanum and cobalt is SrFe 12 O 19 ; Prepare the raw materials for the initial permanent magnet ferrite seed crystals, including 5.0 kg of iron red with a purity of 99.5% and 0.78 kg of strontium carbonate with a purity of 98.5%, put them into a sand mill, add about 7 kg of tap water, and perform wet grinding for 2 hours to obtain an initial slurry with an average particle size of 0.6 to 1 μm, pre-calculate the initial slurry at 1250° C. in air for 2 hours, and then dry-crush until the average particle size is 5 μm, to obtain the pre-calcined powder as the initial permanent magnet ferrite seed crystals;
[0065] (2) Prepare permanent ferrite raw materials, including iron source iron oxide with a purity of ≥99.0wt% and an average particle size of 1.6μm, strontium source strontium carbonate with a purity of ≥97.0wt% and an average particle size of 1.8μm (the main impurities include BaCO3≤1.0wt% and CaCO3≤0.6wt%), and calcium carbonate as a dopant containing calcium element with a purity of ≥98.5wt% and an average particle size of 1.5μm. The chemical formula of the permanent ferrite generated according to the theory of permanent ferrite raw materials is Sr 1-x Ca x Fe 2n O 19 , and 0.05≤x≤0.4, 5.5≤n≤6.0 are measured and mixed, and at the same time, the obtained initial permanent magnet ferrite seed crystals (as shown in Table 1) are added according to 1% to 10% of the total mass of the permanent magnet ferrite raw material, and wet ball milling is performed in a ball mill for 5 hours to obtain a first slurry with an average particle size of 0.85μm; the first slurry is dried in an oven, and then balled to obtain a ball-forming material;
[0066] (3) pre-calcining the pelletizing material at 1140° C. for 1.5 hours in an oxygen-containing atmosphere and then dry-crushing the pelletizing material to obtain a permanent magnet ferrite main phase material (pre-calcined material), which is dry-crushed to obtain 450 g of crushed material;
[0067] (4) mixing the pulverized material with a secondary additive, wherein the secondary additive includes SiO2, CaCO3 and Cr2O3, and the amount thereof is 0.5%, 0.75% and 0.4% of the mass of the pulverized material, respectively, and then adding 680 mL of tap water to wet grind the mixture in a ball mill for 20 hours until the average particle size is 0.74 μm, and adjusting the water content by using tap water to obtain a second slurry with a solid content of 70 wt%, and then subjecting the second slurry to magnetic field molding at a magnetic field strength of 11000 Oe to obtain a molded body; the molded body is a cylinder with a diameter of 43.2 mm and a height of 12 mm, and the molding pressure is 10 MPa;
[0068] (5) The obtained molded body is first sintered at 300°C for 1 hour, and then the temperature is increased at a rate of 150°C / hr, and a second sintering is performed in air at 1220°C for 1.5 hours to obtain a permanent magnet ferrite material.
[0069] Characterization and Testing I
[0070] The upper and lower surfaces of the permanent magnet ferrite material obtained in Example 1 were ground, and the residual magnetic induction intensity (Br), coercive force (Hcb), intrinsic coercive force (Hcj) and maximum magnetic energy product (BH) m at room temperature (20°C) were measured. The results are shown in Table 1.
[0071] Table 1
[0072]
[0073] It can be seen from Table 1 that by optimizing and adjusting the formula and adding different proportions of ferrite powder as crystallization seeds, relatively excellent comprehensive magnetic properties can be obtained under certain process technology conditions.
[0074] Example 2
[0075] This embodiment provides a method for preparing a permanent magnet ferrite. Compared with Example 1, this embodiment adjusts the average particle size of the initial permanent magnet ferrite seed crystals in step (1), adjusts the amount of the initial permanent magnet ferrite seed crystals added in step (2), and adjusts the pre-firing temperature in step (3), as shown in Table 2. Except for the above, other conditions are exactly the same as those in Example 1.
[0076] Characterization and Testing Ⅱ
[0077] The upper and lower surfaces of the permanent magnet ferrite material obtained in Example 2 were ground, and the residual magnetic induction intensity (Br), coercive force (Hcb), intrinsic coercive force (Hcj) and maximum magnetic energy product (BH) m at room temperature (20°C) were measured. The results are shown in Table 2.
[0078] Table 2
[0079]
[0080] It can be seen from Table 2 that after optimizing and adjusting the formula, adding different proportions of ferrite powder as crystallization seeds, under certain process technology conditions, adding more than 2% can obtain relatively excellent comprehensive magnetic properties.
[0081] Examples 3 and 4
[0082] The present embodiment provides a method for preparing a permanent magnet ferrite. Compared with the embodiment 1, the present embodiment does not perform the preparation of the initial permanent magnet ferrite seed crystal in step (1). Instead, in the embodiment 3, a part of the permanent magnet ferrite main phase material (pre-sintered material) obtained in the step (3) of the embodiment 1 is used to be re-crushed to an average particle size of 5.8 μm as a permanent magnet ferrite seed crystal. In the embodiment 4, the permanent magnet ferrite material obtained in the embodiment 1 is used to be re-crushed to an average particle size of 2.8 μm as a permanent magnet ferrite seed crystal. At the same time, the addition amount of the permanent magnet ferrite seed crystal in the step (2) of the embodiment 3 and the embodiment 4 is adjusted, and the pre-sintering temperature in the step (3) is adjusted. The specific conditions are shown in Table 3. Except for the above, the other conditions are exactly the same as those in the embodiment 1.
[0083] Comparative Example 1
[0084] This comparative example provides a method for preparing a permanent magnetic ferrite. The method does not carry out step (1) and does not use any permanent magnetic ferrite seed crystals. Except for the above, other conditions are exactly the same as those in Example 1.
[0085] Characterization and Testing III
[0086] The upper and lower surfaces of the permanent magnet ferrite materials obtained in Example 3, Example 4 and Comparative Example 1 were ground, and their residual magnetic induction intensity (Br), coercive force (Hcb), intrinsic coercive force (Hcj) and maximum magnetic energy product (BH) m at room temperature (20°C) were measured. The results are shown in Table 3.
[0087] Table 3
[0088]
[0089] It can be seen from Table 3 that after optimizing and adjusting the formula, adding different proportions of ferrite powder as crystallization seeds, under certain process technology conditions, adding more than 2% can obtain relatively excellent comprehensive magnetic properties.
[0090] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0091] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0092] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A method for preparing a permanent magnetic ferrite material, characterized in that: The preparation method comprises: A permanent magnet ferrite seed crystal is provided, the permanent magnet ferrite seed crystal is mixed with a permanent magnet ferrite raw material, and pre-sintering and sintering are performed in sequence to obtain a permanent magnet ferrite material.
2. The preparation method according to claim 1, characterized in that: The permanent magnet ferrite seed crystals include permanent magnet ferrite pre-sintered powder and / or waste permanent magnet ferrite material powder; Preferably, the average particle size of the permanent magnet ferrite seed crystal is 0.8 to 10 μm, preferably 1 to 5 μm; Preferably, the amount of the permanent ferrite seed crystals used accounts for 1% to 10% of the total mass of the permanent ferrite raw material, and preferably 2% to 5%.
3. The preparation method according to claim 1 or 2, characterized in that: The permanent ferrite theoretically generated from the permanent ferrite raw material and the permanent ferrite seed crystal belong to the same permanent ferrite system; Preferably, the permanent magnet ferrite system comprises strontium ferrite without lanthanum and cobalt, barium ferrite without lanthanum and cobalt, or barium strontium ferrite without lanthanum and cobalt; Preferably, the chemical formula of the lanthanum-free cobalt-free strontium ferrite comprises SrFe 2n O 19 , and 5.5≤n≤6.0; the permanent magnet ferrite raw material includes an iron source and a strontium source; Preferably, the iron source includes red iron; Preferably, the strontium source comprises strontium carbonate.
4. The preparation method according to claim 3, characterized in that: The chemical formula of the lanthanum-free cobalt-free strontium ferrite includes Sr 1-x M x Fe 2n O 19 , M is a doping element, M includes Ca, and 0.05≤x≤0.4, 5.5≤n≤6.0; the permanent magnet ferrite raw material also includes a dopant containing M; Preferably, the dopant containing M includes calcium carbonate.
5. The preparation method according to any one of claims 1 to 4, characterized in that: The average particle size of the permanent ferrite raw material is less than 2 μm; Preferably, the mixing method comprises wet mixing for 3 to 5 hours to obtain a first slurry with an average particle size of 0.6 to 1 μm, drying the first slurry and then forming a pellet to obtain a pelletized material, and pre-calcining the pelletized material; Preferably, the pre-firing is carried out in an oxygen-containing atmosphere, preferably in air; Preferably, the pre-calcination temperature is 1100-1300° C. and the time is 0.5-3 hr.
6. The preparation method according to any one of claims 1 to 5, characterized in that: After the pre-sintering, dry pulverization is performed to obtain a permanent magnet ferrite main phase material, which is then sintered and / or used as the permanent magnet ferrite seed crystal; Preferably, before the sintering, the permanent magnet ferrite main phase material is first mixed with a secondary additive and wet-ground to obtain a second slurry, the second slurry is molded to obtain a molded body, and the molded body is sintered; Preferably, the secondary additive includes at least one of SiO2, CaCO3, Al2O3, Cr2O3, ZnO, SrCO3 or H3BO3; Preferably, the total amount of the secondary additives accounts for 1.0% to 5.0% of the mass of the permanent ferrite main phase material; Preferably, the average particle size of the secondary additive is less than 2 μm; Preferably, the second slurry has an average particle size of 0.6 to 1 μm and a solid content of 65 wt% to 80 wt%; Preferably, the forming method comprises magnetic field forming; Preferably, the magnetic field strength of the magnetic field forming is greater than 10000 Oe.
7. The preparation method according to any one of claims 1 to 6, characterized in that: The sintering method comprises first sintering at 100-600°C for 0.5-2 hours, and then second sintering at 1180-1230°C for 0.5-3 hours; Preferably, the second sintering is performed in an oxygen-containing atmosphere, preferably in air.
8. The preparation method according to any one of claims 1 to 7, characterized in that: The preparation method comprises: (1) Synthesizing an initial permanent magnet ferrite seed crystal, wherein the initial permanent magnet ferrite seed crystal is a pre-sintered powder of strontium ferrite without lanthanum and cobalt, wherein the chemical formula of the strontium ferrite without lanthanum and cobalt is SrFe 2n O 19 , and 5.5≤n≤6.0, preparing the raw materials of the initial permanent magnet ferrite seed crystals, including iron source iron oxide and strontium source strontium carbonate, and measuring and mixing them according to the chemical formula, and then wet grinding to obtain an initial slurry with an average particle size of 0.6 to 1 μm, and pre-calcining the initial slurry at 1100 to 1300° C. in air for 0.5 to 3 hours, and then dry-crushing until the average particle size is 0.8 to 10 μm, to obtain the pre-calcined powder as the initial permanent magnet ferrite seed crystals; (2) Prepare permanent ferrite raw materials, including iron source iron oxide, strontium source strontium carbonate and calcium carbonate containing calcium element dopant, according to the chemical formula Sr 1-x Ca x Fe 2n O 19 , and 0.05≤x≤0.4, 5.5≤n≤6.0 are measured and mixed, and at the same time, the initial permanent magnet ferrite seed crystals are added according to 1% to 10% of the total mass of the permanent magnet ferrite raw material for wet mixing for 3 to 5 hours to obtain a first slurry with an average particle size of 0.6 to 1 μm; the first slurry is dried and pelletized to obtain a pelletizing material, and the pelletizing material is (3) pre-calcining the pelletizing material at 1100-1300° C. in an oxygen-containing atmosphere for 0.5-3 hours and then dry-crushing the pelletizing material to obtain a permanent magnet ferrite main phase material, using a portion of the obtained permanent magnet ferrite main phase material for subsequent sintering, and re-crushing another portion of the obtained permanent magnet ferrite main phase material to an average particle size of 0.8-10 μm to serve as permanent magnet ferrite seed crystals; (4) mixing the permanent magnet ferrite main phase material for sintering with a secondary additive, wherein the secondary additive includes at least one of SiO2, CaCO3, Al2O3, Cr2O3, ZnO, SrCO3 or H3BO3, and the total amount of the secondary additive accounts for 1.0% to 5.0% of the mass of the permanent magnet ferrite main phase material for sintering, and performing wet grinding to obtain a second slurry with an average particle size of 0.6 to 1 μm and a solid content of 65wt% to 80wt%, and then performing magnetic field molding at a magnetic field strength of >10000Oe to obtain a molded body; (5) The obtained molded body is first sintered at 100-600°C for 0.5-2 hours, and then second sintered at 1180-1230°C in air for 0.5-3 hours to obtain a permanent magnet ferrite material.
9. A permanent magnet ferrite material, characterized in that: Obtained according to the preparation method according to any one of claims 1 to 8.
10. Use of the permanent magnetic ferrite material according to claim 9, characterized in that: The uses include electric motors.
Citation Information
Patent Citations
Preparation method of high-performance sintering permanent magnetic ferrite magnet
CN102942357A
Process for forming high-orientation dry-press permanent magnetic ferrite
CN103304229A
High-performance La-Co-free permanent magnetic ferrite material and preparation method thereof
CN111377724A
Magnet powder, sintered magnet, bonded magnet, and magnetic recording medium
CN1150315A
Productive method of sintering anisotropic permanent magnetic ferrite
CN1450022A