Preparation method for in-situ synthesis of boron nitride fiber reinforced and toughened boron nitride ceramic
By adding non-metal oxide toughening agent to boron nitride ceramics in situ to generate boron nitride fibers, the problems of complex processes and performance losses in the existing technology are solved, and the toughness and strength of boron nitride ceramics are improved. in high stress environment.
Patent Information
- Application Number
- CN202411011066.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the prior art, when improving the toughness of boron nitride ceramics, complex synthesis processes are often required and may affect its other properties, such as reducing insulation and thermal stability, and it is difficult to improve toughness and strength at the same time.
Boron nitride fibers are generated in situ by adding a non-metal oxide toughening agent to enhance the interface bonding of boron nitride ceramic-based materials, and improve the interface crack propagation resistance. The simple synthesis process does not affect the electrical conductivity and thermal stability of the ceramics.
It realizes that the toughness and strength of the boron nitride ceramics are significantly improved without changing other properties, making it possible to apply in high stress environments, and has excellent comprehensive performance.
Smart Images

Figure CN118955159A_ABST
Abstract
Description
Technical Field
[0001] The technical solution mainly relates to the field of ceramic engineering and science, and specifically to a method for preparing in-situ synthesized boron nitride fiber reinforced and toughened boron nitride ceramics. Background Art
[0002] Boron nitride is an important high-performance ceramic material with excellent properties such as high temperature resistance, oxidation resistance, and corrosion resistance. It is widely used in high-end fields such as aerospace, nuclear energy, and electronics. However, the inherent brittleness of boron nitride ceramics limits its application in certain high-stress environments. In order to solve this problem, researchers began to explore improving the toughness of boron nitride ceramics by adding toughening agents. Among them, an effective method is to generate boron nitride fibers in situ by adding toughening agents of non-metallic oxides, enhance the interface bonding with boron nitride ceramic-based materials, thereby improving the interfacial crack propagation resistance and achieving enhancement and toughening of boron nitride ceramic-based materials.
[0003] The existing solution is mainly to enhance the toughness of boron nitride ceramics by adding second phase particles or whiskers. For example, the toughness of boron nitride ceramics can be enhanced by adding nanomaterials such as carbon nanotubes and silicon nanowires. For example, Chinese patent ZL202310759189.1 discloses a flexible high thermal conductivity boron nitride ceramic-based film and its preparation method, which uses boron nitride precursor whiskers, one-dimensional flexible high thermal conductivity materials and binder polyvinyl pyrrolidone as raw materials, wherein the one-dimensional flexible high thermal conductivity material is carbon nanotubes or boron nitride nanotubes. In addition, there are some studies that improve the toughness of boron nitride ceramics by adding toughening agents of metal oxides or non-metal oxides.
[0004] Although existing technologies have improved the toughness of boron nitride ceramics to a certain extent, these methods often require complex synthesis processes and may affect other properties of boron nitride ceramics, such as reducing the insulation and thermal stability of the ceramics. In addition, these methods can often only improve the toughness of boron nitride ceramics to a certain extent, but cannot improve its strength at the same time. Therefore, how to effectively improve the toughness of boron nitride ceramics without changing other properties remains a challenge. Summary of the invention
[0005] In order to overcome the shortcomings of the prior art, the present invention generates boron nitride fibers in situ by adding a toughening agent of non-metallic oxides, strengthens the interface bonding with the boron nitride ceramic-based material, and improves the interface crack propagation resistance through crack deflection, crack bridging, grain pullout and other effects, thereby enhancing and toughening the boron nitride ceramic-based material, and does not affect the insulation of the boron nitride ceramic itself, and improves the toughness of the boron nitride ceramic through a simple synthesis process. Specifically, the present invention is achieved through the following technical solutions:
[0006] A method for preparing in-situ synthesized boron nitride fiber reinforced and toughened boron nitride ceramics, the preparation steps of the boron nitride ceramics are:
[0007] A method for preparing in-situ synthesized boron nitride fiber reinforced and toughened boron nitride ceramics, the preparation steps of the boron nitride ceramics are:
[0008] S1: Raw material ratio: select hexagonal boron nitride with a mass ratio of 90-99wt.%, a purity of 98.0-99.9%, a particle size of 0.5-15μm, and a toughening agent with a mass ratio of 1-10wt.% as raw materials;
[0009] S2: ball milling: adding the raw materials to ball milling media and ball milling beads and putting them into a ball mill for ball milling;
[0010] S3: Filtration: filtering the ball-milled slurry through a sieve to obtain a slurry;
[0011] S4: Drying and sieving: The slurry is placed in a drying oven at 90-110° C. and dried for 12-24 hours. The dried raw material is crushed and ground and then sieved through a 60-400 mesh sieve to form a powder;
[0012] S5: Sintering: The obtained powder is placed in a mold, put into a hot pressing sintering furnace, nitrogen or ammonia is introduced, and sintered under sintering conditions to obtain boron nitride fiber reinforced and toughened boron nitride ceramics.
[0013] Furthermore, the toughening agent is selected from one of ammonium borate, sodium tetraborate, boric acid, borazine, boric anhydride, ethyl borate, and trimethyl borate.
[0014] Furthermore, the ball mill is selected from a grinding mill and a planetary ball mill, and the raw material is ball milled in the ball mill at a rotation speed of 200 to 600 r / min for 0.5 to 4 hours.
[0015] Furthermore, the ball milling medium is selected from one of distilled water and anhydrous ethanol, wherein the mass ratio of raw materials, ball milling medium and ball milling beads is 1:5:8.
[0016] Furthermore, the sintering conditions are: 1700-2000° C., 15-25 MPa pressure, and heat preservation for 2-4 hours.
[0017] The beneficial effects that can be achieved by adopting the technical solution of the present invention are:
[0018] 1. The present invention generates boron nitride fibers in situ by adding a toughening agent of non-metallic oxide, which can not only enhance the interface bonding with the boron nitride ceramic-based material, but also improve the interface crack propagation resistance through crack deflection, crack bridging, grain pullout and other effects, thereby enhancing and toughening the boron nitride ceramic-based material.
[0019] 2. The preparation method of the present invention is simple and does not require a complicated synthesis process, which greatly reduces the production cost. At the same time, the preparation method of the present invention will not affect other properties of boron nitride ceramics, such as electrical conductivity, thermal stability, etc.
[0020] 3. The boron nitride ceramics of the present invention have excellent comprehensive properties, and their performance parameter ranges are: BN purity is 98.0% to 99.9%, density is 1.90 to 2.18 g / cm 3 , flexural strength is 56~230MPa, fracture toughness is 0.8~3.0MPa·m 1 / 2 , dielectric constant is 3.0~3.7, and thermal conductivity is 45~70W / (m·k).
[0021] 4. The present invention further improves the toughness of boron nitride ceramics, making it possible to use them in high-stress environments such as aerospace and nuclear energy fields. Since the insulation performance is not affected, it is of great significance to the development of the electronics field. Therefore, this technical solution has broad market demand and good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is the XRD pattern of the product of Example 1 of the present invention;
[0023] Figure 2 This is the XRD spectrum of the product of Comparative Example 1 of the present invention;
[0024] Figure 3 This is the XRD pattern of the product of Example 2 of the present invention;
[0025] Figure 4 This is the XRD spectrum of the product of Comparative Example 2 of the present invention. DETAILED DESCRIPTION
[0026] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0027] Example 1
[0028] The purity of BN produced in this embodiment is 99.3% and the density is 2.10 g / cm 3 , flexural strength is 110MPa, fracture toughness is 1.09MPa·m 1 / 2 , boron nitride ceramics with a dielectric constant of 3.4 and a thermal conductivity of 48W / (m·k).
[0029] Specifically, the method in this embodiment includes the following steps:
[0030] S1: Raw material ratio: The raw material is selected as hexagonal boron nitride powder with a mass ratio of 99.0wt.%, a purity of 98.8% and a particle size of 0.5μm. The toughening agent is boric acid, and its mass ratio is 1.0wt.%.
[0031] S2: Ball milling: The ball milling beads are silicon nitride balls with a diameter of 5 mm, and the solvent is distilled water. The raw materials, ball milling beads, and solvent are weighed in a mass ratio of 1:5:8 and put into a ball mill. The ball mill is milled at a speed of 400 r / min for 2 hours.
[0032] S3: Filtration: Filter the ball-milled slurry with a sieve.
[0033] S4: Drying and sieving: Place the slurry in a drying oven at 110°C and dry for 24 hours. After crushing and grinding, pass through a 100-mesh sieve into powder.
[0034] S5: Sintering: Place the raw material powder in a graphite mold, put it into a vacuum hot pressing sintering furnace with nitrogen atmosphere, keep it at 1800°C for 2.5 hours, and pressurize it at 18MPa to obtain boron nitride ceramics.
[0035] Comparative Example 1
[0036] The purity of BN produced in this embodiment is 99.5% and the density is 2.14 g / cm 3 , flexural strength is 88MPa, fracture toughness is 0.92MPa·m 1 / 2 , boron nitride ceramics with a dielectric constant of 3.1 and a thermal conductivity of 50W / (m·k).
[0037] Specifically, the method in this embodiment includes the following steps:
[0038] S1: Raw material ratio: The raw material is selected from hexagonal boron nitride powder with a purity of 98.8% and a particle size of 0.5 μm, without adding toughening agent.
[0039] S2: Ball milling: The ball milling beads are silicon nitride balls with a diameter of 5 mm, and the solvent is distilled water. The raw materials, ball milling beads, and solvent are weighed in a mass ratio of 1:5:8 and put into a ball mill, and ball milled at a speed of 400 r / min for 2 h.
[0040] S3: Filtration: Filter the ball-milled slurry with a sieve.
[0041] S4: Drying and sieving: Place the slurry in a drying oven at 110°C and dry for 24 hours. After crushing and grinding, pass through a 100-mesh sieve into powder.
[0042] S5: placing the raw material powder in a graphite mold, putting it into a vacuum hot pressing sintering furnace with an ammonia atmosphere, keeping the temperature at 1800° C. for 2.5 hours, and firing it at a pressure of 18 MPa to obtain boron nitride ceramics.
[0043] Example 2
[0044] The oxygen content of this embodiment is 99.2% and the density is 2.13g / cm 3 , flexural strength is 225MPa, fracture toughness is 2.99MPa·m 1 / 2 , boron nitride ceramics with a dielectric constant of 3.7 and a thermal conductivity of 57W / (m·k).
[0045] Specifically, the method in this embodiment includes the following steps:
[0046] S1: Raw material ratio: The raw material is selected as hexagonal boron nitride powder with a mass ratio of 95.0wt.%, a purity of 98.8%, and a particle size of 8μm, and the toughening agent is selected as borazine, and its mass ratio is 5.0wt.%.
[0047] S2: Ball milling: The ball milling beads are zirconia balls with a diameter of 4 mm, and the solvent is anhydrous ethanol. The raw materials, ball milling beads, and solvent are weighed in a mass ratio of 1:5:8 and put into a ball mill, and the ball milling is carried out at a speed of 400 r / min for 2 h.
[0048] S3: Filtration: Filter the ball-milled slurry with a sieve.
[0049] S4: Drying and sieving: Place the slurry in a drying oven at 110°C and dry for 24 hours. After crushing and grinding, pass through a 200-mesh sieve into powder.
[0050] S5: Sintering: Place the raw material powder in a graphite mold, put it into a vacuum hot pressing sintering furnace with nitrogen atmosphere, keep it at 2000°C for 4 hours, and pressurize it at 20MPa to obtain boron nitride ceramics.
[0051] Comparative Example 2
[0052] The oxygen content of this embodiment is 99.1%, and the density is 2.09g / cm 3 , flexural strength is 185MPa, fracture toughness is 2.86MPa·m 1 / 2 , boron nitride ceramics with a dielectric constant of 3.5 and a thermal conductivity of 55W / (m·k).
[0053] S1: Raw material ratio: The raw material is selected as hexagonal boron nitride powder with a mass ratio of 98.0wt.%, a purity of 98.8%, and a particle size of 8μm, and the toughening agent is selected as borazine, and its mass ratio is 2.0wt.%.
[0054] S2: Ball milling: The ball milling beads are zirconia balls with a diameter of 4 mm, and the solvent is anhydrous ethanol. The raw materials, ball milling beads, and solvent are weighed in a mass ratio of 1:5:8 and put into a ball mill, and the ball milling is carried out at a speed of 400 r / min for 2 h.
[0055] S3: Filtration: Filter the ball-milled slurry with a sieve.
[0056] S4: Drying and sieving: Place the slurry in a drying oven at 110°C and dry for 24 hours. After crushing and grinding, pass through a 200-mesh sieve into powder.
[0057] S5: Sintering: Place the raw material powder in a graphite mold, put it into a vacuum hot pressing sintering furnace with nitrogen atmosphere, keep it at 2000°C for 4 hours, and pressurize it at 20MPa to obtain boron nitride ceramics.
[0058] The preparation conditions and performance comparison of the boron nitride ceramics obtained in Examples 1 and 2 and Comparative Examples 1 and 2 are shown in Table 1.
[0059] Table 1
[0060]
[0061] The results of Example 1 and Comparative Example 1 show that the boron nitride ceramics with the non-metallic oxide toughening agent added according to the scheme of the present invention are significantly superior to the boron nitride ceramics without the non-metallic oxide toughening agent in terms of flexural strength, fracture toughness and dielectric constant. The results of Example 2 and Comparative Example 2 show that the boron nitride ceramics with a higher content of toughening agent have higher flexural strength. In general, the present invention not only improves the toughness of boron nitride ceramics, but also does not affect its original electrical conductivity, thermal stability and other properties, and has obvious advantages over the prior art.
[0062] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing in-situ synthesized boron nitride fiber reinforced and toughened boron nitride ceramics, characterized in that: The preparation steps of the boron nitride ceramic are: S1: Raw material ratio: select hexagonal boron nitride with a mass ratio of 90-99wt.%, a purity of 98.0-99.9%, a particle size of 0.5-15μm, and a toughening agent with a mass ratio of 1-10wt.% as raw materials; S2: ball milling: adding the raw materials to ball milling media and ball milling beads and putting them into a ball mill for ball milling; S3: Filtration: filtering the ball-milled slurry through a sieve to obtain a slurry; S4: Drying and sieving: The slurry is placed in a drying oven at 90-110° C. and dried for 12-24 hours. The dried raw material is crushed and ground and then sieved through a 60-400 mesh sieve to form a powder; S5: Sintering: The obtained powder is placed in a mold, put into a hot pressing sintering furnace, nitrogen or ammonia is introduced, and sintered under sintering conditions to obtain boron nitride fiber reinforced and toughened boron nitride ceramics.
2. The preparation method according to claim 1, characterized in that: The toughening agent is selected from one of ammonium borate, sodium tetraborate, boric acid, borazine, boric anhydride, ethyl borate and trimethyl borate.
3. The preparation method according to any one of claims 1-2, characterized in that: The ball mill is selected from a grinding mill and a planetary ball mill, and the raw material is ball-milled in the ball mill at a speed of 200 to 600 r / min for 0.5 to 4 hours.
4. The preparation method according to any one of claims 1-2, characterized in that: The ball milling medium is selected from distilled water and anhydrous ethanol, wherein the mass ratio of the raw material, the ball milling medium and the ball milling beads is 1:5:
8.
5. The preparation method according to any one of claims 1-2, characterized in that: The sintering conditions are: 1700-2000° C., 15-25 MPa pressure, and heat preservation for 2-4 hours.
Citation Information
Patent Citations
Boron nitride porous ceramic thermal insulation material, preparation and use thereof
CN101323536A
Preparation method of boron nitride fiber enhanced nitride ceramic-based composite material
CN106986658A
Silicon nitride-based composite material and preparation method thereof
CN108395257A
Preparation method of SiCf / SiC ceramic composite material through 3D moulding
CN109851362A
Silicon nitride nanometer fiber reinforced boron nitride ceramic, and preparation method thereof
CN110330349A
Cited By
Preparation method of high-strength heat insulation tile composite material
CN120664884A