Preparation method of anti-oxidation coating on surface of C / C composite material, anti-oxidation C / C composite material and application of anti-oxidation C / C composite material

By forming a MoSi2@SiO2 antioxidant coating on the surface of C/C composite materials, the oxidation problem in high-temperature environment is solved, the high-temperature stability and oxidation resistance of the material are improved, the coating preparation process is simplified, and it is suitable for high-temperature applications.

CN118955182AInactive Publication Date: 2024-11-15ZHEJIANG XINGHUI NEW MATERIALS TECHNOLOGY CO LTD

Patent Information

Application Number
CN202411448281.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-17
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The lack of effective high-temperature and ultra-high-temperature antioxidant coatings in the prior art leads to oxidation of C/C composite materials in a high-temperature environment, and the preparation process of existing antioxidant coatings is complicated.

Method used

MoSi2 is used as the seepage material to permeate the C/C composite material to form a MoSi2 protective layer, and electrostatically adsorb SiO2 to the surface of MoSi2, and finally heat treatment is carried out to form a MoSi2@SiO2 antioxidant coating to enhance the thickness and uniformity of the coating. A glassy dense protective layer is formed.

Benefits of technology

It significantly improves the high temperature stability and oxidation resistance of C/C composite materials, and can avoid oxidation in an environment from room temperature to 1500℃. It is suitable for aerospace missiles, rocket engine nozzle throat linings, aircraft brake pairs and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention provides a preparation method of an anti-oxidation coating on the surface of a C / C composite material, the anti-oxidation C / C composite material and application of the anti-oxidation C / C composite material, and relates to the technical field of C / C composites.The preparation method comprises the following steps that firstly, MoSi2 is adopted as a permeation material to conduct permeation treatment on the C / C composite material, then SiO2 is adsorbed to the surface of MoSi2, then heat treatment is conducted, and the C / C composite material is obtained. Therefore, the anti-oxidation coating is formed on the surface of the C / C composite material. The preparation method solves the technical problems that in the prior art, the C / C composite material is lack of high-temperature and ultrahigh-temperature anti-oxidation coatings, and meanwhile, the preparation process of the anti-oxidation coatings is complex, and the technical effect of remarkably improving the high-temperature stability and the oxidation resistance of the C / C composite material is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of C / C composite materials, and in particular to a method for preparing an anti-oxidation coating on the surface of a C / C composite material, an anti-oxidation C / C composite material and applications thereof. Background Art

[0002] C / C composite materials have the characteristics of high specific strength, high specific modulus, high fracture toughness, low density, good thermal conductivity, good thermal shock resistance, ablation resistance and good chemical stability. In particular, they have excellent high-temperature performance and can maintain high strength even in a non-oxidizing environment with an operating temperature exceeding 2200°C. They are currently the most competitive high-temperature structural materials and have been used in high-tech fields such as aerospace missiles, rocket engine nozzle throat liners and aircraft brake assemblies.

[0003] However, in an oxidizing atmosphere above 450°C, C / C composites will oxidize. Studies have shown that if the material loses 1% of its mass fraction through oxidation, its strength will decrease by more than 10%. Therefore, the anti-oxidation protection of C / C composites is the key to their widespread application. Domestic and foreign scholars have conducted a lot of research on the anti-oxidation protection of C / C composites at low, medium and high temperatures; the prior art CN200410003042.7 discloses an anti-oxidation coating of a series of C / C composites in the low and medium temperature range, which has been successfully applied to aircraft brake pairs and aero-engine shaft seals. However, the research on high-temperature and ultra-high-temperature anti-oxidation coatings of C / C composites has not made a breakthrough, and there is a lack of engineering applications; the prior art CN115745663A discloses a method for preparing a Glass-MoSi2-SiC composite anti-oxidation coating on the surface of a carbon / carbon composite material. Although it can greatly improve the anti-oxidation performance of the carbon / carbon composite material, it requires the preparation of a three-layer coating structure, and the process is complicated.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] One of the purposes of the present invention is to provide a method for preparing an anti-oxidation coating on the surface of a C / C composite material, which solves the technical problems in the prior art that the C / C composite material lacks high-temperature and ultra-high-temperature anti-oxidation coatings and the preparation process of the anti-oxidation coating is complicated, thereby achieving the technical effect of significantly improving the high-temperature stability and anti-oxidation properties of the C / C composite material.

[0006] A second object of the present invention is to provide an oxidation-resistant C / C composite material that can avoid oxidation in the entire temperature range from room temperature to 1500°C in an air atmosphere.

[0007] The third object of the present invention is to provide an application of an antioxidant C / C composite material that can achieve outstanding application effects.

[0008] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted: In a first aspect, a method for preparing an anti-oxidation coating on the surface of a C / C composite material comprises the following steps: First, MoSi2 is used as the infiltration material to infiltrate the C / C composite material, and then SiO2 is adsorbed onto the surface of MoSi2, and then heat treatment is performed to form an anti-oxidation coating on the surface of the C / C composite material; The temperature of the heat treatment is 1000°C-1300°C.

[0009] Furthermore, the particle size of the MoSi2 is 100 mesh-300 mesh.

[0010] Furthermore, the temperature of the infiltration treatment is 1600°C-2200°C.

[0011] Further, the infiltration treatment comprises the following steps: The C / C composite material is buried in MoSi2 and infiltrated under a protective atmosphere; Preferably, the temperature process of the infiltration treatment includes: First keep warm at 1600℃-1800℃ for 1h-3h, then keep warm at 2000℃-2200℃ for 4h-6h.

[0012] Furthermore, the SiO2 is adsorbed onto the surface of MoSi2 by electrostatic adsorption; Preferably, the electrostatic adsorbent used in the electrostatic adsorption comprises tetrabutylammonium bromide; Preferably, the environmental condition of the electrostatic adsorption is alkaline; Preferably, the reagent for creating the alkaline environment includes aqueous ammonia.

[0013] Furthermore, the method of adsorbing SiO2 onto the surface of MoSi2 by electrostatic adsorption comprises the following steps: The C / C composite material after infiltration treatment is immersed in a dispersion liquid, and tetraethyl orthosilicate is added and mixed, so that negatively charged SiO2 oligomers are adsorbed on the MoSi2 surface; Preferably, the ratio of ethanol, ammonia water and tetrabutylammonium bromide solution in the dispersion is 100mL~300mL: 6mL~12mL: 10mL~30mL; Preferably, the ratio of ethanol, ammonia water and tetrabutylammonium bromide solution in the dispersion is 150 mL: 8 mL: 15 mL.

[0014] Further, the size of the C / C composite material is 20 mm×20 mm×10 mm; Preferably, the amount of tetraethyl orthosilicate is 40 mL -80 mL; Preferably, the tetraethyl orthosilicate is added dropwise; Preferably, the speed of adding dropwise is 1 mL every 2 min to 4 min.

[0015] Furthermore, the atmosphere of the heat treatment includes air.

[0016] In a second aspect, an antioxidant C / C composite material is prepared by any of the preparation methods described above.

[0017] In a third aspect, an application of the above-mentioned antioxidant C / C composite material in aerospace missiles, rocket engine nozzle throat linings and aircraft brake pairs.

[0018] Compared with the prior art, the present invention has at least the following beneficial effects: The method for preparing the anti-oxidation coating on the surface of a C / C composite material provided by the present invention comprises the following steps: firstly, a MoSi2 protective layer is generated on the surface of the C / C composite material by an embedding method, and high-temperature oxidation is performed to generate an oxide film layer on the surface of the MoSi2; then, SiO2 is adsorbed onto the surface of MoSi2 particles by electrostatic adsorption to seal cracks and the surface of the coating, thereby increasing the thickness and uniformity of the coating; finally, the MoSi2 coating layer is softened by heat treatment to form a glassy dense protective layer, thereby forming a MoSi2@SiO2 anti-oxidation coating, thereby significantly improving the high-temperature stability and anti-oxidation property of the C / C composite material.

[0019] The anti-oxidation C / C composite material provided by the present invention has a MoSi2@SiO2 high-temperature anti-oxidation coating on its surface with excellent infrared radiation performance, which can avoid oxidation in the entire temperature range from room temperature to 1500°C in an air atmosphere, and is of great significance for the application of C / C composite materials in various fields.

[0020] The application of the antioxidant C / C composite material provided by the present invention can achieve outstanding application effects. DETAILED DESCRIPTION

[0021] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] According to a first aspect of the present invention, there is provided a method for preparing an anti-oxidation coating on the surface of a C / C composite material, comprising the following steps: First, MoSi2 is used as the infiltration material to infiltrate the C / C composite material, and then SiO2 is adsorbed onto the surface of MoSi2, and then heat treatment is performed to form an anti-oxidation coating on the surface of the C / C composite material; The heat treatment temperature is 1000°C-1300°C, and typical but non-limiting temperatures are, for example, 1000°C, 1100°C, 1200°C, and 1300°C, which can soften the MoSi2 coating layer to form a glassy and dense protective layer, thereby effectively improving the high temperature stability and oxidation resistance of the material.

[0023] The present invention firstly generates a MoSi2 protective layer on the surface of the C / C composite material by an embedding method, and performs high-temperature oxidation to generate an oxide film layer on the surface of the MoSi2. Then, SiO2 is adsorbed onto the surface of the MoSi2 particles by electrostatic adsorption to seal the cracks and surface of the coating, thereby increasing the thickness and uniformity of the coating. Finally, the MoSi2 coating layer is softened by heat treatment to form a glassy dense protective layer, thereby forming a MoSi2@SiO2 anti-oxidation coating, thereby significantly improving the high-temperature stability and oxidation resistance of the C / C composite material.

[0024] In a preferred embodiment, the particle size of MoSi2 can be 100 mesh-300 mesh, and its typical but non-limiting particle size is, for example, 100 mesh, 120 mesh, 140 mesh, 160 mesh, 180 mesh, 200 mesh, 220 mesh, 240 mesh, 260 mesh, 280 mesh, and 300 mesh.

[0025] In a preferred embodiment, the high temperature insulation temperature of the infiltration treatment can be 1600°C-2200°C, and typical but non-limiting temperatures are, for example, 1600°C, 1700°C, 1800°C, 1900°C, 2000°C, 2100°C, and 2200°C.

[0026] The high-temperature insulation temperature section is close to the melting point of MoSi2, and the particle size of the MoSi2 infiltrate is small. Therefore, when the corresponding coating is prepared by the embedding method, MoSi2 will have a longer time to flow and diffuse, so that MoSi2 can be fully spread on the surface of the C / C composite material, and the formed coating will be more uniform and dense.

[0027] In a preferred embodiment, the infiltration treatment comprises the following steps: The C / C composite material is buried in MoSi2 and infiltrated under a protective atmosphere.

[0028] In the present invention, the infiltration material MoSi2 powder is placed in a carbon-carbon crucible, and the C / C composite material is buried in the infiltration material, and then the crucible is placed in a high-temperature furnace to perform infiltration treatment at high temperature in an Ar gas atmosphere.

[0029] In a preferred embodiment, the temperature process of the infiltration treatment includes: First keep warm at 1600℃-1800℃ for 1h-3h, then keep warm at 2000℃-2200℃ for 4h-6h.

[0030] In a preferred embodiment, SiO2 is adsorbed onto the MoSi2 surface by electrostatic adsorption.

[0031] The electrostatic adsorbent used in the electrostatic adsorption includes but is not limited to tetrabutylammonium bromide; the environmental condition of the electrostatic adsorption may be alkaline, and the reagents for creating the alkaline environment include but are not limited to ammonia water.

[0032] In a preferred embodiment, the method of adsorbing SiO2 onto the surface of MoSi2 by electrostatic adsorption comprises the following steps: The C / C composite material after infiltration treatment is immersed in a dispersion liquid, and tetraethyl orthosilicate is added and mixed, so that negatively charged SiO2 oligomers are adsorbed onto the MoSi2 surface.

[0033] In the present invention, anhydrous ethanol, ammonia water and tetrabutylammonium bromide solution are mixed, firstly mixed by magnetic stirring, and then dispersed by ultrasonic treatment, so as to obtain a uniformly mixed dispersion.

[0034] Using tetraethyl orthosilicate as a precursor and tetrabutylammonium bromide as an electrostatic adsorbent, negatively charged SiO2 oligomers in an alkaline environment can be adsorbed onto the surface of MoSi2 particles through electrostatic adsorption, thereby effectively sealing the cracks and surface of the coating and increasing the thickness and uniformity of the coating.

[0035] In a preferred embodiment, the ratio of ethanol, ammonia water and tetrabutylammonium bromide solution in the dispersion can be 100mL~300mL:6mL~12mL:10mL~30mL, and can be further preferably 150mL:8mL:15mL; wherein the mass concentration of ammonia water can be 31%, and the mass concentration of tetrabutylammonium bromide solution can be 30%.

[0036] In a preferred embodiment, the size of the C / C composite material may be 20 mm×20 mm×10 mm, but is not limited thereto.

[0037] It should be noted that before the preparation of the antioxidant coating, the surface of the C / C composite material can be polished with 400-mesh sandpaper, and then blown clean with an air gun after polishing, and then cleaned with an ultrasonic cleaner, and then dried to obtain the C / C composite material to be treated, which is more conducive to improving the preparation effect of the subsequent antioxidant coating.

[0038] In a preferred embodiment, the amount of tetraethyl orthosilicate used may be 40 mL-80 mL, and typical but non-limiting amounts thereof are, for example, 40 mL, 50 mL, 60 mL, 70 mL, and 80 mL.

[0039] In the present invention, the method of adding tetraethyl orthosilicate includes but is not limited to dropwise addition, and the speed of dropwise addition can be 1 mL every 2 minutes to 4 minutes.

[0040] In a preferred embodiment, the atmosphere for heat treatment includes but is not limited to air.

[0041] According to a second aspect of the present invention, there is provided an antioxidant C / C composite material prepared by any of the preparation methods described above.

[0042] The anti-oxidation C / C composite material provided by the present invention has a MoSi2@SiO2 high-temperature anti-oxidation coating on its surface with excellent infrared radiation performance, which can avoid oxidation in the entire temperature range from room temperature to 1500°C in an air atmosphere, and is of great significance for the application of C / C composite materials in various fields.

[0043] According to a third aspect of the present invention, there is provided a use of the above-mentioned antioxidant C / C composite material in aerospace missiles, rocket engine nozzle throat linings and aircraft brake pairs.

[0044] The application of the antioxidant C / C composite material provided by the present invention can achieve outstanding application effects.

[0045] The present invention is further described below by way of examples. Unless otherwise specified, the materials in the examples are prepared according to existing methods or directly purchased from the market.

[0046] Example 1 A method for preparing an anti-oxidation coating on the surface of a C / C composite material comprises the following steps: (a) The surface of the C / C composite material with a size of 20 mm × 20 mm × 10 mm was polished with 400-grit sandpaper, and after being polished flat, it was blown clean with an air gun, placed in an ultrasonic cleaner for 1 h, and then placed in an oven for drying at 150 °C to obtain sample A; (b) Putting 100-mesh MoSi2 powder as infiltration material into a carbon-carbon crucible, burying the sample A obtained in step (a) into the infiltration material, and placing it in a high-temperature furnace for infiltration treatment under an Ar gas atmosphere; wherein the temperature process of the infiltration treatment is: first keeping the temperature at 1600°C for 1 hour, and then keeping the temperature at 2000°C for 4 hours; after the infiltration treatment is completed, sample B is obtained; (c) placing anhydrous ethanol (100 mL), ammonia water (6 mL) and tetrabutylammonium bromide aqueous solution (10 mL) into a conical flask and mixing them into a solution, first magnetically stirring for 1 h, and then ultrasonically treating for 0.5 h to obtain a uniform dispersion; wherein the mass concentration of the ammonia water is 31%, and the mass concentration of the tetrabutylammonium bromide aqueous solution is 30%; (d) placing the sample B obtained in step (b) into the dispersion obtained in step (c), and placing the sample in a 50±5°C electric constant temperature water bath for magnetic stirring, while adding 40 mL of tetraethyl orthosilicate dropwise into the dispersion at a dropping speed of 1 mL every 4 min and a stirring speed of 700 rpm. After the dropping is completed, the stirring is stopped; (e) Take out sample B in step (d), place it in an oven, and dry it at 105±5℃ for 24h; (f) The sample dried in step (e) is heat treated in an air atmosphere at 1000° C. for 1 h to form a MoSi2@SiO2 high temperature antioxidant protective coating on the surface of the sample to obtain an antioxidant C / C composite material.

[0047] Example 2 The difference between this embodiment and embodiment 1 is that in step (b), the temperature process of the infiltration treatment is: firstly keeping the temperature at 1700°C for 2 hours, and then keeping the temperature at 2000°C for 4 hours; In step (c), the amounts of anhydrous ethanol, aqueous ammonia and aqueous tetrabutylammonium bromide solution used are 200 mL, 9 mL and 20 mL respectively; In step (f), the heat treatment temperature in air atmosphere is 1100°C; The rest are the same as in Example 1.

[0048] Example 3 The difference between this embodiment and embodiment 1 is that in step (b), the temperature process of the infiltration treatment is: firstly keeping the temperature at 1800°C for 3 hours, and then keeping the temperature at 2000°C for 4 hours; In step (c), the amounts of anhydrous ethanol, aqueous ammonia and aqueous tetrabutylammonium bromide solution used are 300 mL, 12 mL and 30 mL respectively; In step (f), the heat treatment temperature in air atmosphere is 1200°C; The rest are the same as in Example 1.

[0049] Example 4 The difference between this embodiment and embodiment 1 is that in step (b), the temperature process of the infiltration treatment is: firstly keeping the temperature at 1600°C for 1 hour, and then keeping the temperature at 2100°C for 5 hours; In step (d), the amount of tetraethyl orthosilicate is 60 mL, and the dropping speed is 1 mL every 3 minutes; In step (f), the heat treatment temperature in air atmosphere is 1100°C; The rest are the same as in Example 1.

[0050] Example 5 The difference between this embodiment and embodiment 1 is that in step (b), the temperature process of the infiltration treatment is: firstly keeping the temperature at 1600°C for 1 hour, and then keeping the temperature at 2200°C for 6 hours; In step (d), the amount of tetraethyl orthosilicate is 80 mL, and the dropping speed is 1 mL every 2 minutes; In step (f), the heat treatment temperature in air atmosphere is 1200°C; The rest are the same as in Example 1.

[0051] Example 6 The difference between this embodiment and embodiment 1 is that in step (b), 200-mesh MoSi2 powder is used as the infiltration material; The rest are the same as in Example 1.

[0052] Example 7 The difference between this embodiment and embodiment 1 is that in step (b), 200-mesh MoSi2 powder is used as the infiltration material; at the same time, the temperature process of the infiltration treatment is: first, keep the temperature at 1700°C for 2 hours, and then keep the temperature at 2000°C for 4 hours; In step (c), the amounts of anhydrous ethanol, aqueous ammonia and aqueous tetrabutylammonium bromide solution used are 200 mL, 9 mL and 20 mL respectively; In step (f), the heat treatment temperature in air atmosphere is 1100°C; The rest are the same as in Example 1.

[0053] Example 8 The difference between this embodiment and embodiment 1 is that in step (b), 200-mesh MoSi2 powder is used as the infiltration material; at the same time, the temperature process of the infiltration treatment is: first, keep the temperature at 1800°C for 3 hours, and then keep the temperature at 2000°C for 4 hours; In step (c), the amounts of anhydrous ethanol, aqueous ammonia and aqueous tetrabutylammonium bromide solution used are 300 mL, 12 mL and 30 mL respectively; In step (f), the heat treatment temperature in air atmosphere is 1200°C; The rest are the same as in Example 1.

[0054] Example 9 The difference between this embodiment and embodiment 1 is that in step (b), 200-mesh MoSi2 powder is used as the infiltration material; at the same time, the temperature process of the infiltration treatment is: first, keep the temperature at 1600°C for 1 hour, and then keep the temperature at 2100°C for 5 hours; In step (d), the amount of tetraethyl orthosilicate is 60 mL, and the dropping speed is 1 mL every 3 minutes; In step (f), the heat treatment temperature in air atmosphere is 1100°C; The rest are the same as in Example 1.

[0055] Example 10 The difference between this embodiment and embodiment 1 is that in step (b), 200-mesh MoSi2 powder is used as the infiltration material; at the same time, the temperature process of the infiltration treatment is: first, keep the temperature at 1600°C for 1 hour, and then keep the temperature at 2200°C for 6 hours; In step (d), the amount of tetraethyl orthosilicate is 80 mL, and the dropping speed is 1 mL every 2 minutes; In step (f), the heat treatment temperature in air atmosphere is 1200°C; The rest are the same as in Example 1.

[0056] Embodiment 11 The difference between this embodiment and embodiment 1 is that in step (b), 300-mesh MoSi2 powder is used as the infiltration material; The rest are the same as in Example 1.

[0057] Example 12 The difference between this embodiment and embodiment 1 is that in step (b), 300-mesh MoSi2 powder is used as the infiltration material; at the same time, the temperature process of the infiltration treatment is: first, keep the temperature at 1700°C for 2 hours, and then keep the temperature at 2000°C for 4 hours; In step (c), the amounts of anhydrous ethanol, aqueous ammonia and aqueous tetrabutylammonium bromide solution used are 200 mL, 9 mL and 20 mL respectively; In step (f), the heat treatment temperature in air atmosphere is 1100°C; The rest are the same as in Example 1.

[0058] Example 13 The difference between this embodiment and embodiment 1 is that in step (b), 300 mesh MoSi2 powder is used as the infiltration material; at the same time, the temperature process of the infiltration treatment is: firstly keep the temperature at 1800°C for 3 hours, and then keep the temperature at 2000°C for 4 hours; In step (c), the amounts of anhydrous ethanol, aqueous ammonia and aqueous tetrabutylammonium bromide solution used are 300 mL, 12 mL and 30 mL respectively; In step (f), the heat treatment temperature in air atmosphere is 1200°C; The rest are the same as in Example 1.

[0059] Embodiment 14 The difference between this embodiment and embodiment 1 is that in step (b), 300-mesh MoSi2 powder is used as the infiltration material; at the same time, the temperature process of the infiltration treatment is: first, keep the temperature at 1600°C for 1 hour, and then keep the temperature at 2100°C for 5 hours; In step (d), the amount of tetraethyl orthosilicate is 60 mL, and the dropping speed is 1 mL every 3 minutes; In step (f), the heat treatment temperature in air atmosphere is 1100°C; The rest are the same as in Example 1.

[0060] Embodiment 15 The difference between this embodiment and embodiment 1 is that in step (b), 300-mesh MoSi2 powder is used as the infiltration material; at the same time, the temperature process of the infiltration treatment is: first, keep the temperature at 1600°C for 1 hour, and then keep the temperature at 2200°C for 6 hours; In step (d), the amount of tetraethyl orthosilicate is 80 mL, and the dropping speed is 1 mL every 2 minutes; In step (f), the heat treatment temperature in air atmosphere is 1200°C; The rest are the same as in Example 1.

[0061] Comparative Example 1 Take a 20mm×20mm×10mm C / C composite material, polish it with 400 mesh sandpaper, blow it clean with an air gun after polishing, put it in an ultrasonic cleaner for cleaning for 1h, and then put it in an oven for drying at 150°C to obtain the treated C / C composite material.

[0062] Comparative Example 2 (a) The surface of the C / C composite material with a size of 20 mm × 20 mm × 10 mm was polished with 400-grit sandpaper, and after being polished flat, it was blown clean with an air gun, placed in an ultrasonic cleaner for 1 h, and then placed in an oven for drying at 150 °C to obtain sample A; (b) Put 200-mesh MoSi2 powder as infiltration material into a carbon-carbon crucible, bury the sample A obtained in step (a) in the infiltration material, and put it into a high-temperature furnace for infiltration treatment under Ar gas atmosphere; wherein the temperature process of the infiltration treatment is: first keep it at 1700°C for 2h, and then keep it at 2100°C for 5h; after the infiltration treatment, a treated C / C composite material is obtained, and its surface has only a layer of MoSi2 coating.

[0063] Test example The antioxidant properties of the C / C composite materials obtained after treatment in each embodiment and comparative example were tested, and the data results are shown in Table 1.

[0064] Antioxidant performance test and evaluation: 10 mg of sample was accurately weighed and heated from 27°C to 1600°C on a NETZSCH STA 449 F3 thermal analyzer in an air atmosphere, and kept at 1600°C. The heating rate was 10°C / min, and the thermogravimetric data, i.e., the curve of sample weight change with temperature, was obtained. The weight change of samples in different temperature ranges was read from the curve to judge their antioxidant performance.

[0065] Table 1

[0066] As can be seen from Table 1, the C / C composite material treated in Comparative Example 1 is thoroughly oxidized in a high-temperature air atmosphere, and the weight loss rate tends to 100%; the C / C composite material treated in Comparative Example 2 is protected by the MoSi2 coating, so the degree of oxidation is significantly reduced in a high-temperature air atmosphere, but it still shows weight loss, and the weight loss is getting more and more serious; in Examples 1-15, the MoSi2 coating is coated by the embedding method and SiO2, and the cracks and surface of the coating are sealed. The treated C / C composite materials all show oxidation weight gain in a high-temperature air atmosphere, and the weight gain after oxidation at 1600°C for 30 hours is less than 5%. In particular, the weight gain of the C / C composite material treated in Example 1 after oxidation at 1600°C for 30 hours is only 0.77%, showing excellent high-temperature oxidation resistance and high-temperature stability.

[0067] It can be seen that the present invention can form a MoSi2@SiO2 protective coating on the surface of the C / C composite material through the embedding method and the SiO2 coating method. With the coordinated cooperation of each step and its process parameters, the C / C composite material can be wrapped by a dense MoSi2@SiO2 glass layer, thereby significantly improving the antioxidant properties of the C / C composite material and enabling it to have stable high temperature resistance.

[0068] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing an anti-oxidation coating on the surface of a C / C composite material, characterized in that: The following steps are involved: First, MoSi2 is used as the infiltration material to infiltrate the C / C composite material, and then SiO2 is adsorbed onto the surface of MoSi2, and then heat treatment is performed to form an anti-oxidation coating on the surface of the C / C composite material; The temperature of the heat treatment is 1000°C-1300°C.

2. The preparation method according to claim 1, characterized in that: The particle size of the MoSi2 is 100 mesh to 300 mesh.

3. The preparation method according to claim 2, characterized in that: The temperature of the infiltration treatment is 1600°C-2200°C.

4. The preparation method according to claim 3, characterized in that: The infiltration treatment comprises the following steps: The C / C composite material is buried in MoSi2 and infiltrated under a protective atmosphere; The temperature process of the infiltration treatment includes: First keep warm at 1600℃-1800℃ for 1h-3h, then keep warm at 2000℃-2200℃ for 4h-6h.

5. The preparation method according to claim 1, characterized in that: The SiO2 is adsorbed onto the surface of MoSi2 by electrostatic adsorption; The electrostatic adsorbent used in the electrostatic adsorption includes tetrabutylammonium bromide; The environmental condition of the electrostatic adsorption is alkaline; The reagent for creating the alkaline environment includes ammonia water.

6. The preparation method according to claim 5, characterized in that: The method of adsorbing SiO2 onto the surface of MoSi2 by electrostatic adsorption comprises the following steps: The C / C composite material after infiltration treatment is immersed in a dispersion liquid, and tetraethyl orthosilicate is added and mixed, so that negatively charged SiO2 oligomers are adsorbed on the MoSi2 surface; The ratio of ethanol, ammonia water and tetrabutylammonium bromide solution in the dispersion is 100mL~300mL: 6mL~12mL: 10mL~30mL.

7. The preparation method according to claim 6, characterized in that: The size of the C / C composite material is 20 mm×20 mm×10 mm; The dosage of tetraethyl orthosilicate is 40mL-80mL; The method of adding tetraethyl orthosilicate includes dropwise addition; The speed of the dropwise addition is 1 mL every 2 to 4 minutes.

8. The preparation method according to claim 1, characterized in that: The atmosphere of the heat treatment includes air.

9. An antioxidant C / C composite material prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the antioxidant C / C composite material according to claim 9 in aerospace missiles, rocket engine nozzle throat linings and aircraft brake pairs.

Citation Information

Patent Citations

  • Preparation method of wide-temperature-range antioxidant silicon dioxide coated molybdenum disilicide powder

    CN115285997A

  • Preparation method of modified molybdenum disilicide infrared radiation powder

    CN117125716A

  • High adhesion oxidation resistant coating film for c / C composite material and its formation

    JP1996253876A

Cited By

  • Method for rapidly preparing SiO2 coating on surface of C / C composite material

    CN120818785A

  • A method for rapidly preparing a SiO2 coating on a C / C composite material surface

    CN120818785B

  • Heterogeneous high-entropy sandwich gradient coating as well as preparation method and application thereof