Preparation method and application of diamine monomer containing trifluoromethyl and cyclohexyl
By introducing trifluoromethyl and cyclohexyl diamine monomers into the polyimide backbone, the problems of low solubility and transparency of polyimide materials are solved, and the polyamide with high transparency and heat resistance are achieved The preparation of imine materials is suitable for the field of photoelectricity.
Patent Information
- Application Number
- CN202411440372.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-16
- Publication Date
- 2024-11-15
AI Technical Summary
Traditional aromatic polyimide materials are difficult to dissolve in most organic solvents due to the rigidity of the main chain structure, and the extremely high melting point and charge transfer complex formation lead to low material transparency, which limits its application in the field of photoelectricity.
By introducing trifluoromethyl and cyclohexyl diamine monomers into the polyimide backbone, a reasonable preparation method is designed to reduce the aromatic structure content, inhibit the formation of charge transfer complexes, and obtain high solubleness by using suitable processes Transparent polyimide.
It significantly improves the transparency and solubility of polyimide, achieves convenient processing and molding at room temperature, has good heat resistance and high transparency, and is suitable for optoelectronic devices and flat panel display and other fields.
Smart Images

Figure CN118955299A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials and relates to a preparation method and application of a diamine monomer containing trifluoromethyl and cyclohexyl. Background Art
[0002] As a polymer material with excellent comprehensive performance, polyimide has shown wide application potential in many cutting-edge fields such as aerospace, electrical and electronic, mechanical manufacturing, chemical industry and microelectronics due to its outstanding heat resistance, excellent mechanical properties and good resistance to chemical radiation. However, traditional aromatic polyimide is difficult to dissolve in most organic solvents due to the rigid characteristics of its main chain structure, which undoubtedly increases the complexity and cost of material processing. At the same time, its extremely high melting point poses a severe challenge to conventional molding technology, limiting the application of polyimide materials in a wider range of fields.
[0003] What is particularly critical is that charge transfer complexes are easily formed within and between polyimide molecules. This characteristic not only leads to a generally darker color of the material, making it difficult to meet the strict requirements of the optoelectronic field for material transparency, but also affects the stability of its optical properties and application prospects to a certain extent. Therefore, developing a polyimide material that can be easily processed by conventional methods and has high transparency, high heat resistance and excellent mechanical properties has become a major technical problem that needs to be overcome in the current field of materials science.
[0004] Generally, increasing thermoplasticity will lead to a decrease in glass transition temperature and thermal stability, so molecular structure design is often used to improve the solubility of polyimide. Currently, many studies have been devoted to optimizing the solubility of polyimide by introducing flexible groups and changing the molecular chain structure. At the same time, in terms of improving the transparency of materials, although strategies such as introducing large side groups, alicyclic structures, and non-coplanar structures have been tried, in the face of increasingly stringent market demands, the transparency of existing polyimide films still needs to be improved. Summary of the invention
[0005] To this end, the present invention proposes a preparation method and application of a diamine monomer containing trifluoromethyl and cyclohexyl groups, which is used to solve the above-mentioned technical problems, including: The reaction formula for the preparation of diamine monomer is as follows: .
[0006] The preparation method of the diamine monomer containing trifluoromethyl and cyclohexyl comprises the following steps: (1) Under the protection of inert gas, preheat 4.03 g of 2-trifluoromethylaniline, add 1.12 g of cyclohexylcarboxaldehyde and 0.49 g of 37% hydrochloric acid to react, and obtain a viscous reaction liquid; (2) Add 10 mL of 10% sodium hydroxide solution. The reaction system is divided into oil / water two phases. The oily crude product is obtained by liquid separation, washed three times with distilled water, first separated by column chromatography, and then purified by recrystallization with petroleum ether to obtain the diamine monomer.
[0007] Further, the reaction temperature of the 2-trifluoromethylaniline, cyclohexyl formaldehyde and acid is 60 - 160 °C, and the reaction time is 2 - 12 h.
[0008] Further, the diamine monomer containing trifluoromethyl and cyclohexyl is used as a raw material for preparing polyimide, and the structural formula is as follows: ; wherein, 10 < n < 1000, and the Ar group is selected from one of the following chemical structural units: .
[0009] Further, the preparation method of the polyimide is as follows: S1: Add a phenolic solvent, quinoline or isoquinoline, the diamine monomer and an aromatic dianhydride into a reactor, stir and react at 20 - 120 °C to obtain a viscous polyamic acid solution, continue to heat up to 130 - 150 °C and react for 2 - 12 h, and react at 180 - 220 °C for 2 - 24 h to obtain a transparent soluble polyimide solution; S2: After cooling to room temperature, slowly pour it into a precipitant to obtain white fibrous polyimide, and then obtain the polyimide resin through separation, washing and drying.
[0010] Further, the solid content of the polyamic acid solution in S1 is 5 wt% - 30 wt%.
[0011] Further, the precipitant in S2 is one or several of methanol, ethanol, propanol or acetone.
[0012] The present invention further protects that the polyimide is formulated into a solution, and then cast into a film, spun or directly applied, wherein the solid content of the polyimide solution is 0.5 wt% - 20 wt%.
[0013] The beneficial effects of the present invention are: First, a diamine monomer containing trifluoromethyl and cyclohexyl in the present invention introduces trifluoromethyl and cyclohexyl into the polyimide main chain in the form of a diamine monomer, reduces the aromatic structure content, thereby inhibiting the formation of charge transfer complexes, significantly improving the transparency of the polyimide. Moreover, due to the special structure of the designed diamine monomer, the obtained polyimide resin not only has good heat resistance, but also has good solubility, and can be dissolved in low-boiling solvents such as chloroform at room temperature. Therefore, it can be processed and formed at room temperature, and the preparation process is simple and the cost is low; Second, the present invention uses a reasonable molecular design and a suitable preparation method to prepare a type of soluble and highly transparent polyimide containing trifluoromethyl and cyclohexyl groups. The polyimide is soluble in organic solvents at room temperature and can be processed and formed at room temperature, making its processing more convenient; 3. The soluble high-transparency polyimide prepared by the present invention not only has good heat resistance, but also has high transparency, and has broad application prospects in the fields of flexible transparent substrates for optoelectronic devices, flat panel displays, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 The mass spectrum of 4,4'-(cyclohexylmethylene)bis(2-(trifluoromethyl)aniline) prepared in Examples 1 and 2; Figure 2 4,4'-(cyclohexylmethylene)bis(2-(trifluoromethyl)aniline) prepared in Examples 1 and 2 1 H-NMR spectrum; Figure 3 This is the infrared spectrum of Example 3 of the present invention; Figure 4 This is the infrared spectrum of Example 4 of the present invention; Figure 5 This is the infrared spectrum of Example 5 of the present invention. DETAILED DESCRIPTION
[0015] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0016] The synthetic route of the diamine monomer in the present invention is as follows:
[0017] 2-Trifluoromethylaniline and cyclohexylcarboxaldehyde react in the presence of an acid to obtain a diamine monomer; the synthesis process of the diamine monomer and polyimide is described below in conjunction with specific embodiments.
[0018] Example 1 Preparation of compound 4,4'-(cyclohexylmethylene)bis(2-(trifluoromethyl)aniline): Under nitrogen protection, 4.03 g of 2-trifluoromethylaniline was added to a 50 mL three-necked round-bottom flask, the temperature was raised to 80 ° C, 1.12 g of cyclohexylcarboxaldehyde and 0.49 g of 37% hydrochloric acid were added, the temperature was raised to 110 ° C and stirred for reaction for 5 hours to obtain a viscous reaction liquid; the reaction liquid was cooled to room temperature, 10 mL of 10% sodium hydroxide solution was added, the system was separated into oil / water phases, and the water phase was separated with a separatory funnel. The oil was washed three times with distilled water, first separated by column chromatography, and then purified by recrystallization with petroleum ether to obtain a light yellow solid, namely 4,4'-(cyclohexylmethylene)bis(2-(trifluoromethyl)aniline), weighing 1.59 g, with a yield of 38.3%.
[0019] Example 2 Preparation of compound 4,4'-(cyclohexylmethylene)bis(2-(trifluoromethyl)aniline): Under nitrogen protection, 4.03 g of 2-trifluoromethylaniline was added to a 50 mL three-necked round-bottom flask, the temperature was raised to 100 ° C, 1.12 g of cyclohexylcarboxaldehyde and 0.49 g of 37% hydrochloric acid were added, the temperature was raised to 120 ° C and stirred for 10 h to obtain a viscous reaction liquid; the reaction liquid was cooled to room temperature, 10 mL of 10% sodium hydroxide solution was added, the system was separated into oil / water phases, and the water phase was separated with a separatory funnel. The oil was washed three times with distilled water, first separated by column chromatography, and then purified by recrystallization with petroleum ether to obtain a light yellow solid, namely 4,4'-(cyclohexylmethylene)bis(2-(trifluoromethyl)aniline), weighing 1.76 g, with a yield of 42.3%.
[0020] Example 3 Preparation of soluble high-transparency polyimide resin labeled as PI-1: Under nitrogen protection, 416 mg of the diamine monomer was added to a 50 mL three-necked round-bottom flask, and then 5 mL of m-cresol and 294 mg of BPDA were added in sequence, and three drops of isoquinoline were added. The mixture was stirred and reacted at 100 ° C for 12 hours to obtain a viscous reaction solution. The mixture was then heated to 120 ° C, 140 ° C, and 160 ° C in sequence and stirred and reacted for 6 hours, and finally heated to 180 ° C and continued to stir and react for 15 hours. After the reaction solution was cooled to room temperature, 5 mL of chloroform was added to dilute it, and then slowly poured into 200 mL of rapidly stirred methanol to precipitate a white fibrous solid. After suction filtration, the PI-1 resin was obtained after vacuum drying at 200 ° C for 24 hours.
[0021] Example 4 Preparation of soluble high-transparency polyimide resin labeled as PI-2: Under nitrogen protection, 416 mg of the diamine monomer was added to a 50 mL three-necked round-bottom flask, and then 5 mL of m-cresol and 310 mg of OPDA were added in sequence, and three drops of isoquinoline were added. The mixture was stirred and reacted at 95° C. for 12 h to obtain a viscous reaction solution. The mixture was then heated to 120° C., 150° C., and 160° C. and stirred and reacted for 5 h, respectively, and finally heated to 220° C. and continued to stir and react for 15 h. After the reaction solution was cooled to room temperature, 5 mL of chloroform was added to dilute it, and then it was slowly poured into 300 mL of rapidly stirred methanol to precipitate a white fibrous solid. After suction filtration, the PI-2 resin was obtained after vacuum drying at 200° C. for 24 h.
[0022] Example 5 Preparation of soluble high-transparency polyimide resin labeled as PI-3: Under nitrogen protection, 416 mg of the diamine monomer was added to a 50 mL three-necked round-bottom flask, and then 5 mL of m-cresol and 444 mg of 6FDA were added in turn, and two drops of isoquinoline were dropped in. The mixture was stirred and reacted at 85° C. for 12 h to obtain a viscous reaction solution. The mixture was then heated to 120° C. and 160° C. and stirred and reacted for 5 h, respectively, and finally heated to 220° C. and continued to stir and react for 15 h. After the reaction solution was cooled to room temperature, 5 mL of chloroform was added to dilute it, and then it was slowly poured into 300 mL of rapidly stirred methanol to precipitate a white fibrous solid. After suction filtration, the PI-3 resin was obtained after vacuum drying at 200° C. for 24 h.
[0023] At room temperature, PI-1 resin, PI-2 resin and PI-3 resin were dissolved in chloroform to a solid content of 6 wt %. 2 The films were cast onto a clean glass sheet and finally dried in vacuum at 200°C for 12 h to obtain colorless and transparent PI-1 film, PI-2 film and PI-3 film.
[0024] in, Figure 3 This is the infrared spectrum of PI-1 film, where 1784cm -1 and 1732cm -1 The absorption peak is the characteristic absorption peak of the carbonyl group on the imide ring in the polyimide, indicating that the polyimide resin PI-1 was successfully prepared in Example 3; Figure 4 This is the infrared spectrum of PI-2 film, where 1786cm -1 and 1733cm -1 The absorption peak is the characteristic absorption peak of the carbonyl group on the imide ring in the polyimide, indicating that the polyimide resin PI-2 was successfully prepared in Example 4; Figure 5 This is the infrared spectrum of PI-3 film, where 1793cm -1 and 1740cm -1The absorption peak is the characteristic absorption peak of the carbonyl group on the imide ring in the polyimide, indicating that the polyimide resin PI-3 was successfully prepared in Example 5.
[0025] The performance testing method of the samples obtained in each embodiment is as follows: The molecular weight and molecular weight distribution were measured on a PE Series 200 GPC instrument equipped with a differential refractive index detector (RI). The test conditions were: DMF was used as the eluent, the column temperature was 25 o C, flow rate 1.0 mL / min, polystyrene as standard.
[0026] The glass transition temperature is marked as T g, The TA Q2000 differential scanning calorimeter (DSC) was used for the measurement. The test conditions were as follows: in a nitrogen atmosphere, the heating rate was 20 °C / min, and the temperature range was 40 o C-430 o C, The test first eliminates the thermal history of the sample.
[0027] The thermal stability was tested using a TA 550 thermogravimetric analyzer (TGA) under the following test conditions: in nitrogen or air atmosphere, with a heating rate of 20 o C / min, temperature range 50 o C-800 o C, the temperature when the weight loss is 5wt% is marked as T 5wt% as its decomposition temperature.
[0028] The number average molecular weight of PI-1 was determined to be 1.85×10 4 g / mol, molecular weight distribution is 1.97; glass transition temperature T g Greater than 371°C; decomposition temperature in nitrogen T 5wt% The average transmittance of the 25μm thick film in the visible light region is 81%.
[0029] The number average molecular weight of PI-2 was determined to be 2.63×10 4 g / mol, molecular weight distribution (M w / M n ) is 2.08; glass transition temperature T g Greater than 338°C; decomposition temperature in nitrogen T 5wt% The average transmittance of the 25μm thick film in the visible light region is 87%.
[0030] The number average molecular weight of PI-3 was determined to be 6.77×10 4 g / mol, molecular weight distribution is 1.54; glass transition temperature T g Greater than 319°C; decomposition temperature in nitrogen T5wt% The temperature is 474℃. The average transmittance of the 25μm thick film in the visible light region is 88%.
[0031] The solubility of the three soluble high-transparency polyimide resins containing trifluoromethyl and cyclohexyl groups synthesized in Examples 3-5 above is shown in Table 1. The specific test method for solubility is: weigh 10 mg of the sample, place it in 1 mL of the corresponding solvent, add a stirrer and stir at room temperature for 0.5-12 hours, and observe its solubility.
[0032] Table 1 Solubility of polyimide obtained in Examples 3-5 Solvents PI-1 PI-2 PI-3 m-cresol + + + DMAc + + + DMSO + + + DMF + + + THF + + + <![CDATA[CDCl3]]> + + + NMP + + + Note: + means completely soluble at room temperature, - means insoluble.
[0033] It can be seen from the data in Table 1 that the polyimide resins obtained in Examples 3-5 of the present invention can be dissolved in common organic solvents at room temperature, which is convenient for processing and application.
[0034] In summary, the soluble high-transparency polyimide containing trifluoromethyl and cyclohexyl provided by the present invention can maintain its high temperature resistance and also has good solubility in organic solvents, which is convenient for the polyimide to be processed and formed at room temperature; in addition, the polyimide film also has high transparency and has broad application prospects in the fields of flexible transparent substrates of optoelectronic devices, flat panel displays, etc.; and the preparation method of the soluble high-transparency polyimide containing trifluoromethyl and cyclohexyl provided by the present invention is simple to operate, has few steps, and is easy to implement.
[0035] It is worth noting that in the present invention, there is no special limitation on the aromatic dianhydride monomer used for the soluble high-transparency polyimide. Any suitable commercial aromatic dianhydride can be used to prepare the soluble high-transparency polyimide of the present invention. The aromatic dianhydride monomer can be, but is not limited to, one of 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride (OPDA) and 4,4'-(hexafluoroisopropyl) diphthalic anhydride (6FDA) mentioned in the embodiments, and is specifically selected according to the Ar group.
[0036] The raw materials used in the examples, such as catalysts and aromatic dianhydride monomers, are all commercially available products.
[0037] The above embodiments are only used to illustrate the technical method of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical method of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical method of the present invention.
Claims
1. A method for preparing a diamine monomer containing trifluoromethyl and cyclohexyl, characterized in that: The reaction formula for preparing the diamine monomer is as follows: 。 2. The method for preparing a diamine monomer containing trifluoromethyl and cyclohexyl according to claim 1, characterized in that: It includes the following steps: Under the protection of inert gas, after preheating 4.03 g of 2-trifluoromethylaniline, 1.12 g of cyclohexyl formaldehyde and 0.49 g of 37% hydrochloric acid are added for reaction to obtain a viscous reaction solution; 10 mL of 10% sodium hydroxide solution is added. The reaction system is divided into an oil / water two-phase. After liquid separation, an oily crude product is obtained, washed three times with distilled water, first separated by column chromatography, and then purified by recrystallization with petroleum ether to obtain the diamine monomer.
3. The method for preparing a diamine monomer containing trifluoromethyl and cyclohexyl according to claim 2, characterized in that: The reaction temperature of the 2-trifluoromethylaniline, cyclohexyl formaldehyde and acid is 60 - 160 °C, and the reaction time is 2 - 12 h.
4. The use of the diamine monomer containing trifluoromethyl and cyclohexyl according to claim 1, characterized in that: The diamine monomer containing trifluoromethyl and cyclohexyl is used as a raw material for preparing polyimide, and the structural formula is as follows: ; Among them, 10 < n < 1000, and the Ar group is selected from one of the following chemical structural units: 。 5. The use of the diamine monomer containing trifluoromethyl and cyclohexyl according to claim 4, characterized in that: The preparation method of the polyimide is as follows: S1: Add a phenolic solvent, quinoline or isoquinoline, the above-mentioned diamine monomer and an aromatic dianhydride into a reactor, stir and react at 20 - 120 °C to obtain a viscous polyamic acid solution, continue to heat up to 130 - 150 °C for reaction for 2 - 12 h, and react at 180 - 220 °C for 2 - 24 h to obtain a transparent soluble polyimide solution; S2: After cooling to room temperature, slowly pour it into a precipitant to obtain white fibrous polyimide, and then obtain the polyimide resin through separation, washing and drying.
6. The use of the diamine monomer containing trifluoromethyl and cyclohexyl according to claim 5, characterized in that: The solid content of the polyamic acid solution described in S1 is 5 wt% - 30 wt%.
7. The use of the diamine monomer containing trifluoromethyl and cyclohexyl according to claim 5, characterized in that: The precipitant described in S2 is one or several of methanol, ethanol, propanol or acetone.
8. Use of a diamine monomer containing trifluoromethyl and cyclohexyl groups according to any one of claims 4 to 7, characterized in that: The prepared polyimide is formulated into a solution, and then cast into a film, spun or directly applied, wherein the solid content of the polyimide solution is 0.5 wt% - 20 wt%.
Citation Information
Patent Citations
Diamine monomer containing tert-butyl and aliphatic ring, preparation and application thereof
CN108383733A
Maleate of Anti-prion compound, method for producing same, and pharmaceutical composition thereof
EP3106458A1
Diphenyl substituted alkanes
WO2008156721A1