Electrochromic compound, hybrid membrane and preparation method thereof
The electrochromic compound composed of triphenylamine 4,4,4-tricarboxylate and copper ions coordinated with the conductive substrate is combined to form an electrochromic hybrid film, which solves the problem of narrow color development range and slow response time of the electrochromic material. As for the problem of poor stability, the electrochromic effect is achieved with fast response and efficient and stable electrochromic effect, and the use of organic solvents is reduced, which is suitable for large-scale production and environmental protection requirements.
Patent Information
- Application Number
- CN202411033502.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-30
AI Technical Summary
Existing electrochromic materials have environmental safety problems caused by narrow color development range, slow response time, low coloring efficiency, and the use of oily solvents during production, and the stability of organic electrochromic materials is poor.
The electrochromic compound is formed by coordination between 4,4,4-tricarboxylate and copper ions, and an electrochromic hybrid film is formed on the conductive substrate by hydrothermal method to reduce the use of organic solvents, improve the response speed and circulation stability.
The reversible color change, faster response time, high cycle stability and high coloring efficiency of electrochromic materials are achieved, and the process is simple and low cost is suitable for large-scale production and environmentally friendly.
Smart Images

Figure CN118955314A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrochromic materials, and in particular to an electrochromic compound, a hybrid film and a preparation method thereof. Background Art
[0002] Electrochromism (EC) refers to the phenomenon that the color of a material changes reversibly under the action of an electric field. This change is caused by the electric field causing charge transfer or electron rearrangement in the material, thereby affecting the material's ability to absorb or reflect light. This color change phenomenon can be observed in the visible spectrum region (400-800nm) and the near-infrared region (1000-2000nm).
[0003] Electrochromic materials have application prospects in smart windows, displays, military camouflage and other fields due to their color variability and low energy consumption. Electrochromic materials are generally divided into two categories: inorganic electrochromic materials and organic electrochromic materials. Inorganic electrochromic materials are mainly metal oxides such as tungsten trioxide, molybdenum trioxide, iridium oxide or titanium oxide. They have the advantages of good stability, strong adhesion and high device durability, but they also have defects such as narrow color range, slow response time and low coloring efficiency, which limit their application. Organic electrochromic materials mainly include polyaniline, polythiophene, amethyst or phenothiazine compounds and their derivatives, which have the advantages of fast response speed, rich and diverse colors and easy structure modification. However, the production cost of conductive organic polymers is relatively high at this stage, and oily solvents need to be used in the production process, which has environmental safety issues, and the stability of organic electrochromic materials is relatively poor.
[0004] Therefore, doping organic materials with inorganic materials to form organic-inorganic composite electrochromic materials can give full play to the respective advantages of organic and inorganic electrochromic materials, which has important research significance and broad application value.
[0005] For example, the Chinese invention patent with application publication number CN103172274A discloses a method for preparing a nickel oxide / polyaniline composite electrochromic film, and the optical properties and response speed of the composite electrochromic material prepared by the preparation method are improved, but its stability is poor, which is not conducive to the application of the composite electrochromic material. Summary of the invention
[0006] To solve the above problems, in a first aspect, the present invention provides an electrochromic compound.
[0007] An electrochromic compound, the electrochromic compound is composed of 4,4,4-tricarboxylic acid triphenylamine coordinated with copper ions; the structural formula of the electrochromic compound is as follows:
[0008]
[0009] On the other hand, the present invention also provides an electrochromic hybrid film and a preparation method thereof, the preparation method can reduce the use of organic solvents, and the prepared hybrid film has a faster response speed and higher cycle stability.
[0010] An electrochromic hybrid film comprises the electrochromic compound mentioned above.
[0011] The method for preparing the electrochromic hybrid film comprises the following steps:
[0012] S1. providing a conductive substrate, washing the conductive substrate with an alkaline solution, distilled water and an organic solution respectively, then using a three-electrode system to electrodeposit the conductive substrate in an aqueous solution containing copper acetate and sodium acetate, and then washing with deionized water and drying to obtain a conductive substrate loaded with a cuprous oxide base film;
[0013] S2. Take a container, put 4,4,4-tricarboxylic acid triphenylamine and copper acetate, then add N,N-dimethylformamide into the container, ultrasonically treat, put the conductive substrate cuprous oxide film prepared in S1 into the container with the conductive surface facing down, tilt it, place the container in a hydrothermal reactor for reaction, cool the hydrothermal reactor after the reaction, wash and dry the film after the reaction, and obtain an electrochromic hybrid film.
[0014] When voltage is applied to the electrochromic hybrid film, N in the above compound is easily oxidized into N radical cations, thereby changing the color of the hybrid film from light green to dark blue. As the voltage continues to increase, the dark blue deepens and turns into purple.
[0015] Preferably, the conductive substrate in S1 is selected from one of indium tin oxide conductive glass, indium tin oxide conductive film, nanosilver wire conductive film, fluoride-doped tin oxide glass, and polymer conductive film.
[0016] Preferably, the alkaline solution in S1 comprises 0.5-1 wt % sodium hydroxide solution; and the organic solvent is selected from one or more of ethanol, toluene and acetone.
[0017] Preferably, the concentration of the aqueous solution of copper acetate in S1 is 0.01-0.03 mol / L; the concentration of the aqueous solution of sodium acetate is 0.07-0.13 mol / L.
[0018] Preferably, the electrodeposition time in S1 is 5 to 15 seconds.
[0019] Preferably, in S2, the concentration of 4,4,4-triphenylamine tricarboxylate in N,N-dimethylformamide is 0.005-0.015 mol / L; the concentration of copper acetate in N,N-dimethylformamide is 0.02-0.04 mol / L.
[0020] Preferably, the reaction conditions in S2 are 100-140° C. for 1-4 h.
[0021] The invention also provides applications of the electrochromic hybrid film, which can be applied in fields such as electrochromic devices.
[0022] The present invention provides 4,4,4-tricarboxylic acid triphenylamine (H 3 Preparation method of TCA):
[0023] (1) Dissolve p-aminobenzonitrile in DMSO. Then slowly add CsF to the solution under continuous stirring. When CsF is added, the solution first turns yellow and then green. After all CsF is added, some CsF remains undissolved. Then add p-fluorobenzonitrile. After reacting overnight, a brown transparent solution is obtained. After cooling, the reaction mixture is poured into ice water to precipitate the precipitated product, which is filtered, washed with water and ethanol, dried, and purified on a silica gel column to obtain pure 4,4,4-tricyanotriphenylamine (TCTPA);
[0024] (2) TCTPA and potassium hydroxide were added to a three-necked flask, and then ethylene glycol was added and heated to reflux. The turbid liquid changed from white to orange-red, and then to a brown transparent solution. The reaction was cooled to room temperature, water was added to the reaction flask, and the pH was adjusted to 1 with hydrochloric acid. The reaction mixture was filtered under reduced pressure, and the white solid was washed with water and dried to obtain H 3 TCA.
[0025] The above H 3 The reaction formula in the TCA preparation method is as follows:
[0026]
[0027] The present invention has the following beneficial effects:
[0028] (1) The electrochromic compound of the present invention makes full use of the advantages of organic and inorganic electrochromic materials. Therefore, the prepared hybrid film containing the electrochromic compound has the advantages of reversible color change, fast response time, high cycle stability and high coloring efficiency. The coloring efficiency is 243.86 cm 2 / C, contrast ratio is 70.90%, coloring time is 8.19s, and fading time is 2.33s;
[0029] (2) The present invention uses a hydrothermal method to convert 4,4,4-tricarboxylic acid triphenylamine (H 3TCA) reacts with copper ions to form coordination bonds to prepare a hybrid film containing the above electrochromic compound. 2 O substrate, under the induction and participation of the metal oxide substrate, triphenylamine triformate is reacted with copper ions in the solution by a hydrothermal method to prepare an electrochromic hybrid film; the preparation method is simple in process, low in cost, can be mass-produced, and the use of organic solvents is reduced in the preparation process, which is more environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 CuO substrate and hybrid film 2 OH 3 SEM images of TCA;
[0031] Figure 2 Cu hybrid film 2 OH 3 Cyclic voltammetry curve of TCA;
[0032] Figure 3 Cu hybrid film 2 OH 3 Response time and stability diagram of TCA at 700nm wavelength;
[0033] Figure 4 Cu hybrid film 2 OH 3 Coloring efficiency graph of TCA;
[0034] Figure 5 Cu hybrid film 2 OH 3 Flow chart of the preparation of TCA. DETAILED DESCRIPTION
[0035] The present invention is further described in detail below based on the accompanying drawings and implementation examples.
[0036] In order to make the purpose, technical scheme and advantages of the present invention more clear, the present invention is further described in detail in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention, rather than all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] Example 1
[0038] This embodiment provides an electrochromic hybrid film (Cu 2 OH 3 The preparation method of TCA hybrid membrane comprises the following steps:
[0039] (1)Cu2 Preparation of O substrate
[0040] The conductive substrate indium tin oxide (ITO) was ultrasonically cleaned with 0.5wt% NaOH solution, distilled water, ethanol, toluene and acetone solution. Then, a three-electrode system was used for deposition at room temperature, where the working electrode was ITO, the counter electrode was a platinum sheet, the silver electrode was a reference electrode, and the deposition solution was 0.02M copper acetate ((CH 3 COO 2 Cu) and 0.1 M sodium acetate (CH 3 COONa) aqueous solution, the deposition voltage is -0.3V, and it lasts for 10s to obtain a yellow cuprous oxide film. The film is then washed with deionized water three times and placed in a 50℃ oven to dry for 12 hours. The scanning electron microscope photo of the cuprous oxide film is shown in Figure 1 shown.
[0041] (2) Synthesis of 4,4,4-Triphenylamine Tricarboxylate
[0042] 10mmol of p-aminobenzonitrile was dissolved in 50mL of DMSO. Then 40mmol of CsF was slowly added to the solution under continuous stirring. When 2.00g of CsF was added, the solution turned yellow first and then green. After all the CsF was added, some CsF was still undissolved. Then 22mmol of p-fluorobenzonitrile was added. After reacting overnight, it was a brown transparent solution, and the mixture was reacted at 140℃ for 14 hours. After cooling, the reaction mixture was poured into ice water to precipitate the precipitated product, filtered, washed with water (200mL) and ethanol (100mL), dried, and purified with a silica gel column to obtain 2.10g of pure 4,4,4-tricyanotriphenylamine (TCTPA). TCTPA (1.80g, 5.62mmol) and potassium hydroxide (1.89g, 33.72mmol) were added to a 100mL three-necked flask, and then ethylene glycol (25mL) was added and heated to reflux. The turbid solution changed from white to orange-red, and then to a brown transparent solution. The reaction was completed in 14 hours. The reaction mixture was cooled to room temperature, 50 mL of water was added to the reaction flask, and the pH was adjusted to 1 with 4 M hydrochloric acid. The reaction mixture was filtered under reduced pressure, and the white solid was washed with water and dried. 2.05 g of 4,4,4-tricarboxylic acid triphenylamine (H 3 TCA).
[0043] (3) Preparation of hybrid membranes
[0044] Preparation flow chart Figure 5 As shown, 0.0377 g (0.01 M) of H 3TCA, 0.06g (0.03M) copper acetate, add 10mL N,N-dimethylformamide (DMF) to the bottle, ultrasonicate for 15 minutes, put the dry cuprous oxide film with the conductive surface facing down into the bottle, assemble the hydrothermal reactor, put it in a 120℃ oven to react for 2h, take out the hydrothermal reactor from the oven after the reaction and cool it in the air for 1h, take out the film and wash it with DMF, water and ethanol in turn, and dry it at 50℃ for 3h to get a light green Cu 2 OH 3 TCA hybrid membrane, the hybrid membrane biological scanning electron microscope photo is as follows Figure 1 shown.
[0045] Example 2
[0046] This example carried out Cu 2 OH 3 Electrochemical properties of TCA hybrid membranes.
[0047] The hybrid membrane prepared in Example 1 was placed in a three-electrode electrolytic cell with a 0.1 mol / L lithium perchlorate / propylene carbonate solution as the electrolyte solution, wherein the working electrode was a Cu 2 OH 3 The ITO glass of TCA hybrid film, the counter electrode is platinum wire, and the reference electrode is silver-silver chloride electrode. Cyclic voltammetry was used for scanning, the scanning voltage range was 0-1.8V, and the scanning speed was 100mV / s. The results are as follows Figure 2 As shown, Figure 2 The left side is Cu 2 OH 3 Electrochemical properties test diagram of TCA hybrid membrane. From the figure, we can see that Cu 2 OH 3 The TCA hybrid film has a pair of obvious redox peaks, and with the increase of voltage, the color of the film can be observed to change from light green to dark blue. 2 OH 3 The TCA hybrid membrane can achieve a purple color change at 1.61V.
[0048] Example 3
[0049] This example carried out Cu 2 OH 3 Testing of response speed and stability of TCA hybrid membrane.
[0050] The hybrid membrane prepared in Example 1 was placed in a three-electrode electrolytic cell with a 0.1 mol / L lithium perchlorate / propylene carbonate solution as the electrolyte solution, wherein the working electrode was a Cu 2 OH 3The ITO glass of the TCA hybrid film, the counter electrode is platinum wire, and the reference electrode is silver-silver chloride electrode. The electrochemical workstation and UV spectrometer are combined. The electrochemical workstation is set to the multi-potential step method: the initial potential is 0V, the end potential is 1.8V, the potential pulse width is 15s, and the scanning time is 6000s; the UV spectrum is set to spectral dynamics, and the wavelength is set to 700nm. The final data is as follows Figure 3 As shown, it can be seen that Cu 2 OH 3 The coloring time of the TCA hybrid film is 8.19s, the fading time is 2.33s, and the film still maintains a contrast ratio of 96.28% after 200 cycles. According to the results, it can be seen that the hybrid film provided by the present invention has good stability under multiple cycles.
[0051] Example 4
[0052] This example carried out Cu 2 OH 3 Coloring efficiency test of TCA hybrid film. Coloring efficiency refers to the change in optical density caused by the consumption of unit charge per unit area.
[0053] The hybrid film prepared in Example 1 was placed in a three-electrode electrolytic cell with 0.1 mol / L lithium perchlorate / propylene carbonate solution as the electrolyte solution, wherein the working electrode was a Cu 2 OH 3 The ITO glass of TCA hybrid film, the counter electrode is platinum wire, the reference electrode is silver-silver chloride electrode, and the electrochemical workstation adopts multi-potential step method to test such as Figure 4 As shown, Cu 2 OH 3 TCA hybrid membrane test results. Figure 4 It can be seen that Cu 2 OH 3 The TCA hybrid membrane has a higher coloring efficiency of 243.86 cm 2 / C.
Claims
1. An electrochromic compound, characterized in that: The electrochromic compound is composed of 4,4,4-tricarboxylic acid triphenylamine coordinated with copper ions; the structural formula of the electrochromic compound is as follows: 。 2. An electrochromic hybrid film, characterized in that: The hybrid film comprises the electrochromic compound according to claim 1.
3. The method for preparing the electrochromic hybrid film according to claim 2, characterized in that: The following steps are involved: S1. providing a conductive substrate, washing the conductive substrate with an alkaline solution, distilled water and an organic solution respectively, then using a three-electrode system to electrodeposit the conductive substrate in an aqueous solution containing copper acetate and sodium acetate, and then washing with deionized water and drying to obtain a conductive substrate loaded with a cuprous oxide base film; S2. Take a container, put 4,4,4-tricarboxylic acid triphenylamine and copper acetate, then add N,N-dimethylformamide into the container, ultrasonically treat, put the conductive substrate cuprous oxide film prepared in S1 into the container with the conductive surface facing down, tilt it, place the container in a hydrothermal reactor for reaction, cool the hydrothermal reactor after the reaction, wash and dry the film after the reaction, and obtain an electrochromic hybrid film.
4. The preparation method according to claim 3, characterized in that: The conductive substrate in S1 is selected from one of indium tin oxide conductive glass, indium tin oxide conductive film, nano silver wire conductive film, fluoride-doped tin oxide glass, and polymer conductive film.
5. The preparation method according to claim 3, characterized in that: The alkaline solution in S1 includes 0.5-1 wt % sodium hydroxide solution; the organic solvent is selected from one or more of ethanol, toluene and acetone.
6. The preparation method according to claim 3, characterized in that: The concentration of the aqueous solution of copper acetate in S1 is 0.01-0.03 mol / L; the concentration of the aqueous solution of sodium acetate is 0.07-0.13 mol / L.
7. The preparation method according to claim 3, characterized in that: The electrodeposition time in S1 is 5 to 15 seconds.
8. The preparation method according to claim 3, characterized in that: In S2, the concentration of 4,4,4-triphenylamine tricarboxylate in N,N-dimethylformamide is 0.005-0.015 mol / L; the concentration of copper acetate in N,N-dimethylformamide is 0.02-0.04 mol / L.
9. The preparation method according to claim 3, characterized in that: The reaction conditions in S2 are 100-140° C. for 1-4 hours.
10. Application of the electrochromic hybrid film according to claim 2 in the field of electrochromic devices and the like.
Citation Information
Patent Citations
Preparation method of nickel oxide / polyaniline composite electrochromic film
CN103172274A
Preparation method of bimetal center metal organic framework electrochromic film
CN114105486A
Green synthesis process of 4, 4 ', 4' '-triphenylamine triformate
CN114751838A
Perylene bisimide derivative hybrid material, film and preparation method of perylene bisimide derivative hybrid material
CN115340681A
Triphenylamine-based polyion liquid cross-linked porous electrochromic film and preparation method thereof
CN117683268A
Cited By
Preparation method and application of triphenylamine copper coordination polymer film
CN121065785A
Preparation method and application of a triphenylamine-based copper coordination polymer film
CN121065785B