Self-assembly molecular material, preparation method and application thereof, solar cell and preparation method thereof

By using acridinetone-based self-assembly molecular materials in perovskite solar cells, the problems of insufficient interface passivation and poor hole transmission performance are solved, and higher carrier transmission efficiency and thermal stability are achieved, which improves the Overall performance of the device.

CN118955561APending Publication Date: 2024-11-15TRINA SOLAR CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410292779.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-03-14
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the prior art, self-assembled molecular materials have insufficient passivation of semiconductor devices and poor hole transmission performance, resulting in low device efficiency and stability.

Method used

Provide a self-assembled molecular material with acridone as the parent nucleus and phosphonic acid as the anchor group. By combining with a transparent conductive oxide substrate, it regulates interface charge and improves carrier transport efficiency, and is used in perovskites. Used in solar cells to enhance thermal stability and hole extraction capabilities.

Benefits of technology

It effectively improves the carrier transmission efficiency and thermal stability of perovskite solar cells, and enhances the long-term stability and efficiency of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955561A_ABST
    Figure CN118955561A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of semiconductors, in particular to a self-assembly molecular material, a preparation method and application thereof, a solar cell and a preparation method thereof. The problems of insufficient interface passivation, poor device stability and the like of a semiconductor device in the prior art are solved. The invention relates to a self-assembled molecular material. The structural general formula of the self-assembled molecular material is as shown in the following formula (I): # imgabs0 # (I), wherein L is selected from C2-C18 alkyl groups, and X is selected from any one of hydrogen, halogen, substituted or unsubstituted C1-C3 alkyl groups, substituted or unsubstituted C6-C20 aryl groups, cyano groups, amino groups, methoxyl groups and methylthio groups; in a substituted or unsubstituted C1-C3 alkyl group and a substituted or unsubstituted C6-C20 aryl group, a substituent group during substitution is selected from any one of a C1-C10 alkyl group, a C2-C10 hetero-alkyl group and a halogen.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of semiconductor technology, and in particular to a self-assembling molecular material and a preparation method and application thereof, a solar cell and a preparation method thereof. Background Art

[0002] In the field of semiconductor devices, the interface performance in semiconductor devices will have a significant impact on the efficiency, performance and stability of semiconductor devices.

[0003] For example, taking perovskite photovoltaic devices as an example, in order to further improve the efficiency and device stability of perovskite photovoltaic devices, it is usually necessary to passivate the interface defects in perovskite photovoltaic devices. For example, the self-assembled molecular materials currently used on transparent conductive oxide substrates and inorganic oxide hole transport layers can passivate the transparent conductive oxide substrates and inorganic oxide hole transport layers using anchoring groups such as phosphonic acid, thereby reducing substrate defects and further reducing the perovskite degradation problem caused by substrate defects.

[0004] However, the self-assembled molecular materials provided in the current related technologies have problems such as insufficient interface passivation for semiconductor devices and poor hole transport performance, which is not conducive to improving the performance and stability of semiconductor devices. Summary of the invention

[0005] Based on this, it is necessary to provide a self-assembling molecular material and a preparation method and application thereof, a solar cell and a preparation method thereof, so as to solve the problems of insufficient interface passivation and poor device stability of semiconductor devices in related technologies.

[0006] In a first aspect, a self-assembling molecular material is provided, wherein the general structural formula of the self-assembling molecular material is shown in the following formula (I):

[0007] (I)

[0008] Wherein, L is selected from C2~C 18 Alkylene, X is selected from hydrogen, halogen, substituted or unsubstituted C1~C3 alkyl, substituted or unsubstituted C6~C 20 Any of aryl, cyano, amino, methoxy and methylthio; in substituted or unsubstituted C1~C3 alkyl and substituted or unsubstituted C6~C 20 In the case of aryl, the substituent is selected from C1~C 10 Alkyl, C2~C 10 Any of heteroalkyl and halogen.

[0009] Optionally, L is selected from C4~C6 alkylene, X is selected from chlorine, bromine, iodine, methoxy, methylthio and substituted or unsubstituted C6~C 20Any of the aromatic groups.

[0010] Optionally, the self-assembling molecular material comprises one or more combinations of the following structural formulas:

[0011] , , , , , , , and .

[0012] In a second aspect, a method for preparing a self-assembling molecular material is provided, comprising:

[0013] Providing or preparing structures represented by formula (i) and formula (ii);

[0014] Reacting formula (i) and formula (ii) to prepare a structure represented by formula (iii);

[0015] reacting the compound of formula (iii) with trialkyl phosphonate to prepare the self-assembling molecular material;

[0016] Wherein, the structural formula of formula (i) is expressed as: ; The structural formula of formula (ii) is expressed as: , the structural formula of formula (iii) is expressed as: ;

[0017] Wherein, L is selected from C2~C 18 Alkylene, X is selected from hydrogen, halogen, substituted or unsubstituted C1~C3 alkyl, substituted or unsubstituted C6~C 20 any one of aryl, cyano, amino, methoxy and methylthio; in a substituted or unsubstituted C1~C3 alkyl, a substituted or unsubstituted C6~C 20 In the case of aryl, the substituent is selected from C1~C 10 Alkyl, C2~C 10 Any of heteroalkyl and halogen; Y is selected from bromine or iodine.

[0018] In a third aspect, there is provided a use of the self-assembling molecular material as described in the first aspect in the preparation of a semiconductor device.

[0019] In a fourth aspect, a solar cell is provided, comprising:

[0020] Basal layer;

[0021] A first electrode is disposed on the base layer;

[0022] An organic interface modification layer is disposed on a side of the first electrode away from the substrate layer;

[0023] a perovskite layer, disposed on a side of the organic interface modification layer away from the first electrode; and

[0024] A second electrode is disposed on a side of the perovskite layer away from the first electrode;

[0025] Wherein, the material of the organic interface modification layer includes: one or more of the self-assembling molecular materials according to any one of claims 1 to 3.

[0026] Optionally, an electron transport layer is further included, and the electron transport layer is arranged between the perovskite layer and the second electrode.

[0027] Optionally, the material of the electron transport layer includes one or more of [6,6]-phenyl-C61-butyric acid methyl ester, C60 and tin oxide.

[0028] In a fifth aspect, a method for preparing a solar cell is provided, comprising:

[0029] providing a base layer, wherein a first electrode is formed on the base layer;

[0030] Sequentially stacking an organic interface modification layer, a perovskite layer, and a second electrode on the first electrode;

[0031] Wherein, the material of the organic interface modification layer includes: one or more of the self-assembly molecular materials described in the first aspect.

[0032] Optionally, forming an organic interface modification layer on the first electrode comprises:

[0033] Dissolving the material of the organic interface modification layer in an organic solvent to prepare a solution of the material of the organic interface modification layer;

[0034] Laying a solution of the material of the organic interface modification layer on the first electrode to form a liquid film;

[0035] The liquid film is annealed to prepare the organic interface modification layer.

[0036] Optionally, the organic solvent is selected from one or more of tetrahydrofuran, methanol, ethanol, isopropanol, 1,4-dioxane, toluene and xylene.

[0037] Optionally, in the solution of the material for the organic interface modification layer, the concentration of the material for the organic interface modification layer is 0.1 mg / mL to 10.0 mg / mL.

[0038] Compared with the related art, the beneficial technical effects of this application are as follows:

[0039] The self-assembled molecular material uses acridone as the parent core and a phosphonic acid group as the anchoring group, so that the self-assembled molecular material has a larger molecular dipole moment. When it is applied to perovskite solar cells, it has a stronger ability to regulate the work function of the TCO substrate, thereby effectively extracting interfacial charges and improving carrier transfer efficiency; on the other hand, compared with molecules containing intra-ring heteroatoms such as phenothiazine and phenoxazine, the self-assembled molecules provided in the embodiments of the present application have better thermal stability, which is beneficial to the long-term stable operation of the semiconductor device to which it is applied; on the other hand, the embodiments of the present application have good hole extraction and transmission capabilities, which can effectively improve device efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 A schematic diagram of the structure of a solar cell provided in an embodiment of the present application. DETAILED DESCRIPTION

[0041] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application, so the present application is not limited by the specific embodiments disclosed below.

[0042] Unless the context requires otherwise, throughout the specification and claims, the term "including" is to be interpreted as an open, inclusive meaning, that is, "including, but not limited to". In the description of the specification, the terms "one embodiment", "some embodiments", "exemplary embodiments", "exemplarily" or "some examples" and the like are intended to indicate that specific features, structures, materials or characteristics associated with the embodiment or example are included in at least one embodiment or example of the present disclosure. The schematic representation of the above terms does not necessarily refer to the same embodiment or example. In addition, the specific features, structures, materials or characteristics may be included in any one or more embodiments or examples in any appropriate manner.

[0043] Exemplary embodiments are described herein with reference to cross-sectional views and / or plan views that are idealized exemplary drawings. In the drawings, the thickness of layers and regions are exaggerated for clarity. Therefore, variations in shape relative to the drawings due to, for example, manufacturing techniques and / or tolerances are conceivable. Therefore, the exemplary embodiments should not be interpreted as being limited to the shapes of the regions shown herein, but include shape deviations due to, for example, manufacturing. For example, an etched region shown as a rectangle will typically have curved features. Therefore, the regions shown in the drawings are schematic in nature, and their shapes are not intended to illustrate the actual shape of regions of the device, and are not intended to limit the scope of the exemplary embodiments.

[0044] Herein, unless otherwise specified, "one or more" means one or more than or equal to two.

[0045] In this document, "for example", "such as", "example", "for example", etc. are used for descriptive purposes, indicating that the previous and subsequent different technical solutions are related in terms of the content covered, but should not be understood as limiting the previous technical solution, nor can they be understood as limiting the scope of protection of this document. In this document, unless otherwise specified, A (such as B) means that B is a non-limiting example of A, and it can be understood that A is not limited to B.

[0046] In this article, "optionally", "optional", and "optional" mean optional, that is, any one of the two parallel options of "yes" or "no". If there are multiple "options" in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "option" is independent.

[0047] In this document, the terms "first", "second", etc. in "the first aspect", "the second aspect", etc. are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features.

[0048] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0049] In this article, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0050] Herein, when it comes to a numerical interval (i.e., a numerical range), unless otherwise specified, the distribution of the optional numerical values ​​within the numerical interval is considered to be continuous and includes the two numerical endpoints (i.e., the minimum and maximum values) of the numerical interval, and each numerical value between the two numerical endpoints. Unless otherwise specified, when a numerical interval only refers to integers within the numerical interval, including the two endpoint integers of the numerical range, and each integer between the two endpoints, is equivalent to directly listing each integer. When multiple numerical ranges are provided to describe features or characteristics, these numerical ranges can be combined. In other words, unless otherwise specified, the numerical ranges disclosed herein should be understood to include any and all sub-ranges included therein. The "numerical value" in the numerical interval can be any quantitative value, such as a number, a percentage, a ratio, etc. "Numerical interval" allows broadly including numerical interval types such as percentage intervals, ratio intervals, and ratio intervals.

[0051] In this article, the percentage content, unless otherwise specified, refers to mass percentage for solid-liquid mixing and solid-solid mixing, and volume percentage for liquid-liquid mixing.

[0052] In this article, when it comes to percentage concentration, unless otherwise specified, it refers to the final concentration. The final concentration refers to the proportion of the added component in the system after the addition of the component.

[0053] In this article, when it comes to temperature parameters, unless otherwise specified, both constant temperature treatment and treatment within a certain temperature range are allowed. The constant temperature treatment allows the temperature to fluctuate within the accuracy range of instrument control.

[0054] Herein, the term "room temperature" or "normal temperature" generally refers to 4°C to 35°C, for example, 20°C ± 5°C. In some embodiments herein, "room temperature" or "normal temperature" refers to 10°C to 30°C. In some embodiments herein, "room temperature" or "normal temperature" refers to 20°C to 30°C.

[0055] As used in this article, fill factor (FF) refers to the ratio of the actual maximum achievable power (Pm or Vmp * Jmp) to the theoretical (not actually achievable) power (Jsc * Voc). Therefore, FF can be determined by the following formula:

[0056] FF = (Vmp * Jmp) / (Jsc * Voc)

[0057] Where Jmp and Vmp represent the current density and voltage at the maximum power point (Pm), which is obtained by changing the resistance in the circuit until J * V is the maximum value; Jsc and Voc represent the short-circuit current and open-circuit voltage, respectively. Fill factor is a key parameter for evaluating solar cells. Commercial solar cells usually have a fill factor of about 60% or more.

[0058] As used herein, open circuit voltage (Voc) is the potential difference between the anode and cathode of the device with no external load connected.

[0059] The power conversion efficiency (PCE) of a solar cell used in this article refers to the percentage of power converted from absorbed light to electrical energy. The power conversion efficiency (PCE) of a solar cell can be measured by the incident light irradiance (E: W / m 2 ) and the surface area of ​​the solar cell (Ac:m 2 ) divided by the maximum power point (Pm). STC usually refers to the temperature of 25℃ and the irradiance of 1000 W / m 2 , the spectrum of air quality 1.5 (AM1.5).

[0060] the term

[0061] Unless otherwise specified or incompatible herewith, the terms and phrases used herein shall have the following meanings:

[0062] The term "alkyl" refers to a saturated hydrocarbon containing primary (normal) carbon atoms, or secondary carbon atoms, or tertiary carbon atoms, or quaternary carbon atoms, or a combination thereof. A phrase containing the term, for example, "C1-C9 alkyl" refers to an alkyl containing 1 to 9 carbon atoms, and each occurrence may be independently C1 alkyl, C2 alkyl, C3 alkyl, C4 alkyl, C5 alkyl, C6 alkyl, C7 alkyl, C8 alkyl or C9 alkyl. Suitable examples include, but are not limited to, methyl (Me, -CH3), ethyl (Et, -CH2CH3), 1-propyl (n-Pr, n-propyl, -CH2CH2CH3), 2-propyl (i-Pr, i-propyl, -CH(CH3)2), 1-butyl (n-Bu, n-butyl, -CH2CH2CH2CH3), 2-methyl-1-propyl (i-Bu, i-butyl, -CH2CH(CH3)2), 2-butyl (s-Bu, s-butyl, -CH(C H3)CH2CH3), 2-methyl-2-propyl (t-Bu, t-butyl, -C(CH3)3), 1-pentyl (n-pentyl, -CH2CH2CH2CH2CH3), 2-pentyl (-CH(CH3)CH2CH2CH3), 3-pentyl (-CH(CH2CH3)2), 2-methyl-2-butyl (-C(CH3)2CH2CH3), 3-methyl-2-butyl (-CH(CH3)CH(CH3)2), 3-methyl-1-butyl (- CH2CH2CH(CH3)2), 2-methyl-1-butyl (-CH2CH(CH3)CH2CH3), 1-hexyl (-CH2CH2CH2CH2CH2CH3), 2-hexyl (-CH(CH3)CH2CH2CH2CH3), 3-hexyl (-CH(CH2CH3)(CH2CH2CH3)), 2-methyl-2-pentyl (-C(CH3)2CH2CH2CH3), 3-methyl-2-pentyl (-CH(CH3)CH( 2), 2-methyl-3-pentyl (-CH(CH2CH3)CH(CH3)2), 2,3-dimethyl-2-butyl (-C(CH3)2CH(CH3)2), 3,3-dimethyl-2-butyl (-CH(CH3)C(CH3)3 and octyl (-(CH2)7CH3).

[0063] "Aryl" refers to an aromatic hydrocarbon group derived from an aromatic ring compound by removing a hydrogen atom. It can be a monocyclic aromatic group, a condensed aromatic group, or a polycyclic aromatic group. For polycyclic rings, at least one is an aromatic ring system. For example, "C5~C 20 "Aryl" refers to an aromatic group containing 5 to 20 carbon atoms, and each occurrence can be independently C5 aromatic group, C6 aromatic group, C 10 Aryl, C 14 Aryl, C 18 Aryl or C 20 Aryl. Suitable examples include, but are not limited to, benzene, biphenyl, naphthalene, anthracene, phenanthrene, perylene, triphenylene and derivatives thereof. It is understood that multiple aryl groups may also be interrupted by short non-aromatic units (e.g., <10% non-H atoms, such as C, N or O atoms), specifically acenaphthene, fluorene, or 9,9-diarylfluorene, triarylamine, diaryl ether systems should also be included in the definition of aryl.

[0064] "Heteroalkyl" means that at least one carbon atom is replaced by a non-carbon atom on the basis of an alkyl group, and the non-carbon atom can be an N atom, an O atom, an S atom, etc. For example, if the carbon atom connected to the parent core structure in the alkyl group is replaced by a non-carbon atom, the resulting heteroalkyl group is an alkoxy group (e.g., -OCH3, etc.), an amine (e.g., -NHCH3, -N(CH3)2, etc.) or a thioalkyl group (e.g., -SCH3). If the carbon atom not connected to the parent core structure in the alkyl group is replaced by a non-carbon atom, the resulting heteroalkyl group is an alkyl ether (e.g., -CH2CH2-O-CH3, etc.), an alkylamine (e.g., -CH2NHCH3, -CH2N(CH3)2, etc.) or a thioalkyl ether (e.g., -CH2-S-CH3). If the terminal carbon atom of the alkyl group is replaced by a non-carbon atom, the resulting heteroalkyl group is a hydroxyalkyl group (e.g., -CH2CH2-OH), an aminoalkyl group (e.g., -CH2NH2) or an alkylthiol group (e.g., -CH2CH2-SH). Phrases containing this term, for example, "C1~C9 heteroalkyl" refers to heteroalkyl groups containing 1 to 9 carbon atoms, and each occurrence can be independently C2 heteroalkyl, C3 heteroalkyl, C4 heteroalkyl, C5 heteroalkyl, C7 heteroalkyl, C8 heteroalkyl or C9 heteroalkyl.

[0065] "Amino" refers to a derivative of ammonia having the structural features of the formula -N(X)2, wherein each "X" is independently H, substituted or unsubstituted alkyl, substituted or unsubstituted cycloalkyl, substituted or unsubstituted heterocyclyl, etc. Non-limiting types of amino groups include -NH2, -N(alkyl), -NH(alkyl), -N(cycloalkyl), -NH(cycloalkyl), -N(heterocyclyl), -NH(heterocyclyl), -N(aryl), -NH(aryl), -N(alkyl)(aryl), -N(alkyl)(heterocyclyl), -N(cycloalkyl)(heterocyclyl), -N(aryl)(heteroaryl), -N(alkyl)(heteroaryl), etc.

[0066] "Halogen" or "halo" refers to F, Cl, Br or I.

[0067] "Alkylene" refers to a hydrocarbon group with two monovalent radical centers derived from an alkyl group by removing a hydrogen atom, which can be a saturated branched alkyl group or a saturated straight-chain alkyl group. For example, "C1-C9 alkylene" means that the alkyl portion contains 1 to 9 carbon atoms, and each occurrence can be independently C1 alkylene, C4 alkylene, C5 alkylene, C6 alkylene, C7 alkylene, C8 alkylene or C9 alkylene. Suitable examples include, but are not limited to, methylene (-CH2-), 1,1-ethyl (-CH(CH3)-), 1,2-ethyl (-CH2CH2-), 1,1-propyl (-CH(CH2CH3)-), 1,2-propyl (-CH2CH(CH3)-), 1,3-propyl (-CH2CH2CH2-) and 1,4-butyl (-CH2CH2CH2CH2-).

[0068] Based on the above technical problems, in the first aspect, some embodiments of the present application provide a self-assembling molecular material, the general structural formula of the self-assembling molecular material is shown in the following formula (I):

[0069] (I)

[0070] Wherein, L is selected from C2~C 18 Alkylene, X is selected from hydrogen, halogen, substituted or unsubstituted C1~C3 alkyl, substituted or unsubstituted C6~C 20 Any of aryl, cyano, amino, methoxy and methylthio; substituted or unsubstituted C1~C3 alkyl and substituted or unsubstituted C6~C 20 In the case of aryl, the substituent is selected from C1~C 10 Alkyl, C2~C 10 Any of heteroalkyl and halogen.

[0071] In the self-assembling molecular material provided in the embodiment of the present application, the self-assembling molecular material uses acridone as the parent core and a phosphonic acid group as the anchoring group, so that the self-assembling molecular material has a larger molecular dipole moment. When it is applied to perovskite solar cells, the ability to regulate the work function of the TCO substrate is stronger, thereby effectively extracting interfacial charges and improving carrier transfer efficiency; on the other hand, compared with molecules containing intracyclic heteroatoms such as phenothiazine and phenoxazine, the self-assembling molecules provided in the embodiment of the present application have better thermal stability, which is beneficial to the long-term stable operation of the semiconductor device to which it is applied; on the other hand, the embodiment of the present application has good hole extraction and transmission capabilities, which can effectively improve device efficiency.

[0072] In some embodiments, L is selected from C4-C6 alkylene, X is selected from chlorine, bromine, iodine, methoxy, methylthio and substituted or unsubstituted C6-C 20 Any of the aromatic groups.

[0073] In these embodiments, the self-assembled molecular material has a simple structure and is easy to prepare.

[0074] In some embodiments, the self-assembling molecular material comprises one or more combinations of the following structural formulas:

[0075] , , , , , , , and .

[0076] In these embodiments, these self-assembled monomolecular materials have good hole transport properties, thereby improving the efficiency of semiconductor devices.

[0077] In a second aspect, some embodiments of the present application provide a method for preparing a self-assembling molecular material, comprising:

[0078] Providing or preparing structures represented by formula (i) and formula (ii);

[0079] Reacting formula (i) and formula (ii) to prepare a structure represented by formula (iii);

[0080] reacting the compound of formula (iii) with trialkyl phosphonate to prepare the self-assembling molecular material;

[0081] Wherein, the structural formula of formula (i) is expressed as: ; The structural formula of formula (ii) is expressed as: , the structural formula of formula (iii) is expressed as: ;

[0082] Wherein, L is selected from C2~C 18 Alkylene, X is selected from hydrogen, halogen, substituted or unsubstituted C1~C3 alkyl, substituted or unsubstituted C6~C 20 any one of aryl, cyano, amino, methoxy and methylthio; in a substituted or unsubstituted C1~C3 alkyl, a substituted or unsubstituted C6~C 20 In the case of aryl, the substituent is selected from C1~C 10 Alkyl, C2~C 10 Any of heteroalkyl and halogen; Y is selected from bromine or iodine.

[0083] In these embodiments, the preparation method is simple and the raw materials are readily available.

[0084] In some embodiments, the reaction of formula (i) and formula (ii) can be carried out under alkaline conditions. The alkaline conditions can be obtained by adding potassium hydroxide or sodium hydroxide to the reaction system.

[0085] In some embodiments, the temperature for reacting the compound (iii) with trialkyl phosphonate may be 120° C. to 180° C., and the time may be 12 h to 24 h. After the reaction is completed, the self-assembling molecular material may be prepared by hydrolysis.

[0086] In a third aspect, some embodiments of the present application provide a use of the self-assembling molecular material as described in the first aspect in the preparation of a semiconductor device.

[0087] The semiconductor device may be illustratively any one of a dye-sensitized solar cell, an organic photovoltaic cell, a perovskite solar cell, an organic light-emitting semiconductor, and an organic transistor.

[0088] Optionally, the semiconductor device is a solar cell.

[0089] In a fourth aspect, some embodiments of the present application provide a solar cell, such as Figure 1 As shown, the solar cell includes: a substrate layer 10, a first electrode 11, an organic interface modification layer 12, a perovskite layer 13 and a second electrode 14; wherein the first electrode 11 is arranged on the substrate layer 10, the organic interface modification layer 12 is arranged on the side of the first electrode 11 away from the substrate layer 10, the perovskite layer 13 is arranged on the side of the organic interface passivation layer 12 away from the first electrode 11, and the second electrode 14 is arranged on the side of the perovskite layer 13 away from the first electrode 11. The material of the organic interface modification layer 12 includes: one or more of the self-assembly molecular materials described in the first aspect.

[0090] The material of the first electrode 11 may include: TCO (Transparent Conductive Oxides) material. In this case, the organic interface modification layer 14 may be combined with the TCO material via a phosphonic acid anchoring group.

[0091] In the solar cell provided in the embodiment of the present application, by using the above-mentioned self-assembled molecular material as the organic interface modification layer, on the one hand, the self-assembled molecular material is combined with the first electrode through the phosphonic acid anchoring group, and the molecular dipole moment can be used to reduce the electrode work function, thereby enhancing the extraction and transmission efficiency of hole carriers at the interface; on the other hand, the carbonyl group in the self-assembled molecular material can act as a Lewis base to coordinate with the lead ions in the perovskite layer, thereby passivating the perovskite layer. Compared with the molecules containing intra-ring heteroatoms such as phenothiazine and phenoxazine used in the related art, it has stronger defect passivation ability and good thermal stability.

[0092] In some embodiments, the solar cell further includes an electron transport layer 15 , which is disposed between the perovskite layer 13 and the second electrode 14 .

[0093] In these embodiments, the electron transport performance of the solar cell can be effectively improved, thereby further improving the efficiency of the solar cell.

[0094] In some embodiments, the material of the electron transport layer 15 may include one or more of [6,6]-phenyl-C61-butyric acid methyl ester, C60, and tin oxide.

[0095] In some embodiments, the material of the second electrode may include one or more of silver, copper, TCO and a carbon electrode.

[0096] In a fourth aspect, some embodiments of the present application provide a method for preparing a solar cell, comprising:

[0097] providing a base layer, on which a first electrode is formed;

[0098] An organic interface modification layer, a perovskite layer, and a second electrode are sequentially stacked on the first electrode;

[0099] Wherein, the material of the organic interface modification layer includes: one or more of the self-assembly molecular materials described in the first aspect.

[0100] In the method for preparing a solar cell provided in an embodiment of the present application, an organic interface modification layer is formed on the surface of the first electrode away from the substrate layer, and the material of the organic interface modification layer includes the above-mentioned self-assembled molecular material. Therefore, the above-mentioned solar cell with higher efficiency can be prepared.

[0101] In some embodiments, forming an organic interface modification layer on the first electrode includes:

[0102] Dissolving the material of the organic interface modification layer in an organic solvent to prepare a solution of the material of the organic interface modification layer;

[0103] Laying a solution of a material of an organic interface modification layer on the first electrode to form a liquid film;

[0104] The liquid film is annealed to prepare an organic interface modification layer.

[0105] In these embodiments, the organic interface modification layer is prepared by a solution method, which can achieve low-cost preparation and effectively control the anchoring of the self-assembled molecular materials in the organic interface modification layer on the TCO substrate.

[0106] In some embodiments, the organic solvent is selected from one or more of tetrahydrofuran, methanol, ethanol, isopropanol, 1,4-dioxane, toluene, and xylene.

[0107] In some embodiments, in the solution of the material for the organic interface modification layer, the concentration of the material for the organic interface modification layer is 0.1 mg / mL to 10.0 mg / mL.

[0108] In a fifth aspect, some embodiments of the present application provide a photovoltaic assembly, the photovoltaic assembly comprising: a plurality of solar cells connected in series and / or in parallel;

[0109] At least one of the solar cells is a solar cell as described in the fourth aspect.

[0110] Since the photovoltaic module includes the solar cell provided by the above embodiment, it has the same beneficial effects as the solar cell described in the fourth aspect, which will not be described in detail here.

[0111] In a sixth aspect, some embodiments of the present application provide a photovoltaic system, comprising the photovoltaic component as described in the fifth aspect.

[0112] Since the photovoltaic system includes the photovoltaic assembly provided by the above embodiment, it has the same beneficial effects as the photovoltaic assembly described in the fifth aspect, which will not be described in detail here.

[0113] Photovoltaic systems can be used in photovoltaic power stations, such as ground power stations, rooftop power stations, water power stations, etc., and can also be used in equipment or devices that use solar energy to generate electricity, such as user solar power supplies, solar street lights, solar cars, solar buildings, etc. Of course, it is understandable that the application scenarios of photovoltaic systems are not limited to this, that is to say, photovoltaic systems can be used in all fields that require solar energy to generate electricity. Taking the photovoltaic power generation system network as an example, the photovoltaic system may include a photovoltaic array, a junction box and an inverter. The photovoltaic array can be an array combination of multiple solar cells. For example, multiple solar cells can form multiple photovoltaic arrays. The photovoltaic array is connected to the junction box. The junction box can converge the current generated by the photovoltaic array. The converged current flows through the inverter and is converted into the alternating current required by the mains power grid. After that, it is connected to the mains network to realize solar power supply.

[0114] In order to objectively evaluate the technical effects of the embodiments of the present application, the present application will be described in detail and exemplarily through the following embodiments and comparative examples.

[0115] In the following examples and comparative examples, all raw materials can be purchased commercially, and in order to maintain the reliability of the experiment, the raw materials used in the following examples and comparative examples have the same physical and chemical parameters or are prepared by the same processing method.

[0116] Example 1

[0117] The preparation method of the self-assembling molecular material provided in Example 1 is as follows:

[0118]

[0119] Step 1), under nitrogen protection, add acridone a (1.00 g, 5.1mmol), tetrabutylammonium bromide (160 mg, 0.5 mmol) and 1,4-dibromobutane (27 g, 125 mmol) to a 100 mL round-bottom flask in sequence, then drop 50% KOH solution (3.02 g, 53.8 mmol) into it, react at 65°C for 12h, and the solution is a white-green suspension. After the reaction, 1,4-dibromobutane is removed by oil pump rotary evaporation, and then extracted by a mixed system of DCM (dichloromethane) and H2O, dried over anhydrous sodium sulfate and then dried by rotary drying. Separate by column chromatography, the eluent is a mixed solvent of PE (petroleum ether) and DCM, and segmented elution is adopted. The volume ratio of PE (petroleum ether) and DCM in the first segment is 4:1, and the volume ratio of PE (petroleum ether) and DCM in the second segment is 1:4. A white solid b (648 mg, 2.0 mmol) was obtained with a yield of 41.0%.

[0120] Step 2) Under nitrogen protection, add b (2.07 g, 6.5 mmol) and triethyl phosphite (5.82 g, 204 mmol) to a 100 mL round-bottom flask in sequence. After heating, the solid is completely dissolved and reacted at 160°C for 15 hours. After the reaction, the unreacted triethyl phosphite is removed by oil pump rotary evaporation. Column chromatography separation is performed in two stages. The first stage eluent is a mixed solvent of PE and DCM in a volume ratio of 1:1, and the second stage eluent is A mixed solvent of PE and EA (ethyl acetate) with a volume ratio of 1:1 was used to obtain a yellow-white solid c (1.73 g, 4.6 mmol) with a yield of 70.7%.

[0121] Step 3), under nitrogen protection, add c (1.69 g, 4.4 mmol), trimethylsilyl bromide (5.34 g, 34.9 mmol) and dichloromethane (15 mL) to a 100 mL round-bottom flask in sequence and react for 24 hours. After the reaction, add MeOH (30 mL) and H2O (5 mL) and react for 7 hours. The solution is a yellow suspension. Filter the reaction solution, wash with a large amount of water and then with about 30 mL of methanol. A yellow solid product (1.24 g, 3.9 mmol), i.e., self-assembled molecular material P1, is obtained with a yield of 88.6%.

[0122] The final NMR data of the self-assembled molecular material P1 is: 1 H NMR (400 MHz, DMSO-d6) δ: 8.34(d, J = 7.9 Hz, 2H), 7.91-7.77 (m, 4H), 7.33 (t, J = 7.2 Hz, 2H), 4.48 (t, J= 8.0 Hz, 2H), 1.89 (t, J = 7.8 Hz, 2H), 1.81-1.57 (m, 4H).

[0123] Example 2

[0124] The preparation method of the self-assembling molecular material P2 provided in Example 2 is as follows:

[0125]

[0126] The initial raw material was changed from acridone 1a to 2,7-dibromoacridone 2a. The synthesis steps were the same as those of the self-assembled molecular material P1. The final product P2 was a dark yellow solid. The NMR data were as follows: 1H NMR (400 MHz, DMSO-d6) δ 7.96 (d, J = 2.0Hz, 2H), 7.62 (dd, J = 8.8, 2.3 Hz, 2H), 7.20 (d, J = 8.8 Hz, 2H), 4.45 (t, J= 8.0 Hz, 2H), 1.86 (t, J = 7.8 Hz, 2H), 1.82-1.59 (m, 4H).

[0127] Example 3

[0128] The preparation method of the self-assembling molecular material P3 provided in Example 3 is as follows:

[0129]

[0130] Step 01), 2,7-dibromofluorenone 3a (1.76 g, 5.0 mmol) and cuprous iodide (1.90 g, 10.0 mmol) were dissolved in N,N-dimethylformamide, 5 mL of 30% sodium methoxide methanol solution was added dropwise, and then the reaction system was heated to 100°C and stirred for 24 hours. After the reaction was completed, the inorganic salt was filtered off, the organic phase was concentrated and purified by column chromatography, and the eluent was petroleum ether and dichloromethane in a volume ratio of 1:1 to obtain intermediate 3b as a yellow solid.

[0131] Step 1), step 2) and step 3) are the same as in Example 1, and finally the self-assembled molecular material P3 is obtained as a yellow solid, and the NMR data is: 1 H NMR (400 MHz, DMSO-d6) δ 7.54 (d, J = 2.3 Hz, 2H), 7.24 (d, J =8.5 Hz, 2H), 7.01 (dd, J = 8.8, 2.3 Hz, 2H), 4.46 (t, J = 5.3 Hz, 2H), 3.95 (s, 6H), 1.90 (t, J = 7.6 Hz, 2H), 1.80-1.56 (m, 4H).

[0132] Example 4

[0133] The preparation method of the self-assembling molecular material P4 provided in Example 4 is as follows:

[0134]

[0135] Step 1), dissolve intermediate 2b (1.46 g, 3.0 mmol) with diphenylamine (1.18 g, 7.0 mmol), sodium tert-butoxide (0.86 g, 9.0 mmol), tri(dibenzylideneacetone)dipalladium (137 mg, 0.15 mmol), tri-tert-butylphosphine tetrafluoroboric acid (174 mg, 0.6 mmol) in anhydrous toluene, heat to 110°C under inert gas atmosphere, stir and reflux for 12 hours. After the reaction is completed, filter to remove inorganic salts, concentrate the organic phase by rotary evaporation and purify by column chromatography, the eluent is petroleum ether and dichloromethane in a volume ratio of 3:1 to 1:1, and obtain intermediate 4b.

[0136] Step 2) and step 3) are the same as in Example 1, and the self-assembled molecular material P4 is finally obtained as a yellow solid, and the NMR data is: 1 H NMR (400 MHz, DMSO-d6) δ 7.69 (d, J = 2.4 Hz, 2H), 7.34-7.25 (m, 10H), 7.21 (dd, J = 8.2, 2.3 Hz, 2H), 7.12 (dd, J = 6.8, 1.5 Hz, 8H), 7.08-7.00 (m,4H), 4.45 (t, J = 5.3 Hz, 2H), 1.91 (t, J = 7.8 Hz, 2H), 1.80-1.57 (m, 4H).

[0137] Example 5

[0138] The preparation method of the perovskite solar cell provided in Example 5 is as follows:

[0139] (1) The TCO conductive glass was ultrasonically cleaned with deionized water, acetone and isopropanol for 15 min respectively, and finally dried in a drying oven at 75°C for later use; the dried TCO glass substrate was placed in a UV ozone machine for 5 min to remove organic impurities on its surface and improve its surface wettability;

[0140] (2) Dissolve 0.5 mg of the self-assembled molecular materials provided in Examples 1 to 4 in 1 mL of tetrahydrofuran, stir at room temperature until completely dissolved, to obtain an organic interface modification material solution, deposit the organic interface modification material solution on the TCO conductive glass by coating or scraping, and then heat and anneal at 100° C. on a hot stage for 10 min to form an organic interface modification layer;

[0141] (3) Dissolve 53.5 g of lead iodide, 7.1 g of lead bromide, 2.2 g of methylamine hydrobromide, and 19.0 g of formamidine hydroiodide in 100 mL of a mixed reagent of DMF and NMP (the volume ratio of DMF to NMP is 90:10), and stir at room temperature for 2 h to obtain a 1.3 mol / L perovskite precursor solution;

[0142] (4) spin coating the perovskite precursor solution prepared in step (3), and then placing the TCO conductive glass spin-coated with the perovskite precursor solution on a hot stage for heating and annealing at 100° C. for 40 min to form a perovskite layer;

[0143] (5) Dissolve 20 mg of methanefullerene phenyl-C61-butyric acid methyl ester (PCBM) in 1 mL of chlorobenzene and stir at room temperature to obtain a [6,6]-phenyl-C61-butyric acid methyl ester solution. Take the electron transport layer solution and deposit it on the perovskite layer by spin coating to form an electron transport layer;

[0144] (6) Dissolve 1 mg of 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline (BCP) in 2 mL of isopropanol and stir at room temperature to obtain a hole blocking layer solution, which is then scraped and coated on the perovskite layer to form a hole blocking layer;

[0145] (7) Silver electrode was prepared by vacuum evaporation with a thickness of 100 nm.

[0146] Comparative Example 1

[0147] The preparation method of the perovskite solar cell provided in Comparative Example 1 is substantially the same as the preparation method of the perovskite solar cell provided in Example 5, except that:

[0148] In step (2), [4-(9H-carbazole-9-yl)butyl]phosphonic acid (4PACz) is used as an organic interface modification material.

[0149] Test Case

[0150] The solar cells provided in Example 5 and Comparative Example 1 were subjected to performance tests, and the specific test results are shown in Table 1 below:

[0151] Table 1

[0152]

[0153] As can be seen from Table 1, acridone has a better defect passivation effect than 4PACz, so that the solar cell provided by Example 5 has a higher short-circuit current and fill factor than that of Comparative Example 1, thereby improving the photoelectric conversion efficiency of the solar cell.

[0154] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0155] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims.

Claims

1. A self-assembling molecular material, characterized in that: The general structural formula of the self-assembling molecular material is shown in the following formula (I): (I) Wherein, L is selected from C2~C 18 Alkylene, X is selected from hydrogen, halogen, substituted or unsubstituted C1~C3 alkyl, substituted or unsubstituted C6~C 20 Any of aryl, cyano, amino, methoxy and methylthio; in substituted or unsubstituted C1~C3 alkyl and substituted or unsubstituted C6~C 20 In the case of aryl, the substituent is selected from C1~C 10 Alkyl, C2~C 10 Any of heteroalkyl and halogen.

2. The self-assembled molecular material according to claim 1, characterized in that: The L is selected from C4~C6 alkylene, and X is selected from chlorine, bromine, iodine, methoxy, methylthio and substituted or unsubstituted C6~C 20 Any of the aromatic groups.

3. The self-assembled molecular material according to claim 2, characterized in that: The self-assembling molecular material includes one or more combinations of the following structural formulas: , , , , , , , and .

4. A method for preparing a self-assembling molecular material, characterized in that: include: Providing or preparing structures represented by formula (i) and formula (ii); Reacting formula (i) and formula (ii) to prepare a structure represented by formula (iii); reacting the compound of formula (iii) with trialkyl phosphonate to prepare the self-assembling molecular material; Wherein, the structural formula of formula (i) is expressed as: ; The structural formula of formula (ii) is expressed as: , the structural formula of formula (iii) is expressed as: ; Wherein, L is selected from C2~C 18 Alkylene, X is selected from hydrogen, halogen, substituted or unsubstituted C1~C3 alkyl, substituted or unsubstituted C6~C 20 any one of aryl, cyano, amino, methoxy and methylthio; in a substituted or unsubstituted C1~C3 alkyl, a substituted or unsubstituted C6~C 20 In the case of aryl, the substituent is selected from C1~C 10 Alkyl, C2~C 10 Any of heteroalkyl and halogen; Y is selected from bromine or iodine.

5. Use of the self-assembling molecular material according to any one of claims 1 to 3 in the preparation of semiconductor devices.

6. A solar cell, characterized in that: include: basal layer; A first electrode is disposed on the base layer; An organic interface modification layer is disposed on a side of the first electrode away from the substrate layer; A perovskite layer, disposed on a side of the organic interface modification layer away from the first electrode; as well as A second electrode is disposed on a side of the perovskite layer away from the first electrode; Wherein, the material of the organic interface modification layer includes: one or more of the self-assembling molecular materials according to any one of claims 1 to 3.

7. The solar cell according to claim 6, characterized in that: The method further includes an electron transport layer, wherein the electron transport layer is disposed between the perovskite layer and the second electrode.

8. The solar cell according to claim 7, characterized in that: The material of the electron transport layer includes one or more of [6,6]-phenyl-C61-butyric acid methyl ester, C60 and tin oxide.

9. A method for preparing a solar cell, characterized in that: include: providing a base layer, wherein a first electrode is formed on the base layer; Sequentially stacking an organic interface modification layer, a perovskite layer, and a second electrode on the first electrode; Wherein, the material of the organic interface modification layer includes: one or more of the self-assembling molecular materials according to any one of claims 1 to 3.

10. The preparation method according to claim 9, characterized in that: Forming an organic interface modification layer on the first electrode, comprising: Dissolving the material of the organic interface modification layer in an organic solvent to prepare a solution of the material of the organic interface modification layer; Laying a solution of the material of the organic interface modification layer on the first electrode to form a liquid film; The liquid film is annealed to prepare the organic interface modification layer.

11. The preparation method according to claim 10, characterized in that: The organic solvent is selected from one or more of tetrahydrofuran, methanol, ethanol, isopropanol, 1,4-dioxane, toluene and xylene.

12. The preparation method according to claim 10, characterized in that: In the solution of the material for the organic interface modification layer, the concentration of the material for the organic interface modification layer is 0.1 mg / mL to 10.0 mg / mL.

Citation Information

Cited By

  • Self-assembly material based on acridone, perovskite solar cell and preparation method

    CN119823182A