Hydrogel with high-sensitivity detection performance as well as preparation method and application thereof

By using natural polymer chitosan, methacrylic acid, acrylamide and zinc salts, the problem of insufficient electromechanical response performance of ionic conductive hydrogels is solved, and high sensitivity detection performance and large-scale production are achieved. Feasibility, suitable for flexible wearable electronic devices.

CN118955805APending Publication Date: 2024-11-15SUZHOU YIPU SCIENTIFIC INSTRUMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411067697.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing ionic conductive hydrogels have insufficient electromechanical and electrical response performance in wearable electronic devices, which affects their application, and complex preparation processes are not conducive to large-scale production.

Method used

Using natural polymer chitosan, methacrylic acid, acrylamide and zinc salt as the main raw materials, hydrogels with porous network structures are prepared by free radical polymerization, and the electrostatic interaction between amino and carboxyl groups is used to restrict the movement of water molecules, thereby improving the Mechanical properties and ionic conductivity of hydrogels.

Benefits of technology

It achieves excellent mechanical properties and ionic conductivity of the hydrogel, breaks through the limitation of water decomposition voltage, and the maximum withstand voltage reaches 2.4V, significantly improves the electromechanical response characteristics and detection sensitivity, and is suitable for flexible wearable electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955805A_ABST
    Figure CN118955805A_ABST
Patent Text Reader

Abstract

The invention discloses hydrogel with high-sensitivity detection performance as well as a preparation method and application thereof, and belongs to the technical field of ionic conductive hydrogel. Comprising the following steps: step 1, preparing a chitosan solution, a functional monomer mixed solution and a zinc salt solution; step 2, slowly dropwise adding the functional monomer mixed solution into the chitosan solution, and stirring after dropwise adding to obtain a first mixed solution; step 3, slowly dropwise adding a zinc salt solution into the first mixed solution, and stirring after dropwise adding to obtain a second mixed solution; 4, slowly dropwise adding an initiator into the second mixed solution to obtain a third mixed solution; and 5, heating and stirring the third mixed solution, and cooling to room temperature to obtain the hydrogel. The natural polymer hydrogel with a porous network structure is jointly constructed by taking natural polymer chitosan as a skeleton structure and taking methacrylic acid and acrylamide as functional monomers, so that the hydrogel has excellent mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ionic conductive hydrogels, and specifically relates to a hydrogel with high-sensitivity detection performance and a preparation method and application thereof. Background Art

[0002] Ionic conductive hydrogels have excellent mechanical properties and electrical conductivity due to their unique three-dimensional network structure and rich water content. Ionic conductive hydrogels are widely used in flexible wearable electronic devices such as flexible supercapacitors, sensors, soft robots, and bionic electronic skin.

[0003] Although ionic conductive hydrogels have effectively promoted the rapid development of wearable electronic devices, existing ionic conductive hydrogels generally have the problem of insufficient electromechanical response performance, which seriously affects the application of ionic conductive hydrogels in wearable electronic devices.

[0004] Although a lot of research work has been done in the past to try to improve the electromechanical response performance of ionic conductive hydrogels by improving mechanical properties, conductivity or special structural design, no significant effect has been achieved. On the contrary, the increased complexity of the preparation process is not conducive to large-scale production. Summary of the invention

[0005] Purpose of the invention: In order to solve the above problems, the present invention provides a hydrogel with high sensitive detection performance and a preparation method and application thereof.

[0006] Technical solution: A method for preparing a hydrogel with high sensitive detection performance, comprising the following steps:

[0007] Step 1: prepare chitosan solution, functional monomer mixed solution, and zinc salt solution respectively.

[0008] The preparation of chitosan solution in step 1 comprises the following steps:

[0009] Add a certain amount of acid into deionized water, stir at 800-900 rpm at 35-40°C, and continue stirring for 0.8-1.0 h;

[0010] Then chitosan was added, the temperature was maintained constant, the stirring speed was increased to 1500-1600 rpm, stirring was continued for 1.0-3.0 h until the chitosan was completely dissolved in the deionized water, and the mixture was naturally cooled to room temperature to obtain a chitosan solution;

[0011] The mass ratio of chitosan, deionized water, and acid is (1.0-5.0):100:(1.0-10.0).

[0012] Preferably, the acid is glacial acetic acid or dilute hydrochloric acid.

[0013] Preferably, the molecular weight of the chitosan is 50-500 mPa·s.

[0014] The step 1 of preparing the functional monomer mixed solution comprises the following steps:

[0015] Dissolve a certain amount of methacrylic acid and acrylamide in deionized water at a dissolving temperature of 25°C, stir at a speed of 300 to 400 rpm, and continue stirring for 0.5 to 1 hour to obtain a functional monomer mixed solution;

[0016] The mass ratio of methacrylic acid, acrylamide and deionized water is (1.0-4.0): (1.0-4.0): 2.0.

[0017] The preparation of the zinc salt solution in step 1 comprises the following steps:

[0018] Mix a certain amount of zinc salt with deionized water, and stir at a stirring speed of 400 to 500 rpm, a stirring temperature of 25° C., and a stirring time of 0.5 to 1 h to obtain a zinc salt solution;

[0019] Wherein, the mass ratio of zinc salt to deionized water is (0.1-0.6):1.0.

[0020] Preferably, the zinc salt is one of zinc sulfate heptahydrate, zinc sulfate monohydrate or ammonium zinc sulfate.

[0021] Step 2: slowly drop the functional monomer mixed solution into the chitosan solution, and stir after the dropwise addition to obtain a first mixed solution; wherein the mass ratio of the chitosan solution to the functional monomer mixed solution is 4.0:(1.0-6.0).

[0022] The dropping time in step 2 is 2.0 to 2.5 hours; the stirring conditions are: stirring speed 1000 to 1200 rpm, stirring temperature 25° C., and stirring time 6.0 to 8.0 hours.

[0023] Step 3: slowly dropwise add the zinc salt solution to the first mixed solution, and stir after the dropwise addition to obtain a second mixed solution; wherein the mass ratio of the first mixed solution to the zinc salt solution is 5:(0.1-0.5).

[0024] The dropping time in step 3 is 0.5 to 1 h; the stirring conditions are: stirring speed 1000 to 1200 rpm, stirring for 3 to 4.0 h.

[0025] Step 4: slowly drop an initiator into the second mixed solution to obtain a third mixed solution after the dropwise addition is complete; wherein the mass ratio of the second mixed solution to the initiator is 100:(1.0-3.0).

[0026] The dropping time in step 4 is 0.5 to 1 hour; the stirring conditions are: stirring speed 1000 to 1200 rpm, stirring 0.5 to 1 hour.

[0027] Preferably, the initiator is one of potassium persulfate, ammonium persulfate or cerium persulfate.

[0028] Step 5: After heating and stirring the third mixed solution, cooling it to room temperature to obtain a hydrogel.

[0029] The heating and stirring conditions in step 5 are: heating temperature is 45-55° C., and stirring time is 6.0-8.0 h.

[0030] In another technical solution, a hydrogel with high-sensitivity detection performance is provided, which is prepared by the above-mentioned method for preparing a hydrogel with high-sensitivity detection performance.

[0031] Another technical solution provides an application of the above-mentioned hydrogel with high sensitive detection performance in flexible wearable electronic devices.

[0032] The key invention of the method for preparing the natural polymer conductive hydrogel with high sensitive detection performance provided by the present invention is that natural polymer chitosan, methacrylic acid, acrylamide and zinc salt are used as main raw materials, initiator, acid and deionized water are used as auxiliary raw materials, free radical polymerization is carried out at 25-55°C in seven steps, and finally cooled to obtain the target hydrogel. The preparation method of the present invention is simple and easy to operate, can be completed by one pot method, the water system is pollution-free and residue-free, the synthesis method used is environmentally friendly, and is convenient for large-scale production and preparation.

[0033] Beneficial effects:

[0034] (1) The hydrogel prepared by the present invention uses natural polymer chitosan as the skeleton structure, and uses methacrylic acid and acrylamide as functional monomers to jointly construct a natural polymer hydrogel with a porous network structure, so that the hydrogel has excellent mechanical properties;

[0035] (2) The polymer network structure of the hydrogel prepared by the present invention simultaneously contains amino and carboxyl functional groups with opposite electrical properties. The amino and carboxyl groups can form a "cage" of water molecules in the hydrogel network structure through electrostatic interaction, effectively restraining the movement of water molecules in the gel, thereby increasing the dissociation energy of water molecules, thereby increasing the withstand voltage value of water molecules in the hydrogel, achieving a hydrogel working voltage range that exceeds the limit of 1.23V of water decomposition voltage, a maximum withstand voltage value of 2.4V, and a stable working voltage range of 0 to 2.4V;

[0036] (3) The raw materials of the hydrogel prepared by the present invention are natural polymer chitosan, methacrylic acid, acrylamide and zinc salt. The raw materials used have the advantages of low toxicity, easy biodegradation and high safety. The mechanical properties of the hydrogel can be effectively regulated by adjusting the ratio of methacrylic acid and acrylamide to meet different application requirements. Zinc salt is used as an electrolyte. The zinc salt exists in the form of ions in the hydrogel system and can migrate freely in the porous network of the hydrogel, giving the hydrogel excellent ionic conductivity.

[0037] (4) Based on the excellent mechanical properties and ionic conductivity of the hydrogel prepared by the present invention, it is used as a stress-strain sensor to show excellent electromechanical response characteristics. The intensity, frequency, speed, number, cycle and process of the external force can be fed back in the form of electrical signals, thereby realizing real-time detection of the external force. Based on this electromechanical response characteristic of the hydrogel, it can be used for the detection of human joint and limb health, bionic machine control, electronic skin and other flexible wearable electronic devices;

[0038] (5) Based on the wide voltage tolerance range of the hydrogel prepared by the present invention, the stress and strain detection sensitivity of the hydrogel can be significantly improved by increasing the working voltage value during the stress detection process; using it as a stress and strain sensor, it can be found through comparison that under high working voltage detection conditions, the stress and strain detection sensitivity of the hydrogel is significantly higher than that under low working voltage detection conditions, and the detection minimum stress value is also significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 is the infrared spectra of the hydrogels obtained in Examples 1 to 3;

[0040] Figure 2 The mechanical properties of the hydrogels obtained in Examples 1 to 3;

[0041] Figure 3 The conductive properties of the hydrogels obtained in Examples 1 to 3;

[0042] Figure 4 The withstand voltage performance test of the hydrogels obtained in Examples 1 to 3;

[0043] Figure 5 The electromechanical response performance of the hydrogel obtained in Example 3 to the same deformation under different voltages;

[0044] Figure 6 This is the minimum detected stress value of the hydrogel obtained in Example 3. DETAILED DESCRIPTION

[0045] Example 1

[0046] Step 1: Add 10.0 g of dilute hydrochloric acid to 100 g of deionized water, stir at 800 rpm at 35 ° C, and continue stirring for 1.0 hour, then add 5.0 g of chitosan (50 mPa·s), maintain the temperature unchanged, increase the stirring speed to 1500 rpm, and continue stirring for 3.0 hours until the chitosan is completely dissolved in the deionized water, and naturally cool to 25 ° C to obtain a chitosan solution.

[0047] Step 2: Dissolve 1.0 g of methacrylic acid and 1.0 g of acrylamide in 2.0 g of deionized water at a dissolving temperature of 25° C., a stirring speed of 300 rpm, and a stirring time of 0.5 h to obtain a functional monomer mixed solution.

[0048] Step 3: Dissolve 0.6 g of zinc sulfate heptahydrate in 1.0 g of deionized water at a stirring speed of 500 rpm, a stirring temperature of 25° C., and a stirring time of 0.5 h until the zinc sulfate heptahydrate is completely dissolved to obtain a zinc sulfate aqueous solution.

[0049] Step 4: Weigh 4.0 g of the chitosan solution prepared in step 1, and then slowly add 6.0 g of the functional monomer mixed solution prepared in step 2. The addition is completed in 2.0 h, with a stirring speed of 1000 rpm, a stirring temperature of 25° C., and a stirring time of 8.0 h.

[0050] Step 5: Slowly add 1.0 g of aqueous zinc sulfate solution to the mixed solution obtained in step 4 within 0.5 h, maintain stirring speed at 1000 rpm, and stir for 4.0 h.

[0051] Step 6: Slowly add 0.33 g of cerium persulfate to the mixed solution obtained in step 5 within 0.5 h, maintain the stirring speed at 1000 rpm, and stir for 0.5 h.

[0052] Step 7: Heat the solution obtained in step 6 to 55°C, continue stirring, and react for 8.0 hours, then cool to room temperature to obtain a light yellow transparent hydrogel.

[0053] Example 2

[0054] Step 1: Add 10.0 g of glacial acetic acid to 100 g of deionized water, stir at 800 rpm at 35 ° C, and continue stirring for 3.0 hours. Then, add 5.0 g of chitosan (500 mPa·s), maintain the temperature unchanged, increase the stirring speed to 1500 rpm, and continue stirring for 3.0 hours until the chitosan is completely dissolved in the deionized water, and cool naturally to 25 ° C to obtain a chitosan solution.

[0055] Step 2: Dissolve 4.0 g of methacrylic acid and 4.0 g of acrylamide in 2.0 g of deionized water at a dissolving temperature of 25° C., a stirring speed of 300 rpm, and a stirring time of 0.5 h to obtain a functional monomer mixed solution.

[0056] Step 3: Dissolve 0.1 g of zinc sulfate monohydrate in 1.0 g of deionized water at a stirring speed of 500 rpm, a stirring temperature of 25° C., and a stirring time of 0.5 h until the zinc sulfate monohydrate is completely dissolved to obtain a zinc sulfate aqueous solution.

[0057] Step 4: Weigh 4.0 g of the chitosan solution prepared in step 1, and then slowly add 1.0 g of the functional monomer mixed solution prepared in step 2. The addition is completed in 2.0 hours, with a stirring speed of 1000 rpm, a stirring temperature of 25° C., and a stirring time of 6.0 hours.

[0058] Step 5: Slowly add 0.5 g of aqueous zinc sulfate solution to the mixed solution obtained in step 4 within 0.5 h, maintain stirring speed at 1000 rpm, and stir for 4.0 h.

[0059] Step 6: Slowly add 0.165 g of potassium persulfate to the mixed solution obtained in step 5 within 0.5 h, maintain the stirring speed at 1000 rpm, and stir for 0.5 h.

[0060] Step 7: Heat the solution obtained in step 6 to 45°C, continue stirring, react for 6.0 hours, and then cool to room temperature to obtain a light yellow transparent hydrogel.

[0061] Example 3

[0062] Step 1: Add 1.0 g of glacial acetic acid to 100 g of deionized water, stir at 800 rpm at 35 ° C, and continue stirring for 1.0 hour, then add 0.1 g of chitosan (200 mPa·s), maintain the temperature unchanged, increase the stirring speed to 1500 rpm, and continue stirring for 1.0 hour until the chitosan is completely dissolved in the deionized water, and naturally cool to 25 ° C to obtain a chitosan solution.

[0063] Step 2: Dissolve 2.0 g of methacrylic acid and 1.0 g of acrylamide in 2.0 g of deionized water at a dissolving temperature of 25° C., a stirring speed of 300 rpm, and a stirring time of 0.5 h to obtain a functional monomer mixed solution.

[0064] Step 3: Dissolve 0.3 g of ammonium zinc sulfate in 1.0 g of deionized water at a stirring speed of 500 rpm, a stirring temperature of 25° C., and a stirring time of 0.5 h until the ammonium zinc sulfate is completely dissolved to obtain an ammonium zinc sulfate aqueous solution.

[0065] Step 4: Weigh 4.0 g of the chitosan solution prepared in step 1, and then slowly add 4.0 g of the functional monomer mixed solution prepared in step 2. The addition is completed in 2.0 hours, with a stirring speed of 1000 rpm, a stirring temperature of 25° C., and a stirring time of 6.0 hours.

[0066] Step 5: Slowly add 0.16 g of ammonium zinc sulfate aqueous solution to the mixed solution obtained in step 4 within 0.5 h, maintain the stirring speed at 1000 rpm, and stir for 4.0 h.

[0067] Step 6: Slowly add 0.0816 g of ammonium persulfate to the mixed solution obtained in step 5 within 0.5 h, maintain the stirring speed at 1000 rpm, and stir for 0.5 h.

[0068] Step 7: Heat the solution obtained in step 6 to 45°C, continue stirring, react for 6.0 hours, and then cool to room temperature to obtain a light yellow transparent hydrogel.

[0069] Example 4

[0070] The mechanical properties of the hydrogels obtained in Examples 1 to 3 were measured:

[0071] The hydrogels prepared by the methods of Examples 1 to 3 were set as cylindrical samples (with a diameter of 1.0 cm and a height of 2.5 cm). The mechanical properties of the hydrogels prepared in Examples 1 to 3 were measured using a universal mechanical testing machine. The compression rate was 2.0 mm / min and the compression deformation was 50%.

[0072] The hydrogels prepared in Examples 1 to 3 all exhibit excellent mechanical properties: the maximum pressure value of the hydrogel prepared in Example 1 is 0.08 MPa when the compression deformation is 50%; the maximum pressure value of the hydrogel prepared in Example 2 is 0.35 MPa when the compression deformation is 50%; the maximum pressure value of the hydrogel prepared in Example 3 is 0.12 MPa when the compression deformation is 50%.

[0073] Example 5

[0074] The ionic conductivity of the hydrogels obtained in Examples 1 to 3 was measured:

[0075] The hydrogel obtained in Examples 1 to 3 was set into sample strips (length x width x height: 1.0 cm x 0.5 cm x 0.1 cm), used as electrolyte, and graphite sheets were used as test electrodes. The ionic conductivity of the hydrogel was tested using an electrochemical workstation.

[0076] The hydrogels prepared in Examples 1-3 all exhibited excellent ionic conductivity: the conductivity of the hydrogel prepared in Example 1 was 63.73 mS / cm; the conductivity of the hydrogel prepared in Example 2 was 26.23 mS / cm; and the conductivity of the hydrogel prepared in Example 3 was 43.16 mS / cm.

[0077] Example 6

[0078] The withstand voltage range of the hydrogels obtained in Examples 1 to 3 was measured.

[0079] The hydrogels obtained in Examples 1 to 3 were set as sample strips (length x width x height: 1.0 cm x 0.5 cm x 0.1 cm), which were used as electrolytes, commercial carbon electrodes as positive electrodes, and zinc foil as negative electrodes to assemble into sandwich-type supercapacitors. The hydrogel withstand voltage range was tested using an electrochemical workstation.

[0080] The hydrogel prepared in Example 1 exhibits a wide range of tolerable working voltages, with a maximum tolerable voltage value of 2.0 V and a working voltage range of 0 to 2.0 V. The hydrogel prepared in Example 2 has a maximum tolerable voltage value of 1.8 V and a working voltage range of 0 to 1.8 V. The hydrogel prepared in Example 3 has a maximum tolerable voltage value of 2.4 V and a working voltage range of 0 to 2.4 V.

[0081] Example 7

[0082] The electromechanical response performance of the hydrogel obtained in Example 3 was measured.

[0083] The hydrogel obtained in Example 3 was set as a sample strip (length x width x height: 1.0 cm x 0.5 cm x 0.1 cm), which was used as a stress-strain sensor, and was connected to an electrochemical workstation and a universal mechanical testing machine to test the electromechanical response performance of the hydrogel.

[0084] The hydrogel prepared in Example 3 exhibits excellent electromechanical response characteristics and can provide synchronous feedback in the form of electrical signals. More importantly, when the test working voltage is increased from 0.1V to 2.4V, for the same deformation amount, the relative resistance value change rate of the hydrogel is significantly improved, that is, the detection sensitivity of the hydrogel is improved, and the minimum detection stress value reaches 10Pa.

[0085] Comparative Example 1

[0086] Step 1: Add 10.0 g of dilute hydrochloric acid to 100 g of deionized water, stir at 800 rpm at 35 ° C, and continue stirring for 1.0 hour, then add 5.0 g of chitosan (50 mPa·s), maintain the temperature unchanged, increase the stirring speed to 1500 rpm, and continue stirring for 3.0 hours until the chitosan is completely dissolved in the deionized water, and naturally cool to 25 ° C to obtain a chitosan solution.

[0087] Step 2: Dissolve 1.0 g of methacrylic acid and 1.0 g of acrylamide in 2.0 g of deionized water at a dissolving temperature of 25° C., a stirring speed of 300 rpm, and a stirring time of 0.5 h to obtain a functional monomer mixed solution.

[0088] Step 3: Dissolve 0.6 g of zinc chloride in 1.0 g of deionized water at a stirring speed of 500 rpm, a stirring temperature of 25° C., and a stirring time of 0.5 h until the zinc chloride is completely dissolved to obtain a zinc chloride aqueous solution.

[0089] Step 4: Weigh 4.0 g of the chitosan solution prepared in step S1, and then slowly add 6.0 g of the functional monomer mixed solution prepared in step S2. The addition is completed in 2.0 h, with a stirring speed of 1000 rpm, a stirring temperature of 25° C., and a stirring time of 8.0 h.

[0090] Step 5: Slowly add 1.0 g of aqueous zinc chloride solution to the mixed solution obtained in step 4 within 0.5 h, maintain stirring speed at 1000 rpm, and stir for 4.0 h.

[0091] Step 6: Slowly add 0.33 g of cerium persulfate to the mixed solution obtained in step 5 within 0.5 h, maintain the stirring speed at 1000 rpm, and stir for 0.5 h.

[0092] Step 7: Heat the solution obtained in step 6 to 55°C, continue stirring, and react for 8.0 hours, then cool to room temperature to obtain a light yellow transparent hydrogel.

[0093] However, the prepared hydrogel has a withstand voltage range of only 0.2 to 1.8 V, and cannot reach 0 to 2.0 V. This is because when comparing zinc chloride and zinc sulfate, under the same metal ion conditions, the anion will directly affect the electrochemical properties of the electrolyte.

[0094] Comparative Example 2

[0095] Step 1: Add 10.0 g of dilute hydrochloric acid to 100 g of deionized water, stir at 800 rpm at 35 ° C, and continue stirring for 1.0 hour, then add 5.0 g of chitosan (50 mPa·s), maintain the temperature unchanged, increase the stirring speed to 1500 rpm, and continue stirring for 3.0 hours until the chitosan is completely dissolved in the deionized water, and naturally cool to 25 ° C to obtain a chitosan solution.

[0096] Step 2: Dissolve 1.0 g of acrylamide in 2.0 g of deionized water at a dissolving temperature of 25° C., a stirring speed of 300 rpm, and a stirring time of 0.5 h to obtain a functional monomer mixed solution.

[0097] Step 3: Dissolve 0.6 g of zinc sulfate heptahydrate in 1.0 g of deionized water at a stirring speed of 500 rpm, a stirring temperature of 25° C., and a stirring time of 0.5 h until the zinc sulfate heptahydrate is completely dissolved to obtain a zinc sulfate aqueous solution.

[0098] Step 4: Weigh 4.0 g of the chitosan solution prepared in step S1, and then slowly add 6.0 g of the functional monomer mixed solution prepared in step S2. The addition is completed in 2.0 h, with a stirring speed of 1000 rpm, a stirring temperature of 25° C., and a stirring time of 8.0 h.

[0099] Step 5: Slowly add 1.0 g of aqueous zinc sulfate solution to the mixed solution obtained in step 4 within 0.5 h, maintain stirring speed at 1000 rpm, and stir for 4.0 h.

[0100] Step 6: Slowly add 0.33 g of ammonium persulfate to the mixed solution obtained in step 5 within 0.5 h, maintain the stirring speed at 1000 rpm, and stir for 0.5 h.

[0101] Step 7: Heat the solution obtained in step 6 to 55°C, continue stirring, react for 8.0 hours, and then cool to room temperature to obtain a colorless and transparent hydrogel.

[0102] However, the prepared hydrogel has a voltage tolerance range of only 0 to 1.6 V, and cannot reach 0 to 2.0 V.

[0103] Comparative Example 3

[0104] Step 1: Add 10.0 g of dilute hydrochloric acid to 100 g of deionized water, stir at 800 rpm at 35 ° C, and continue stirring for 1.0 hour, then add 5.0 g of chitosan (50 mPa·s), maintain the temperature unchanged, increase the stirring speed to 1500 rpm, and continue stirring for 3.0 hours until the chitosan is completely dissolved in the deionized water, and naturally cool to 25 ° C to obtain a chitosan solution.

[0105] Step 2: Dissolve 1.0 g of methacrylic acid and 1.0 g of acrylamide in 2.0 g of deionized water at a dissolving temperature of 25° C., a stirring speed of 300 rpm, and a stirring time of 0.5 h to obtain a functional monomer mixed solution.

[0106] Step 3: Dissolve 0.6 g of zinc sulfate heptahydrate in 1.0 g of deionized water at a stirring speed of 500 rpm, a stirring temperature of 25° C., and a stirring time of 0.5 h until the zinc sulfate heptahydrate is completely dissolved to obtain a zinc sulfate aqueous solution.

[0107] Step 4: Weigh 4.0 g of the chitosan solution prepared in step S1, and then slowly add 6.0 g of the functional monomer mixed solution prepared in step S2. The addition is completed in 2.0 h, with a stirring speed of 1000 rpm, a stirring temperature of 25° C., and a stirring time of 8.0 h.

[0108] Step 5: Slowly add 0.05 g of aqueous zinc sulfate solution to the mixed solution obtained in step 4 within 0.5 h, maintain stirring speed at 1000 rpm, and stir for 4.0 h.

[0109] Step 6: Slowly add 0.33 g of cerium persulfate to the mixed solution obtained in step 5 within 0.5 h, maintain the stirring speed at 1000 rpm, and stir for 0.5 h.

[0110] Step 7: Heat the solution obtained in step 6 to 55°C, continue stirring, and react for 8.0 hours, then cool to room temperature to obtain a light yellow transparent hydrogel.

[0111] However, the prepared hydrogel has a voltage tolerance range of only 0 to 1.4 V, and cannot reach 0 to 2.0 V.

[0112] Comparative Example 4

[0113] Step 1: Add 10.0 g of dilute hydrochloric acid to 100 g of deionized water, stir at 800 rpm at 35°C for 1.0 hour, then add 5.0 g of sodium alginate, maintain the temperature unchanged, increase the stirring speed to 1500 rpm, and continue stirring for 3.0 hours until chitosan is completely dissolved in the deionized water, and cool naturally to 25°C to obtain a chitosan solution.

[0114] Step 2: Dissolve 1.0 g of methacrylic acid and 1.0 g of acrylamide in 2.0 g of deionized water at a dissolving temperature of 25° C., a stirring speed of 300 rpm, and a stirring time of 0.5 h to obtain a functional monomer mixed solution.

[0115] Step 3: Dissolve 0.6 g of zinc sulfate heptahydrate in 1.0 g of deionized water at a stirring speed of 500 rpm, a stirring temperature of 25° C., and a stirring time of 0.5 h until the zinc sulfate heptahydrate is completely dissolved to obtain a zinc sulfate aqueous solution.

[0116] Step 4: Weigh 4.0 g of the chitosan solution prepared in step 1, and then slowly add 6.0 g of the functional monomer mixed solution prepared in step 2. The solution system will immediately agglomerate to form a gel block, making subsequent experiments impossible.

[0117] Comparative Example 5

[0118] Step 1: Add 1.0 g of glacial acetic acid to 100 g of deionized water, stir at 800 rpm at 35 ° C, and continue stirring for 1.0 hour, then add 0.1 g of chitosan (200 mPa·s), maintain the temperature unchanged, increase the stirring speed to 1500 rpm, and continue stirring for 1.0 hour until the chitosan is completely dissolved in the deionized water, and naturally cool to 25 ° C to obtain a chitosan solution.

[0119] Step 2: Dissolve 5.0 g of methacrylic acid and 1.0 g of acrylamide in 2.0 g of deionized water at a dissolving temperature of 25° C., a stirring speed of 300 rpm, and a stirring time of 0.5 h to obtain a functional monomer mixed solution.

[0120] Step 3: Dissolve 0.3 g of ammonium zinc sulfate in 1.0 g of deionized water at a stirring speed of 500 rpm, a stirring temperature of 25° C., and a stirring time of 0.5 h until the ammonium zinc sulfate is completely dissolved to obtain an aqueous solution of zinc sulfate.

[0121] Step 4: Weigh 4.0 g of the chitosan solution prepared in step 1, and then slowly add 4.0 g of the functional monomer mixed solution prepared in step 2. The addition is completed in 2.0 hours, with a stirring speed of 1000 rpm, a stirring temperature of 25° C., and a stirring time of 6.0 hours.

[0122] Step 5: Slowly add 0.16 g of zinc salt aqueous solution to the mixed solution obtained in step 4 within 0.5 h, maintain stirring speed at 1000 rpm, and stir for 4.0 h.

[0123] Step 6: Slowly add 0.0816 g of cerium persulfate to the mixed solution obtained in step 5 within 0.5 h, maintain the stirring speed at 1000 rpm, and stir for 0.5 h.

[0124] Step 7: The solution obtained in step 6 was heated to 45° C. and stirred continuously for 6 h. The reaction time was then cooled to room temperature to obtain a light yellow transparent hydrogel.

[0125] The prepared hydrogel is completely hard and not flexible, and cannot meet the application requirements of flexible wearable electronic devices.

[0126] Comparative Example 6

[0127] Step 1: Add 1.0 g of glacial acetic acid to 100 g of deionized water, stir at 800 rpm at 35 ° C, and continue stirring for 1.0 hour, then add 0.1 g of chitosan (200 mPa·s), maintain the temperature unchanged, increase the stirring speed to 1500 rpm, and continue stirring for 1.0 hour until the chitosan is completely dissolved in the deionized water, and naturally cool to 25 ° C to obtain a chitosan solution.

[0128] Step 2: Dissolve 1.0 g of methacrylic acid and 5.0 g of acrylamide in 2.0 g of deionized water at a dissolving temperature of 25° C., a stirring speed of 300 rpm, and a stirring time of 0.5 h to obtain a functional monomer mixed solution.

[0129] Step 3: Dissolve 0.3 g of ammonium zinc sulfate in 1.0 g of deionized water at a stirring speed of 500 rpm, a stirring temperature of 25° C., and a stirring time of 0.5 h until the ammonium zinc sulfate is completely dissolved to obtain an ammonium zinc sulfate aqueous solution.

[0130] Step 4: Weigh 4.0 g of the chitosan solution prepared in step 1, and then slowly add 4.0 g of the functional monomer mixed solution prepared in step 2. The addition is completed in 2.0 hours, with a stirring speed of 1000 rpm, a stirring temperature of 25° C., and a stirring time of 6.0 hours.

[0131] Step 5: Slowly add 0.16 g of zinc salt aqueous solution to the mixed solution obtained in step 4 within 0.5 h, maintain stirring speed at 1000 rpm, and stir for 4.0 h.

[0132] Step 6: Slowly add 0.0816 g of cerium persulfate to the mixed solution obtained in step 5 within 0.5 h, maintain the stirring speed at 1000 rpm, and stir for 0.5 h.

[0133] Step 7: Heat the solution obtained in step 6 to 45°C, continue stirring, react for 6.0 hours, and then cool to room temperature to obtain a light yellow transparent hydrogel.

[0134] The prepared hydrogel is too soft to maintain a stable shape for a long time and does not meet the application requirements of flexible wearable electronic devices.

[0135] Comparative Example 7

[0136] Step 1: Add 1.0 g of glacial acetic acid to 100 g of deionized water, stir at 800 rpm at 25°C for 1.0 hour, then add 5 g of chitosan (200 mPa·s), maintain the temperature unchanged, and increase the stirring speed to 1500 rpm. Chitosan cannot be dissolved.

[0137] Comparative Table of Hydrogel Properties Prepared by Examples 1 to 3 and Comparative Examples 1 to 7

[0138]

Claims

1. A method for preparing a hydrogel with high sensitivity detection performance, characterized in that: The following steps are involved: Step 1, preparing chitosan solution, functional monomer mixed solution, and zinc salt solution respectively; Step 2, slowly adding the functional monomer mixed solution to the chitosan solution, stirring after the addition is completed, to obtain a first mixed solution; wherein the mass ratio of the chitosan solution to the functional monomer mixed solution is 4.0: (1.0-6.0); Step 3, slowly adding the zinc salt solution to the first mixed solution, stirring after the addition is completed, to obtain a second mixed solution; wherein the mass ratio of the first mixed solution to the zinc salt solution is 5:(0.1-0.5); Step 4: slowly dropwise adding the initiator to the second mixed solution to obtain a third mixed solution after the dropwise addition is complete; wherein the mass ratio of the second mixed solution to the initiator is 100:(1.0-3.0); Step 5: After heating and stirring the third mixed solution, cooling it to room temperature to obtain a hydrogel.

2. The method for preparing a hydrogel with high sensitivity detection performance according to claim 1, characterized in that: The preparation of chitosan solution in step 1 comprises the following steps: Add a certain amount of acid into deionized water, stir at 800-900 rpm at 35-40°C, and continue stirring for 0.8-1.0 h; Then chitosan was added, the temperature was maintained constant, the stirring speed was increased to 1500-1600 rpm, and stirring was continued for 1.0-3.0 h until the chitosan was completely dissolved in the deionized water, and the mixture was naturally cooled to room temperature to obtain a chitosan solution; The mass ratio of chitosan, deionized water, and acid is (1.0-5.0):100:(1.0-10.0).

3. The method for preparing a hydrogel with high sensitive detection performance according to claim 1, characterized in that: The step 1 of preparing the functional monomer mixed solution comprises the following steps: Dissolve a certain amount of methacrylic acid and acrylamide in deionized water at a dissolving temperature of 25°C, stir at a speed of 300 to 400 rpm, and continue stirring for 0.5 to 1 hour to obtain a functional monomer mixed solution; The mass ratio of methacrylic acid, acrylamide and deionized water is (1.0-4.0): (1.0-4.0): 2.

0.

4. The method for preparing a hydrogel with high sensitivity detection performance according to claim 1, characterized in that: The preparation of the zinc salt solution in step 1 comprises the following steps: Mix a certain amount of zinc salt with deionized water, and stir at a stirring speed of 400 to 500 rpm, a stirring temperature of 25° C., and a stirring time of 0.5 to 1 h to obtain a zinc salt solution; Wherein, the mass ratio of zinc salt to deionized water is (0.1-0.6):1.

0.

5. The method for preparing a hydrogel with high sensitive detection performance according to claim 1, characterized in that: The dropping time in step 2 is 2.0 to 2.5 hours; the stirring conditions are: stirring speed 1000 to 1200 rpm, stirring temperature 25° C., and stirring time 6.0 to 8.0 hours.

6. The method for preparing a hydrogel with high sensitive detection performance according to claim 1, characterized in that: The dropping time in step 3 is 0.5 to 1 h; the stirring conditions are: stirring speed 1000 to 1200 rpm, stirring for 3 to 4.0 h.

7. The method for preparing a hydrogel with high sensitive detection performance according to claim 1, characterized in that: The dropping time in step 4 is 0.5 to 1 hour; the stirring conditions are: stirring speed 1000 to 1200 rpm, stirring 0.5 to 1 hour.

8. The method for preparing a hydrogel with high sensitive detection performance according to claim 1, characterized in that: The heating and stirring conditions in step 5 are: heating temperature is 45-55° C., and stirring time is 6.0-8.0 h.

9. A hydrogel with high sensitive detection performance, characterized in that: The hydrogel is prepared by the method for preparing a hydrogel with high sensitive detection performance as described in any one of claims 1 to 8.

10. Use of the hydrogel with high sensitive detection performance as claimed in claim 9 in flexible wearable electronic devices.