Aliphatic polycarbonate containing different cyclic substituent groups and preparation method thereof
By introducing aliphatic polycarbonate with different cyclic substituents in polycarbonate synthesis, the ring-opening polymerization reaction is used to solve the preparation problems of high molecular weight and high mechanical strength in the prior art, and the preparation of high-performance polycarbonate is realized , has good heat resistance and mechanical properties, which broadens its application range.
Patent Information
- Application Number
- CN202411210051.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-30
AI Technical Summary
In the field of polycarbonate synthesis, it is difficult to prepare high molecular weight and high mechanical strength aliphatic polycarbonate in the prior art, limiting its widespread use in industrial applications.
By introducing aliphatic polycarbonate with different cyclic substituents, 6,8-dioxaspiro[3.5]nono-7-one, 7,9-dioxaspiro[4.5]dec-8-one or 2 ,4-dioxaspiro[5.5]undecane-3-one is used as a monomer, and the ring-opening polymerization reaction is carried out under melting conditions, using stannous octanoate or Lewis acid and Lewis base as catalysts, and small alcohol molecules are used as initiators. and prepare polycarbonate with high molecular weight and high mechanical strength.
It has achieved high molecular weight and high mechanical strength polycarbonate preparation, with good heat resistance and mechanical properties, avoided side reactions under high temperature and high pressure conditions, uniform molecular weight distribution, significantly improved melting temperature and glass transition temperature, widened Application range of degradable polycarbonate materials.
Smart Images

Figure CN118955885A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer material synthesis, and in particular relates to aliphatic polycarbonate containing different cyclic substituents and a preparation method thereof. Background Art
[0002] Polycarbonate can be divided into aromatic, aliphatic, and aromatic-aliphatic polycarbonates according to the different R groups in the molecular chain. Aromatic polycarbonate is a thermoplastic engineering plastic with good comprehensive properties such as thermal properties, mechanical properties and optical properties. It is widely used in electronic appliances, panels, automotive parts, packaging, aviation, medical equipment and other fields, but it is difficult to process and not easy to degrade. Compared with aromatic polycarbonate, the molecular chain rigidity of aliphatic polycarbonate is weaker, so the thermal and mechanical properties are poor, which limits its industrial application. Biodegradable aliphatic polycarbonate has surface solubility and can be completely degraded into neutral diols and CO2. It also has good biocompatibility, and the main chain chemical structure can be adjusted through reaction. A variety of products can be produced to meet the needs of different fields. In particular, the relative weight average molecular weight of 7×10 4 The above high molecular weight aliphatic polycarbonates have good thermal and mechanical properties and can replace the polymer products previously used in the field of biodegradable plastics (Reference: Research Progress of Aliphatic Polycarbonates [J]. Contemporary Chemical Industry, 2018, 47, 1709-1712).
[0003] At present, there are four methods for synthesizing aliphatic polycarbonates: phosgene method, copolymerization of carbon dioxide and epoxide, ring-opening polymerization of aliphatic cyclic carbonate, and transesterification. Among them, the phosgene method is relatively toxic, has low yield, low molecular weight, and poor product performance, which limits its application; the copolymerization of carbon dioxide and epoxide has poor controllability and low molecular weight; the transesterification method requires reaction under harsh conditions such as high temperature and high vacuum, and the polymerization process is usually accompanied by many side reactions, such as backbiting at the chain end to generate cyclic low molecular weight polycarbonate; 1,4-butanediol is dehydrated to generate tetrahydrofuran, etc. (Reference: Macromolecules 2013, 46, 3301-330). In contrast, the ring-opening polymerization of aliphatic cyclic carbonates not only has relatively mild reaction conditions and the advantages of high and controllable molecular weight, but can also be ring-opened copolymerized with a variety of carbonate monomers to adjust polymer properties. For example, the ring-opening copolymerization of trimethylene carbonate and 2,2-diethyl-trimethylene carbonate not only has a controllable molecular weight, but also has the advantages of two polymers (reference: Macromolecules 2023, 56, 3641-3649).
[0004] The thermal and mechanical properties of polycarbonate are not only related to the molecular weight, but also depend on its chain structure and side functional groups, such as increasing the number of continuous methylene groups between two adjacent carbonate groups, changing the main chain structure, and introducing methods containing functional groups or reactive groups. Suitable functional groups can effectively regulate the physical and chemical properties and biological properties of polymer materials, such as hydrophilicity, permeability, degradability, biocompatibility, cell adhesion, etc.; and the introduction of functional groups provides greater possibilities for further modification of materials. The research on the functionalization of six-membered and seven-membered cyclic carbonates is the most common. Common functional groups such as hydroxyl, carboxyl, amino, sugar ring, etc. can be introduced into carbonate monomers (reference: Research Progress of Trimethylene Carbonate-Responsive Aliphatic Polycarbonates [J]. Polymer Bulletin, 2024, 37, 603-615). Taking the monomer trimethylene carbonate (TMC) as an example, the polymer obtained by ring-opening polymerization itself cannot crystallize, has poor mechanical properties, and a glass transition temperature of -17.8°C. When regular side groups are introduced into the monomer, such as two methyl groups, the monomer becomes 2,2-dimethyltrimethylene carbonate (DMTMC), and the resulting polymer exhibits crystallinity, a glass transition temperature of 19.7°C, and a melting point of about 120°C (reference: Macromolecules 2023, 56, 2062-206); when two ethyl groups are introduced, the monomer becomes 2,2-diethyltrimethylene carbonate, and the resulting polymer also exhibits crystallinity, a glass transition temperature of -6°C, and a melting point of about 90°C (reference: Macromolecules 2023, 56, 3641-3649); although the above examples improve their crystallization properties by introducing regular functional groups, the melting point is not high enough and the heat resistance is not good enough. In addition to introducing relatively regular groups, irregular side groups can also be introduced. Ethyl and allyloxymethyl groups are introduced at the same time, and the monomer becomes 2-allyloxymethyl-2-ethyltrimethylene carbonate (AOMEC). Double bonds are introduced into the side groups, so that the polymer can be post-functionalized (reference: Macromolecules 2014, 47, 6189-6195). The literature does not disclose relevant information such as the mechanical properties of the polycarbonate. Generally speaking, the structure is too irregular to crystallize, and the performance is usually poor.
[0005] From the above analysis, it can be seen that in the field of polycarbonate synthesis, it is still a great challenge to prepare aliphatic polycarbonates with both high molecular weight and high mechanical strength by ring-opening polymerization. High molecular weight and high mechanical strength can make the application range of polycarbonate more extensive. Therefore, it is very necessary to provide a method for synthesizing polycarbonate with high molecular weight and high mechanical strength to promote the development of high-performance polycarbonate. Summary of the invention
[0006] The object of the present invention is to provide aliphatic polycarbonate containing different cyclic substituents and a preparation method thereof. The provided aliphatic polycarbonate containing different cyclic substituents has high molecular weight and high mechanical strength.
[0007] To achieve the above object, the present invention provides the following technical solutions:
[0008] One of the technical solutions of the present invention is to provide an aliphatic polycarbonate containing different cyclic substituents, the structural formula of which is as follows:
[0009]
[0010] In the above formula, x=1, 2 or 3.
[0011] When x=1, the aliphatic polycarbonate is P(4C-TMC); when x=2, the aliphatic polycarbonate is P(5C-TMC); when x=3, the aliphatic polycarbonate is P(6C-TMC).
[0012] The second technical solution of the present invention is to provide a method for preparing the above-mentioned aliphatic polycarbonate containing different cyclic substituents. When x=1, 2 or 3, the preparation steps include:
[0013] Using 6,8-dioxaspiro[3.5]nonane-7-one (4C-TMC), 7,9-dioxaspiro[4.5]decane-8-one (5C-TMC) or 2,4-dioxaspiro[5.5]undecane-3-one (6C-TMC) as monomers, stannous octoate as a catalyst, and alcohol small molecules as an initiator, a ring-opening polymerization reaction is carried out under the condition of monomer melting to prepare an aliphatic polycarbonate containing a cyclic substituent structure;
[0014] When x=3, the preparation steps include:
[0015] The 2,4-dioxaspiro[5.5]undecane-3-one (6C-TMC) monomer is dissolved in a solvent, a Lewis pair consisting of a Lewis acid and a Lewis base is used as a catalyst, and an alcohol small molecule is used as an initiator to carry out a ring-opening polymerization reaction to prepare an aliphatic polycarbonate containing a cyclic substituent structure.
[0016] The reaction formula is shown below:
[0017]
[0018] In the preparation method provided by the present invention, polymers that are not easily soluble, such as P(4C-TMC) and P(5C-TMC), can be prepared by adding 4C-TMC or 5C-TMC monomers under molten conditions; polymers that can be dissolved under certain solvent conditions, such as P(6C-TMC), can be prepared by adding 6C-TMC monomers under molten conditions, or by dissolving 6C-TMC in a solvent and then performing a ring-opening polymerization reaction for preparation.
[0019] Preferably, the alcohol small molecule is benzyl alcohol.
[0020] Preferably, the molar ratio of the catalyst, initiator and monomer is 1:1:1000-2000.
[0021] Preferably, the temperature of the ring-opening polymerization reaction is 50 to 150° C., and the time is 1 to 24 hours.
[0022] Preferably, the Lewis acid is diphenylzinc (Zn(C6H5)2); the Lewis base is 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU); and the molar ratio of the Lewis acid to the Lewis base in the Lewis pair is 1:1.
[0023] Preferably, the solvent is toluene, and the concentration of 2,4-dioxaspiro[5.5]undecan-3-one in toluene is 0.5 mol / L.
[0024] The beneficial technical effects of the present invention are as follows:
[0025] Compared with most aliphatic polycarbonates currently on the market, the present invention introduces cyclic substituents on the basis of the original 1,3-dioxane-2-one (TMC), so that it has both the degradability of aliphatic polycarbonates and the good heat resistance and mechanical properties of aromatic polycarbonates. At the same time, the polymerization method provided by the present invention does not require high temperature and high pressure to eliminate small molecule by-products, the reaction conditions are relatively mild, the controllability is better, and the polymer molecular weight is higher. The present invention uses Lewispair composed of Lewis acid and Lewis base as a catalyst. The Lewis acid / base synergistic effect can effectively inhibit the ester exchange side reaction of the polymerization reaction, and it is easy to prepare high molecular weight polycarbonate materials. The number average molecular weight of P(5C-TMC) and P(4C-TMC) in the polycarbonate obtained by the present invention is 175000-227000Da, the molecular weight distribution is 1.5-1.82, both are crystalline polymers, and the melting temperatures are 208.9℃-217.5℃ and 181.6℃-187.2℃ respectively; the number average molecular weight of P(6C-TMC) is 14700-153500Da, the molecular weight distribution is 1.29-1.98, and the glass transition temperature is 34℃. The polycarbonate obtained by the present invention has excellent mechanical properties. For P(4C-TMC), the breaking strength is 72MPa and the breaking elongation is 4.5%; for P(5C-TMC), the breaking strength is 65MPa and the breaking elongation is 3.5%; for P(6C-TMC), the yield strength is 29MPa, the breaking elongation is 300%, and the breaking strength is 21MPa.
[0026] The invention provides 6,8-dioxaspiro[3.5]nonane-7-one (4C-TMC), 7,9-dioxaspiro[4.5]decane-8-one (5C-TMC) and 2,4-dioxaspiro[5.5]undecane-3-one (6C-TMC) for preparing polycarbonate with high molecular weight and high mechanical strength, which is of great significance for achieving high performance of polycarbonate and broadening the application scope of degradable polycarbonate materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 P(4C-TMC) prepared in Example 1 of the present invention 1 HNMR spectrum;
[0028] Figure 2 The DSC curve of P(4C-TMC) prepared in Example 1 of the present invention;
[0029] Figure 3 is the stress-strain curve of P(4C-TMC) prepared in Example 1 of the present invention;
[0030] Figure 4 P(5C-TMC) prepared in Example 2 of the present invention 1HNMR spectrum;
[0031] Figure 5 The DSC curve of P(5C-TMC) prepared in Example 2 of the present invention;
[0032] Figure 6 is the stress-strain curve of P(5C-TMC) obtained in Example 2 of the present invention;
[0033] Figure 7 P(6C-TMC) prepared in Example 3 of the present invention 1 HNMR spectrum;
[0034] Figure 8 The DSC curve of P(6C-TMC) prepared in Example 3 of the present invention;
[0035] Fig. 9 This is the stress-strain curve of P(6C-TMC) obtained in Example 3 of the present invention. DETAILED DESCRIPTION
[0036] Now, various exemplary embodiments of the present invention are described in detail, and this detailed description should not be considered as a limitation of the present invention, but should be understood as a more detailed description of certain aspects, characteristics and embodiments of the present invention. It should be understood that the terms described in the present invention are only for describing specific embodiments and are not used to limit the present invention.
[0037] In addition, for the numerical range in the present invention, it is understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0038] Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which the invention pertains. Although only preferred methods and materials have been described herein, any methods and materials similar or equivalent to those described herein may also be used in the practice or testing of the invention.
[0039] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0040] In the process of preparing aliphatic polycarbonate by ring-opening polymerization of monomers 6,8-dioxaspiro[3.5]nonane-7-one, 7,9-dioxaspiro[4.5]decane-8-one and 2,4-dioxaspiro[5.5]undecane-3-one of the present invention, all operations sensitive to moisture and oxygen are carried out by professionals familiar with the technical field in an MBraun glove box or using standard Schlenk technology under nitrogen protection.
[0041] When the prepared polymer is subjected to relevant tests, the structure of the polymer is determined by nuclear magnetic resonance spectroscopy, the molecular weight and molecular weight distribution index of the polymer are determined by gel chromatography (GPC), the thermal properties of the polymer are determined by differential scanning calorimetry, and the mechanical properties of the polymer are determined by a universal tensile machine. 1 H and 13 C NMR was measured by a Bruker-400 NMR instrument at 25°C, TMS was used as the internal standard, and the solvent was deuterated chloroform; gel chromatography was measured by a Waters gel permeation chromatograph: tetrahydrofuran (THF) (with 0.05 wt% of 2,6-di-tert-butyl-4-methylphenol as an antioxidant) or hexafluoroisopropanol (HFIP) (with 0.05 wt% of sodium trifluoroacetate as an antioxidant) as the solvent, the test temperature was 40°C, the flow rate was 1.0 mL / min, and PL EasiCal was used. PS-1 is the standard sample; the differential scanning calorimeter is measured by TA, firstly heating to 250.00°C at a rate of 2.000°C / min, keeping the temperature constant for 10.00min, then cooling at a rate of 2.000°C / min to -50.00°C, and then keeping the temperature constant for 10.00min for the second heating; when the mechanical properties are measured by the universal stretching machine, the polymer is directly hot-pressed into 2×12mm tensile strips at 10-20°C above the melting point, and the stretching rate is 10mm / min.
[0042] The stannous octoate, Zn(C6H5)2 and DBU used in the examples of the present invention are all commercially available catalysts.
[0043] Example 1
[0044] Preparation of P(4C-TMC):
[0045] (1) In an inert atmosphere, 20000 μmol of 6,8-dioxaspiro[3.5]nonan-7-one was added to a dry 15 mL pressure bottle, and 20 μmol of benzyl alcohol and 20 μmol of stannous octoate were added to 0.2 mL of toluene solvent to prepare a catalyst solution. After shaking evenly, 0.1 mL of the catalyst solution was injected into the pressure bottle, and ring-opening polymerization was carried out at 150° C. The polymerization reaction was carried out for 8 hours under strong stirring.
[0046] (2) After the polymerization is completed, the polymer is first dissolved in a mixed solvent of dichloromethane and hexafluoroisopropanol, and then the polymer solution is added dropwise to 100 mL of ethanol for precipitation, and then filtered, washed, and vacuum dried to obtain P(4C-TMC).
[0047] The conversion rate of 6,8-dioxaspiro[3.5]nonan-7-one monomer in this example is >99%.
[0048] The prepared P(4C-TMC) was subjected to NMR analysis, GPC analysis, DSC analysis and mechanical property test: NMR analysis showed that the polycarbonate content of the polymer was >99%; GPC analysis results showed that the polymer molecular weight was 175 kDa and the molecular weight distribution was 1.82; DSC analysis showed that the polymer T m The test results of the universal tensile machine show that the elongation at break of the polymer prepared in Example 1 is 4.5%, and the breaking strength is 72 MPa.
[0049] Example 1 P (4C-TMC) 1 H NMR spectrum is shown in Figure 1 .
[0050] The DSC curve of P(4C-TMC) obtained in Example 1 is shown in Figure 2 .
[0051] The stress-strain curve of P(4C-TMC) obtained in Example 1 is shown in Figure 3 .
[0052] Example 2
[0053] Preparation of P(5C-TMC):
[0054] (1) In an inert atmosphere, 20000 μmol 7,9-dioxaspiro[4.5]decan-8-one was added to a dry 15 mL pressure bottle, and 20 μmol benzyl alcohol and 20 μmol stannous octoate were added to 0.2 mL toluene solvent to prepare a catalyst solution. After shaking evenly, 0.1 mL of the catalyst solution was injected into the pressure bottle, and ring-opening polymerization was carried out at 150° C. The polymerization reaction was carried out for 8 hours under strong stirring.
[0055] (2) After the polymerization is completed, the polymer is first dissolved in a mixed solvent of dichloromethane and hexafluoroisopropanol, and then the polymer solution is added dropwise to 100 mL of ethanol for precipitation, and then filtered, washed, and vacuum dried to obtain P(5C-TMC).
[0056] The conversion rate of 7,9-dioxaspiro[4.5]decan-8-one monomer in this example was 93.5%.
[0057] The prepared P(5C-TMC) was subjected to NMR analysis, GPC analysis, DSC analysis and mechanical property test: NMR analysis showed that the polycarbonate content of the polymer was >99%; GPC analysis results showed that the polymer molecular weight was 227.1 kDa and the molecular weight distribution was 1.50; DSC analysis showed that the polymer T m The temperatures were 181.6°C and 187.2°C; the test results of the universal tensile machine showed that the elongation at break of the polymer prepared in Example 2 was 3.5%, and the breaking strength was 65 MPa.
[0058] Example 2 P (5C-TMC) 1 H NMR spectrum is shown in Figure 4 .
[0059] The DSC curve of P(5C-TMC) obtained in Example 2 is shown in Figure 5 .
[0060] The stress-strain curve of P(5C-TMC) obtained in Example 2 is shown in Figure 6 .
[0061] Example 3
[0062] Preparation of P(6C-TMC):
[0063] (1) In an inert atmosphere, 20000 μmol of 2,4-dioxaspiro[5.5]undecan-3-one was added to a dry 15 mL pressure bottle, and 20 μmol of benzyl alcohol and 20 μmol of stannous octoate were added to 0.2 mL of toluene solvent to prepare a catalyst solution. After shaking evenly, 0.1 mL of the catalyst solution was injected into the pressure bottle, and ring-opening polymerization was carried out at 150° C. The polymerization reaction was carried out for 8 h under strong stirring.
[0064] (2) After the polymerization is completed, the polymer is first dissolved in dichloromethane, and then the polymer solution is dropped into 100 mL of ethanol for precipitation, and then filtered, washed, and vacuum dried to obtain P(6C-TMC).
[0065] The 2,4-dioxaspiro[5.5]undecane-3-one monomer conversion rate in this example was 70.4%.
[0066] The prepared P(6C-TMC) was subjected to NMR analysis, GPC analysis, DSC analysis and mechanical property test: NMR analysis showed that the polycarbonate content of the polymer was >99%; GPC analysis results showed that the polymer molecular weight was 153.5 kDa and the molecular weight distribution was 1.98; DSC analysis showed that the polymer T g The temperature is 34°C; the test results of the universal tensile machine show that the polymer obtained in Example 3 has a yield strength of 29 MPa, an elongation at break of 300%, and a breaking strength of 21 MPa.
[0067] Example 3 P(6C-TMC) 1 H NMR spectrum is shown in Figure 7 .
[0068] The DSC curve of P(6C-TMC) obtained in Example 3 is shown in Figure 8 .
[0069] The stress-strain curve of P(6C-TMC) obtained in Example 3 is shown in Fig. 9 .
[0070] Example 4
[0071] Preparation of P(6C-TMC):
[0072] (1) Under an inert atmosphere, 10000 μmol 2,4-dioxaspiro[5.5]undecane-3-one and 19.8 mL toluene were added to a dry 50 mL pressure bottle, and 0.4 mL toluene, 20 μmol benzyl alcohol, 20 μmol Zn(C6H5)2 and 20 μmol DBU were added to another sample bottle to prepare a catalyst solution. After shaking evenly, 0.2 mL of the catalyst solution was injected into the pressure bottle, and the ring-opening polymerization was carried out at 50°C. The polymerization reaction was carried out for 24 hours under strong stirring;
[0073] (2) After the polymerization is completed, the polymer is first dissolved in dichloromethane, and then the polymer solution is added dropwise to 100 mL of ethanol for precipitation, and then filtered, washed, and vacuum dried to obtain P(6C-TMC).
[0074] The 2,4-dioxaspiro[5.5]undecan-3-one monomer conversion rate in this example is 70.4%.
[0075] The prepared P(6C-TMC) was subjected to NMR analysis, GPC analysis, DSC analysis and mechanical property test: NMR analysis showed that the polycarbonate content of the polymer was >99%; GPC analysis results showed that the polymer molecular weight was 142.4 kDa and the molecular weight distribution was 1.45; DSC analysis showed that the polymer T g is 34℃.
[0076] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. Aliphatic polycarbonates containing different cyclic substituents, characterized in that: The structural formula is as follows: In the above formula, x=1, 2 or 3.
2. The method for preparing aliphatic polycarbonate containing different cyclic substituents according to claim 1, characterized in that: When x=1, 2 or 3, the preparation steps include: With 6,8-dioxaspiro[3.5]nonane-7-one, 7,9-dioxaspiro[4.5]decane-8-one or 2,4-dioxaspiro[5.5]undecane-3-one as monomers, stannous octoate as catalyst and alcohol small molecule as initiator, ring-opening polymerization reaction is carried out under the condition of monomer melting to prepare aliphatic polycarbonate containing cyclic substituents.
3. The method for preparing aliphatic polycarbonate containing different cyclic substituents according to claim 1, characterized in that: When x=3, the preparation steps include: The 2,4-dioxaspiro[5.5]undecane-3-one monomer is dissolved in a solvent, a Lewis pair consisting of a Lewis acid and a Lewis base is used as a catalyst, and an alcohol small molecule is used as an initiator to carry out a ring-opening polymerization reaction to prepare an aliphatic polycarbonate containing a cyclic substituent.
4. The method for preparing aliphatic polycarbonate containing different cyclic substituents according to claim 2 or 3, characterized in that: The alcohol small molecule is benzyl alcohol.
5. The method for preparing aliphatic polycarbonate containing different cyclic substituents according to claim 2 or 3, characterized in that: The molar ratio of the catalyst, the initiator and the monomer is 1:1:1000-2000.
6. The method for preparing aliphatic polycarbonate containing different cyclic substituents according to claim 2 or 3, characterized in that: The temperature of the ring-opening polymerization reaction is 50-150° C., and the time is 1-24 hours.
7. The method for preparing aliphatic polycarbonate containing different cyclic substituents according to claim 3, characterized in that: The Lewis acid is diphenylzinc; the Lewis base is 1,8-diazabicyclo[5.4.0]undec-7-ene; and the molar ratio of the Lewis acid to the Lewis base in the Lewispair is 1:
1.
8. The method for preparing aliphatic polycarbonate containing different cyclic substituents according to claim 3, characterized in that: The solvent is toluene, and the concentration of 2,4-dioxaspiro[5.5]undecan-3-one in toluene is 0.5 mol / L.
Citation Information
Patent Citations
Biodegradable slow / controlled-release drug delivery system and preparation method thereof
CN106667897A
Polycarbonate resin composition
CN116507671A
Crystalline aliphatic polycarbonate with high molecular weight and high mechanical property and preparation method thereof
CN117004007A
Improved method for production of poly(trimethylene carbonate)
CN1449422A
Poly (2, 2-dimethylene dioxy group-1, 3 propylene glycol carbonic ester), preparaton method and application
CN1563144A