Wear-resistant non-slip rubber composite material and preparation method thereof
By using the combination of superpolymeric natural rubber, rare earth butyl rubber and polar rubber in sole materials, combined with a modification method of silane coupling agent and an alcohol amine solvent, the white carbon black is solved in the prior art. The problem of improving wear resistance and slip resistance of the sole material is difficult and costly, sole materials with high performance and good processability are achieved.
Patent Information
- Application Number
- CN202411290407.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-11-15
AI Technical Summary
Existing sole materials face matrix selection and nanofiller dispersion problems when improving wear resistance and anti-slip properties, resulting in difficult performance improvement, high cost and poor processability, which makes it difficult to meet various needs.
Using the coordinated cooperation of superpolymeric natural rubber, rare earth butyl rubber and polar rubber, white carbon black is modified through chemical and physical modification methods of silane coupling agent and alcohol amine solvent to form a stronger interface effect and enhance Wear resistance and anti-slip properties of rubber composites.
It achieves high wear resistance, anti-slip properties and good rebound properties of sole materials, while reducing raw material costs, improving processability, and suitable for large-scale production.
Smart Images

Figure BDA0005044409990000141 
Figure BDA0005044409990000151
Abstract
Description
Technical Field
[0001] The invention belongs to the field of shoe materials, and in particular relates to a wear-resistant and anti-skid rubber composite material and a preparation method thereof. Background Art
[0002] The outsole (also known as the "outsole") is the part of the shoe that is in direct contact with the ground. The wear resistance and anti-skid properties (also known as "anti-slip properties") of the outsole material are key indicators for measuring the quality and technical level of footwear products. The outsole wear process is a microscopic friction process of stretching and tearing when the outsole is against the ground during exercise. At the same time, wear resistance also affects the anti-slip properties of the outsole. For example, the outsole with poor wear resistance will be worn out quickly during use, and the grip will decrease, causing slipping when walking or exercising, affecting sports safety. The anti-slip properties of the outsole are divided into dry anti-slip and wet anti-slip, which measure the grip of the outsole in dry and wet environments respectively. The anti-slip properties are directly related to people's safety performance. Therefore, in order to ensure people's walking or sports safety, research on the high wear resistance and anti-slip properties of the outsole is also a hot topic.
[0003] Rubber materials are widely used in the field of shoe outsoles due to their excellent elasticity, elongation and flex resistance. Traditional shoe outsoles mainly use butyl rubber as the main rubber, and use some natural rubber, styrene-butadiene rubber, EPDM rubber, nitrile rubber and other rubbers to balance the wear resistance and anti-slip performance of the outsole material. However, there are two key problems in improving the performance of traditional rubber outsole materials: one is the selection of rubber matrix. Traditional butyl rubber is mainly based on lithium, cobalt and nickel. The type and proportion of catalysts have a great influence on wear resistance or anti-slip performance. It can only balance wear resistance or anti-slip performance, but it is difficult to improve wear resistance and anti-slip performance at the same time. The traditional natural rubber preparation process will go through acid flocculation, crushing, high-temperature baking and other processes, which will lead to the loss of non-rubber components in the natural rubber raw materials, the decrease of rubber molecular weight, and the decrease of elasticity, strength and wear resistance of natural rubber; secondly, the filler dispersion and mixing interface. The pure rubber has low strength and poor wear resistance, and needs to be filled with nanofillers for reinforcement to meet the use requirements. The degree of dispersion of a large number of inorganic nanoparticles in the organic rubber matrix and the strength of the interface between the nanoparticles and the rubber matrix are the key to determining the comprehensive performance of rubber composite materials. Therefore, in the rubber outsole formula, in addition to conventional antioxidants, vulcanizers and plasticizers, the rubber matrix selection and the modification and dispersion method of nanofillers are particularly important.
[0004] Patent application CN117511013A discloses a weather-resistant, super-wear-resistant, non-slip rubber material with synthetic rubber as the main material. The formula design balances the soft wear-resistant properties of rare earth cis-1,4-butadiene rubber molecules and the saturated weather resistance and non-slip properties of brominated butyl rubber. However, due to the hysteresis loss of the side chain of brominated butyl rubber molecules, mixing and processing are difficult, and the high saturation structure of brominated butyl also brings problems such as slow vulcanization speed.
[0005] Patent application CN117430875A discloses a wear-resistant and non-slip material with rare earth cis-1,2-butadiene rubber, isoprene rubber and EPDM rubber as main rubbers, bio-based silica as reinforcing filler, and silica activator and silane coupling agent are added to improve the dispersibility of silica. Due to the large number of components and large amount of silica modifier in the rubber mixing process, the modification efficiency of silica modifier is low, and the modification effect of silica cannot be achieved by simple mechanical blending, so the material's superior performance cannot be fully exerted.
[0006] Patent application CN116535749A discloses a method for preparing an extremely wear-resistant and highly anti-slip rubber outsole, selecting three rubber systems: tin chloride modified rare earth butadiene rubber, methyl methacrylate grafted modified natural rubber copolymer, and hydrogenated nitrile rubber; in terms of fillers, coupling agent-modified carbon nitride and methacrylic acid-modified fumed silica are selected. Although the results mentioned that it can achieve extremely wear-resistant and high anti-slip properties, from the perspective of raw materials, the molecular regularity of rare earth rubber modified with tin chloride is generally higher, but the molecular chain mobility will decrease, the elongation characteristics are insufficient, and the rare earth modification superimposed tin coupling preparation process is relatively complicated, so the main material cost is relatively high; in addition, for the methyl methacrylate grafting modification of natural rubber, methyl methacrylate modification mainly includes chemical initiation, radiation initiation and photoinitiation. The modification requires the introduction of small molecules such as monomers and initiators. The preparation process of raw materials is complicated. At the same time, the drying or washing process during the modification process will also cause the loss of non-rubber components such as proteins and phospholipids in natural rubber, affecting the processing properties of the natural rubber material itself. While increasing the polarity of natural rubber molecules, it will also cause the elasticity of natural rubber materials to decrease. From the perspective of fillers, the hydroxyl groups on the surface of carbon nitride or fumed silica that are not chemically grafted can still form hydrogen bonds, which will induce the aggregation of inorganic nanoparticles. The inorganic component aggregates are also prone to form defects around the aggregates due to the difference in modulus between the filler and the rubber matrix under the dynamic strain of the sole rubber material. In short, this type of rubber outsole has high raw material costs and poor processability of the rubber matrix, making it unsuitable for large-scale production.
[0007] Therefore, although the industry has conducted a lot of research on the wear resistance and anti-slip properties of soles, there is still a need to continuously explore rubber matrix materials and filler modification and dispersion technologies with better performance to meet the multi-faceted needs of outsole materials for super wear resistance and high anti-slip performance, cost, and processability. Summary of the invention
[0008] In view of the problem that the wear resistance and anti-skid property, cost, processability and other multi-faceted requirements of the soles in the prior art still need to be continuously improved, the present invention provides a wear-resistant and anti-skid rubber composite material for soles and a preparation method thereof.
[0009] The technical solution of the present invention is as follows:
[0010] A wear-resistant and non-slip rubber composite material comprises, by mass fraction, 10-50 parts of superpolymerized natural rubber, 30-80 parts of rare earth cis-1,4-butadiene rubber, 5-20 parts of polar rubber, 3-8 parts of zinc oxide, 0.5-3 parts of stearic acid, 10-90 parts of modified white carbon black, 0.5-5 parts of antioxidant, 0.5-20 parts of plasticizer, 1-5 parts of accelerator and 1-5 parts of sulfur; wherein the sum of the mass fractions of the superpolymerized natural rubber, the rare earth cis-1,4-butadiene rubber and the polar rubber is 100 parts; the modified white carbon black is firstly chemically modified by an ethanol solution of a silane coupling agent, and then physically modified by an ethanol solution of at least one of polyethylene glycol, diethanolamine, triethanolamine, butanediamine and tetramethylenetetramine.
[0011] Furthermore, the polar rubber is one or more of nitrile rubber, carboxyl nitrile, hydrogenated nitrile rubber, the acrylonitrile content in the polar rubber is 10-50%, the Mooney viscosity ML (1+4) at 100°C is 30-100, and the molecular weight is 500,000-1,000,000.
[0012] Furthermore, the cis structure content in the rare earth butadiene rubber is greater than 96%, the Mooney viscosity ML (1+4) at 100° C. is 40 to 80, and the molecular weight is 400,000 to 800,000.
[0013] Furthermore, the rubber hydrocarbon content in the hyperpolymerized natural rubber is 97-99%, the non-rubber component content is 1-3%, the Mooney viscosity ML (1+4) at 100° C. is 40-90, and the molecular weight is 1.5 million to 2.5 million.
[0014] Furthermore, the specific modification method of modified silica includes the following steps:
[0015] S1. Add the powder of white carbon black into a high-speed stirring mixer with electric heating and vacuuming functions, set the stirring speed of the mixer to 100-2000rpm, spray the ethanol dispersion of silane coupling agent with a concentration of 5-50wt% onto the white carbon black powder by using an atomizing device, and control the amount of coupling agent to be 2-15wt% of the mass of white carbon black; then vacuum the high-speed stirrer, turn on the heating, set the temperature to 100-150°C, the reaction time to 10-60min, release the pressure after stirring, and set the temperature to 30-70°C;
[0016] S2. Spraying an ethanol dispersion of at least one of polyethylene glycol, diethanolamine, triethanolamine, butanediamine and tetramethylenetetramine onto the chemically modified silica using an atomizing device, stirring and mixing for 5 to 30 minutes, setting the rotation speed to 100 to 2000 rpm, and vacuuming to remove the ethanol solvent after sufficient mixing to obtain modified silica.
[0017] Further, the silane coupling agent is at least one of bis-[γ-(triethoxysilyl)propyl]tetrasulfide, bis-[γ-(triethoxysilyl)propyl]disulfide, γ-mercaptopropyltrimethoxysilane, γ-mercaptopropylethoxybis-(propyl-hexaethoxysiloxane), γ-mercaptopropyltriethoxysilane, γ-aminopropyltriethoxysilane, γ-methacryloxypropyltrimethoxysilane, and γ-glycidoxypropyltrimethoxysilane.
[0018] Furthermore, the antioxidant is at least one of antioxidant 1010, antioxidant 1076, antioxidant 264, antioxidant SP, antioxidant MB, antioxidant 168, antioxidant 445, antioxidant 405, and microcrystalline wax.
[0019] Furthermore, the plasticizer is at least one of naphthenic oil, epoxidized soybean oil, paraffin oil, coumarone resin, terpene resin, rosin resin, and petroleum resin.
[0020] Furthermore, the accelerator is at least one of accelerator M, accelerator DM, accelerator CZ, accelerator NOBS, accelerator TMTD, accelerator TBzTD, and accelerator D.
[0021] The present invention also provides a method for preparing a wear-resistant and anti-skid rubber composite material, which is used to prepare the wear-resistant and anti-skid rubber composite material, comprising the following steps:
[0022] S1. According to the formula of the rubber composite material, weigh the corresponding components, put the superpolymerized natural rubber, rare earth butadiene rubber and polar rubber into the internal mixer respectively, set the initial temperature of the internal mixer to 60-90°C, control the speed of the internal mixer to 50-100rpm, and mix for 1-5min;
[0023] S2, adding modified white carbon black, zinc oxide, stearic acid, antioxidant and plasticizer into an internal mixer twice, mixing for 2 to 5 minutes, and discharging the rubber when the temperature of the rubber reaches 120 to 150°C, discharging the rubber by an open mixer, and leaving the mixer for 24 hours to obtain a mixed rubber sheet;
[0024] S3, adding accelerator and sulfur to the mixed film by using an open mill, mixing evenly and then producing the film for standby use;
[0025] S4. Cut the corresponding size according to the outsole sample, hot-press and mold it on a flat vulcanizer to prepare the sample.
[0026] The advantages of the present invention are: based on the performance characteristics of different substrates, the synergistic advantages of super-polymerized natural rubber, rare earth butadiene rubber, and polar rubber are combined, and a simple and effective two-step silica modification method is proposed in terms of filler, and modified silica is obtained under the dual effects of chemical grafting modification and physical adsorption coating. The modified silica is evenly dispersed in the rubber matrix, and a stronger interface is formed with the rubber matrix, thereby improving the strength, wear resistance, and anti-skid performance of the rubber composite material. The processability of the rubber material is finally improved on the basis of controlling the cost of raw materials, and the obtained sole material not only has high wear resistance and anti-skid properties, but also has good resilience. DETAILED DESCRIPTION
[0027] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] The wear-resistant and non-slip rubber composite material of the present invention selects three main base materials as the main rubber base material: rare earth butadiene rubber with high cis structure, super-polymerized natural rubber, and polar rubber with cyano groups; the filler is low-cost and commonly used white carbon black is modified by combining chemical and physical modification to improve the dispersibility of white carbon black particles in the rubber matrix and enhance the compatibility of inorganic nanoparticles with the rubber matrix. The wear-resistant and non-slip rubber composite material also includes additives such as zinc oxide, stearic acid, antioxidant, plasticizer, accelerator, and sulfur.
[0029] In terms of mass fraction, the wear-resistant and anti-skid rubber composite material of the present invention comprises: 10-50 parts of superpolymerized natural rubber, 30-80 parts of rare earth butadiene rubber, 5-20 parts of polar rubber, 3-8 parts of zinc oxide, 0.5-3 parts of stearic acid, 10-90 parts of modified silica, 0.5-5 parts of antioxidant, 0.5-20 parts of plasticizer, 1-5 parts of accelerator, and 1-5 parts of sulfur; wherein the sum of the mass fractions of the superpolymerized natural rubber, the rare earth butadiene rubber, and the polar rubber is 100 parts.
[0030] Specifically, the rare earth cis-butadiene rubber has a cis structure content of >96%, a Mooney viscosity ML (1+4) of 40-80 at 100°C, and a molecular weight of 400,000-800,000. This rare earth cis-rubber has high regularity of molecular chain, can meet the high wear resistance and tear resistance required for the outsole of shoes, and has high elasticity and is easy to process.
[0031] Superpolymerized natural rubber is produced by low-shear low-temperature rapid drying technology. The characteristics of low-temperature direct drying retain the polymer structure of natural rubber. Non-rubber components such as proteins and phospholipids in rubber are more likely to form physical bonding points in the rubber system, which improves the compatibility and processability of superpolymerized natural rubber. Superpolymerized natural rubber has a hydrocarbon content of 97-99%, a non-rubber component content of 1-3%, a Mooney viscosity ML (1+4) of 40-90 at 100°C, and a molecular weight of 1.5-2.5 million. Superpolymerized natural rubber has tear resistance, aging resistance and elongation properties in the matrix.
[0032] The polar rubber is one or more of nitrile rubber, carboxyl nitrile, hydrogenated nitrile rubber, with an acrylonitrile content of 10-50%, a Mooney viscosity ML (1+4) of 30-100 at 100°C, and a molecular weight of 500,000-1,000,000; the polar rubber has the characteristics of high wear resistance, anti-slip and improved melt strength in the matrix. At the same time, it can form hydrogen bonds with white carbon black particles, acting as a compatible medium for fillers and non-polar rubbers.
[0033] By selecting the above-mentioned different rubber varieties to synergistically exert their respective advantages, while improving wear resistance and anti-slip properties, processability is guaranteed in terms of compatibility, elasticity and melt strength.
[0034] In terms of fillers, the modified silica is firstly chemically modified by an ethanol solution of a silane coupling agent, and then physically modified by an ethanol solution of at least one of polyethylene glycol, diethanolamine, triethanolamine, butanediamine, and tetramethylenetetramine. The specific modification methods include:
[0035] S1. Add the powder of white carbon black into a high-speed stirring mixer with electric heating and vacuuming functions, set the stirring speed of the mixer to 100-2000rpm, spray the ethanol dispersion of silane coupling agent with a concentration of 5-50wt% onto the white carbon black powder by using an atomizing device, and control the amount of coupling agent to be 2-15wt% of the mass of white carbon black; then vacuum the high-speed stirrer, turn on the heating, set the temperature to 100-150°C, the reaction time to 10-60min, release the pressure after stirring, and set the temperature to 30-70°C;
[0036] S2. Spraying an ethanol dispersion of at least one of polyethylene glycol, diethanolamine, triethanolamine, butanediamine and tetramethylenetetramine onto the chemically modified silica using an atomizing device, stirring and mixing for 5 to 30 minutes, setting the rotation speed to 100 to 2000 rpm, and vacuuming to remove the ethanol solvent after sufficient mixing to obtain modified silica.
[0037] This two-step modification method is relatively simple, using silane coupling agent to form chemical grafting with hydroxyl groups on the surface of silica, and then using solvents such as alcohols or amines to form hydrogen bonds with unreacted hydroxyl groups on the surface of silica to form physical coating, and obtain modified silica under the dual effects of chemical grafting modification and physical adsorption coating. The modified silica is evenly dispersed in the rubber matrix, and can be combined with polar rubber by hydrogen bonds, and can also form physical bonding points with non-rubber components of hyperpolymerized natural rubber. Therefore, a stronger interface is formed between the two-step modified silica and the rubber matrix of the present invention, further improving the strength, wear resistance and anti-slip performance of the rubber composite material.
[0038] Preferably, the silane coupling agent is at least one of bis-[γ-(triethoxysilyl)propyl]tetrasulfide, bis-[γ-(triethoxysilyl)propyl]disulfide, γ-mercaptopropyltrimethoxysilane, γ-mercaptopropylethoxybis-(propyl-hexaethoxysiloxane), γ-mercaptopropyltriethoxysilane, γ-aminopropyltriethoxysilane, γ-methacryloxypropyltrimethoxysilane and γ-glycidoxypropyltrimethoxysilane.
[0039] In terms of additives, the antioxidant is at least one of antioxidant 1010, antioxidant 1076, antioxidant 264, antioxidant SP, antioxidant MB, antioxidant 168, antioxidant 445, antioxidant 405, and microcrystalline wax; the plasticizer is at least one of cyclohexane oil, epoxidized soybean oil, paraffin oil, coumarone resin, terpene resin, rosin resin, and petroleum resin; the accelerator is at least one of accelerator M, accelerator DM, accelerator CZ, accelerator NOBS, accelerator TMTD, accelerator TBzTD, and accelerator D.
[0040] The present invention also provides a method for preparing the wear-resistant and anti-slip rubber composite material, the steps of which are as follows:
[0041] S1. According to the formula of the rubber composite material, weigh the corresponding components, put the superpolymerized natural rubber, rare earth butadiene rubber and polar rubber into the internal mixer respectively, set the initial temperature of the internal mixer to 60-90°C, control the speed of the internal mixer to 50-100rpm, and mix for 1-5min;
[0042] S2, adding modified white carbon black, zinc oxide, stearic acid, antioxidant and plasticizer into an internal mixer twice, mixing for 2 to 5 minutes, and discharging the rubber when the temperature of the rubber reaches 120 to 150°C, discharging the rubber by an open mixer, and leaving the mixer for 24 hours to obtain a mixed rubber sheet;
[0043] S3, adding accelerator and sulfur to the mixed film by using an open mill, mixing evenly and then producing the film for standby use;
[0044] S4. Cut the corresponding size according to the outsole sample, hot-press and mold it on a flat vulcanizer to prepare the sample.
[0045] The effects of the wear-resistant and anti-slip rubber composite material of the present invention are further illustrated by means of several groups of specific embodiments.
[0046] Example 1
[0047] The wear-resistant and anti-skid rubber composite material includes the following components by mass fraction: 30 parts of hyperpolymerized natural rubber, 60 parts of rare earth butadiene rubber, 10 parts of carboxyl nitrile rubber, 5 parts of zinc oxide, 1.5 parts of stearic acid, 40 parts of modified white carbon black, 10101 parts of antioxidant, 2 parts of antioxidant SP, 3 parts of cyclohexane oil, 3 parts of epoxidized soybean oil, 2 parts of accelerator DM, 0.4 parts of accelerator TMTD, and 1.8 parts of sulfur.
[0048] The modified silica modification method is as follows:
[0049] S1. Add the powder of silica to a high-speed stirring mixer with electric heating and vacuuming functions, set the stirring speed of the mixer to 200 rpm, spray the ethanol dispersion of bis-[γ-(triethoxysilyl)propyl]tetrasulfide with a concentration of 10 wt% onto the silica powder using an atomizer, and control the amount of the coupling agent to be 10 wt% of the mass of silica; then vacuum the high-speed stirrer, turn on the heating, set the temperature to 150° C., and the reaction time to 10 min. After the stirring is completed, release the pressure and set the temperature to 50° C.;
[0050] S2. Spray the ethanol dispersion of triethanolamine onto the chemically modified silica using an atomizer, stir and mix for 30 minutes, set the rotation speed to 2000 rpm, and after sufficient mixing, vacuumize to remove the ethanol solvent to obtain modified silica.
[0051] The preparation method of the wear-resistant and anti-skid rubber composite material comprises:
[0052] S1. According to the formula of the rubber composite material, weigh the corresponding components, put the superpolymerized natural rubber, rare earth cis-1,4-butadiene rubber and carboxyl nitrile rubber into an internal mixer respectively, set the initial temperature of the internal mixer to 90°C, control the speed of the internal mixer to 50rpm, and mix for 5min;
[0053] S2, adding modified white carbon black, zinc oxide, stearic acid, antioxidant 1010, antioxidant SP, cyclohexane oil, and epoxidized soybean oil into an internal mixer twice, mixing for 5 minutes, and discharging the rubber when the temperature of the rubber reaches 120°C, discharging the rubber by an open mixer, and keeping it aside for 24 hours to obtain a mixed rubber sheet;
[0054] S3, adding accelerator DM, accelerator TMTD and sulfur to the mixed film by using an open mixer, mixing evenly and then producing the film for standby use;
[0055] S4. Cut the corresponding size according to the outsole sample, hot-press and mold it on a flat vulcanizer to prepare the sample.
[0056] Comparative Example 1
[0057] The rubber composite material includes the following components by mass fraction: 30 parts of natural rubber cloud standard 1#, 60 parts of rare earth butadiene rubber, 10 parts of carboxyl nitrile rubber, 5 parts of zinc oxide, 1.5 parts of stearic acid, 40 parts of modified white carbon black, 1 part of antioxidant 1010, 2 parts of antioxidant SP, 3 parts of cyclohexane oil, 3 parts of epoxidized soybean oil, 2 parts of accelerator DM, 0.4 parts of accelerator TMTD, and 1.8 parts of sulfur.
[0058] The modification method of white carbon black is the same as that in Example 1.
[0059] The method for preparing the rubber composite material comprises:
[0060] S1. According to the formula of the rubber composite material, weigh the corresponding components, put the natural rubber Yunbiao 1#, rare earth butadiene rubber, and carboxyl nitrile rubber into the internal mixer respectively, set the initial temperature of the internal mixer to 90°C, control the speed of the internal mixer to 50rpm, and mix for 5min;
[0061] S2, adding modified white carbon black, zinc oxide, stearic acid, antioxidant 1010, antioxidant SP, cyclohexane oil, and epoxidized soybean oil into an internal mixer twice, mixing for 5 minutes, and discharging the rubber when the temperature of the rubber reaches 120°C, discharging the rubber by an open mixer, and keeping it aside for 24 hours to obtain a mixed rubber sheet;
[0062] S3, adding accelerator DM, accelerator TMTD and sulfur to the mixed film by using an open mixer, mixing evenly and then producing the film for standby use;
[0063] S4. Cut the corresponding size according to the outsole sample, hot-press and mold it on a flat vulcanizer to prepare the sample.
[0064] Comparative Example 2
[0065] The rubber composite material includes the following components by mass fraction: 30 parts of hyperpolymerized natural rubber, 60 parts of nickel-based butadiene rubber, 10 parts of carboxyl nitrile rubber, 5 parts of zinc oxide, 1.5 parts of stearic acid, 40 parts of modified silica, 1 part of antioxidant 1010, 2 parts of antioxidant SP, 3 parts of cyclohexane oil, 3 parts of epoxidized soybean oil, 2 parts of accelerator DM, 0.4 parts of accelerator TMTD, and 1.8 parts of sulfur.
[0066] The modification method of modified silica is the same as that in Example 1.
[0067] The method for preparing the rubber composite material comprises:
[0068] S1. According to the formula of the rubber composite material, weigh the corresponding components, put the superpolymerized natural rubber, nickel-based butadiene rubber, and carboxyl nitrile rubber into an internal mixer respectively, set the initial temperature of the internal mixer to 90°C, control the speed of the internal mixer to 50rpm, and mix for 5min;
[0069] S2, adding modified white carbon black, zinc oxide, stearic acid, antioxidant 1010, antioxidant SP, cyclohexane oil, and epoxidized soybean oil into an internal mixer twice, mixing for 5 minutes, and discharging the rubber when the temperature of the rubber reaches 120°C, discharging the rubber by an open mixer, and keeping it aside for 24 hours to obtain a mixed rubber sheet;
[0070] S3, adding accelerator DM, accelerator TMTD and sulfur to the mixed film by using an open mixer, mixing evenly and then producing the film for standby use;
[0071] S4. Cut the corresponding size according to the outsole sample, hot-press and mold it on a flat vulcanizer to prepare the sample.
[0072] Example 2
[0073] The wear-resistant and anti-skid rubber composite material includes the following components by mass fraction: 50 parts of hyperpolymerized natural rubber, 30 parts of rare earth butadiene rubber, 20 parts of nitrile rubber, 8 parts of zinc oxide, 3 parts of stearic acid, 85 parts of modified white carbon black, 1 part of antioxidant 1076, 4 parts of antioxidant 264, 10 parts of cyclohexane oil, 10 parts of epoxidized soybean oil, 3 parts of accelerator NOBS, 0.5 parts of accelerator TBzTD, and 1.5 parts of sulfur.
[0074] The modified silica modification method is as follows:
[0075] S1. Add the powder of silica to a high-speed stirring mixer with electric heating and vacuuming functions, set the stirring speed of the mixer to 2000 rpm, spray the ethanol dispersion of bis-[γ-(triethoxysilyl)propyl] disulfide with a concentration of 20wt% onto the silica powder using an atomizer, and control the amount of the coupling agent to be 15wt% of the mass of silica; then vacuum the high-speed stirrer, turn on the heating, set the temperature to 100°C, and the reaction time to 60min. After the stirring is completed, release the pressure and set the temperature to 70°C;
[0076] S2. Spray the ethanol dispersion of triethanolamine onto the chemically modified silica using an atomizer, stir and mix for 10 minutes, set the rotation speed to 500 rpm, and after sufficient mixing, vacuumize to remove the ethanol solvent to obtain modified silica.
[0077] The preparation method of the wear-resistant and anti-skid rubber composite material comprises:
[0078] S1. According to the formula of the rubber composite material, weigh the corresponding components, put the superpolymerized natural rubber, rare earth butadiene rubber and nitrile rubber into the internal mixer respectively, set the initial temperature of the internal mixer to 60°C, control the speed of the internal mixer to 100 rpm, and mix for 5 minutes;
[0079] S2, adding modified white carbon black, zinc oxide, stearic acid, antioxidant 1076, antioxidant 264, cyclohexane oil and epoxidized soybean oil into an internal mixer twice, mixing for 3 minutes, and removing the rubber when the temperature of the rubber reaches 130°C, using an open mixer to discharge the rubber, and leaving it for 24 hours to obtain a mixed rubber sheet;
[0080] S3, adding accelerator NOBS, accelerator TBzTD and sulfur to the mixed film by using an open mill, mixing evenly and then producing the film for standby use;
[0081] S4. Cut the corresponding size according to the outsole sample, hot-press and mold it on a flat vulcanizer to prepare the sample.
[0082] Comparative Example 3
[0083] The components included in the rubber composite material by mass fraction are the same as those in Example 2.
[0084] The modified silica modification method is as follows:
[0085] S1. Add the powder of silica to a high-speed stirring mixer with electric heating and vacuuming functions, set the stirring speed of the mixer to 2000 rpm, spray the ethanol dispersion of bis-[γ-(triethoxysilyl)propyl] disulfide with a concentration of 20wt% onto the silica powder using an atomizer, and control the amount of the coupling agent to be 15wt% of the mass of the silica; then vacuum the high-speed mixer to extract the ethanol;
[0086] S2. Spray the ethanol dispersion of triethanolamine onto the chemically modified silica using an atomizer, stir and mix for 10 minutes, set the rotation speed to 500 rpm, and after sufficient mixing, vacuumize to remove the ethanol solvent to obtain modified silica.
[0087] The preparation method of the rubber composite material is the same as that of Example 2.
[0088] Example 3
[0089] The wear-resistant and anti-skid rubber composite material includes the following components by mass fraction: 10 parts of hyperpolymerized natural rubber, 70 parts of rare earth butadiene rubber, 20 parts of hydrogenated nitrile rubber, 3.5 parts of zinc oxide, 1 part of stearic acid, 50 parts of modified white carbon black, 1680.5 parts of antioxidant, 3 parts of antioxidant MB, 0.5 parts of paraffin oil, 2 parts of coumarone resin, 2.5 parts of accelerator CZ, 2.5 parts of accelerator D, and 2.8 parts of sulfur.
[0090] The modified silica modification method is as follows:
[0091] S1. Add the powder of silica to a high-speed stirring mixer with electric heating and vacuuming functions, set the stirring speed of the mixer to 150 rpm, spray the ethanol dispersion of 50 wt% γ-mercaptopropylethoxybis-(propyl-hexaethoxysiloxane) onto the silica powder using an atomizing device, and control the amount of the coupling agent to be 10 wt% of the mass of silica; then vacuum the high-speed stirrer, turn on the heating, set the temperature to 120° C., and the reaction time to 15 min. After the stirring is completed, release the pressure and set the temperature to 60° C.;
[0092] S2. Spray the ethanol dispersion of dibutyl amine onto the chemically modified silica using an atomizer, stir and mix for 20 minutes, set the rotation speed to 1000 rpm, and after sufficient mixing, vacuumize to remove the ethanol solvent to obtain modified silica.
[0093] The preparation method of the wear-resistant and anti-skid rubber composite material comprises:
[0094] S1. According to the formula of the rubber composite material, weigh the corresponding components, put the superpolymerized natural rubber, rare earth butadiene rubber, and hydrogenated nitrile rubber into an internal mixer respectively, set the initial temperature of the internal mixer to 80°C, control the speed of the internal mixer to 60rpm, and mix for 5 minutes;
[0095] S2, adding modified white carbon black, zinc oxide, stearic acid, antioxidant 168, antioxidant MB, paraffin oil, and coumarone resin into an internal mixer twice, mixing for 10 minutes, and discharging the rubber when the temperature of the rubber reaches 150°C, discharging the rubber with an open mixer, and leaving the mixer for 24 hours to obtain a mixed rubber sheet;
[0096] S3, adding accelerator CZ, accelerator D and sulfur to the mixed film by an open mill, mixing evenly and then producing the film for standby use;
[0097] S4. Cut the corresponding size according to the outsole sample, hot-press and mold it on a flat vulcanizer to prepare the sample.
[0098] Comparative Example 4
[0099] The components included in the rubber composite material by mass fraction are the same as those in Example 3, wherein the modified silica modification method includes (only chemical modification): adding silica powder to a high-speed stirring mixer with electric heating and vacuuming functions, setting the stirring speed of the stirrer to 150 rpm, spraying an ethanol dispersion of 50 wt% γ-mercaptopropylethoxybis-(propyl-hexaethoxysiloxane) into the silica powder using an atomizer, and controlling the amount of the coupling agent to be 10 wt% of the mass of the silica; then evacuating the high-speed stirrer, turning on the heating, setting the temperature to 120°C, the reaction time to 15 min, releasing the pressure after stirring, and setting the temperature to 60°C; obtaining chemically modified silica.
[0100] The method for preparing the rubber composite material is the same as that in Example 3.
[0101] Comparative Example 5
[0102] The rubber composite material includes the following components in mass fraction as in Example 3, wherein the modified silica modification method includes (only physical modification is performed): adding silica powder to a high-speed stirring mixer with electric heating and vacuuming functions, spraying an ethanol dispersion of diaminobutane onto the chemically modified silica using an atomizing device, stirring and mixing for 20 minutes, setting the rotation speed to 1000 rpm, and after sufficient mixing, vacuuming to remove the ethanol solvent to obtain physically modified silica.
[0103] The preparation method of the rubber composite material is the same as that of Example 3.
[0104] Example 4
[0105] The wear-resistant and anti-skid rubber composite material includes the following components by mass fraction: 25 parts of hyperpolymerized natural rubber, 70 parts of rare earth butadiene rubber, 5 parts of hydrogenated nitrile rubber, 4 parts of zinc oxide, 1.5 parts of stearic acid, 10 parts of modified white carbon black, 3 parts of antioxidant 105, 2 parts of microcrystalline wax, 5 parts of epoxidized soybean oil, 5 parts of rosin resin, 0.5 parts of accelerator TMTD, 0.5 parts of accelerator TBzTD, and 5 parts of sulfur.
[0106] The modified silica modification method is as follows:
[0107] S1. Add the powder of silica to a high-speed stirring mixer with electric heating and vacuuming functions, set the stirring speed of the mixer to 1500 rpm, spray the ethanol dispersion of γ-mercaptopropyltriethoxysilane with a concentration of 30 wt% onto the silica powder using an atomizing device, and control the amount of the coupling agent to be 8 wt% of the mass of silica; then vacuum the high-speed stirrer, turn on the heating, set the temperature to 100°C, and the reaction time to 60 min. After the stirring is completed, release the pressure and set the temperature to 50°C;
[0108] S2. Spray the ethanol dispersion of tetramethylenetetramine onto the chemically modified silica using an atomizer, stir and mix for 30 minutes, set the rotation speed to 100 rpm, and after sufficient mixing, vacuumize to remove the ethanol solvent to obtain modified silica.
[0109] The preparation method of the wear-resistant and anti-skid rubber composite material comprises:
[0110] S1. According to the formula of the rubber composite material, weigh the corresponding components, put the superpolymerized natural rubber, rare earth cis-1,4-butadiene rubber and hydrogenated nitrile rubber into an internal mixer respectively, set the initial temperature of the internal mixer to 80°C, control the speed of the internal mixer to 80rpm, and mix for 2min;
[0111] S2, adding modified white carbon black, zinc oxide, stearic acid, antioxidant 105, microcrystalline wax, epoxidized soybean oil, and rosin resin into an internal mixer twice, mixing for 3 minutes, and removing the rubber when the temperature of the rubber reaches 130°C, using an open mixer to discharge the rubber, and leaving it for 24 hours to obtain a mixed rubber sheet;
[0112] S3, adding accelerator TMTD, accelerator TBzTD and sulfur to the mixed film by using an open mill, mixing evenly and then producing the film for standby use;
[0113] S4. Cut the corresponding size according to the outsole sample, hot-press and mold it on a flat vulcanizer to prepare the sample.
[0114] Example 5
[0115] The wear-resistant and anti-skid rubber composite material includes the following components by mass fraction: 40 parts of hyperpolymerized natural rubber, 40 parts of rare earth butadiene rubber, 20 parts of hydrogenated nitrile rubber, 4.5 parts of zinc oxide, 3 parts of stearic acid, 90 parts of modified white carbon black, 10100.5 parts of antioxidant, 5 parts of terpene resin, 3 parts of accelerator CZ, 0.5 parts of accelerator TBzTD, and 1 part of sulfur.
[0116] The modified silica modification method is as follows:
[0117] S1. Add the powder of silica to a high-speed stirring mixer with electric heating and vacuuming functions, set the stirring speed of the mixer to 200 rpm, spray the ethanol dispersion of γ-mercaptopropyltriethoxysilane with a concentration of 10 wt% onto the silica powder using an atomizing device, and control the amount of the coupling agent to be 2 wt% of the mass of silica; then vacuum the high-speed stirrer, turn on the heating, set the temperature to 110°C, and the reaction time to 60 min. After the stirring is completed, release the pressure and set the temperature to 30°C;
[0118] S2. Spray the ethanol dispersion of tetramethylenetetramine onto the chemically modified silica using an atomizer, stir and mix for 30 minutes, set the rotation speed to 500 rpm, and after sufficient mixing, vacuumize to remove the ethanol solvent to obtain modified silica.
[0119] The preparation method of the wear-resistant and anti-skid rubber composite material comprises:
[0120] S1. According to the formula of the rubber composite material, weigh the corresponding components, put the superpolymerized natural rubber, rare earth butadiene rubber and hydrogenated nitrile rubber into an internal mixer respectively, set the initial temperature of the internal mixer to 60°C, control the speed of the internal mixer to 100 rpm, and mix for 1 min;
[0121] S2, adding modified white carbon black, zinc oxide, stearic acid, antioxidant 1010, and terpene resin into an internal mixer twice, mixing for 4 minutes, and removing the rubber when the temperature of the rubber reaches 140°C, using an open mixer to discharge the rubber, and leaving it for 24 hours to obtain a mixed rubber sheet;
[0122] S3, adding accelerator CZ, accelerator TBzTD and sulfur to the mixed film by using an open mill, mixing evenly and then producing the film for standby use;
[0123] S4. Cut the corresponding size according to the outsole sample, hot-press and mold it on a flat vulcanizer to prepare the sample.
[0124] The properties of the wear-resistant and non-slip rubber composite materials of Examples 1-5 and Comparative Examples 1-5 are shown in the following table:
[0125] Table 1 Performance of various embodiments and comparative examples of wear-resistant and non-slip rubber composite materials
[0126]
[0127]
[0128] Note: Density test corresponds to GB / T 533-2008, resilience test corresponds to GB / T 2009, DIN abrasion test corresponds to GB / T 9867-2008, Akron abrasion test corresponds to GB / T 1689-2014, anti-slip performance test corresponds to GB / T3903.6-2017, hardness test corresponds to GB / T 533.1-2008, tensile strength and elongation at break test correspond to GB / T528-2009, tear strength test corresponds to GB / T 529-2009.
[0129] It can be concluded from the above examples and comparative examples that the strength, wear resistance, anti-slip properties and other properties of the rubber composite material are related to the type of rubber matrix, the dispersion of the silica reinforcing filler and the silica-rubber interface.
[0130] Compared with Comparative Examples 1 and 2, it can be seen that the types of natural rubber and cis-1,1-butadiene rubber affect the performance of the composite material. The superpolymerized natural rubber has more physical bonding points, so it has better compatibility and processability. The rare earth cis-1,1-butadiene rubber has better wear resistance, anti-slip properties and mechanical strength than nickel-based rare earth cis-1,1-butadiene rubber due to its high cis structure. At the same time, it has higher elasticity (good elongation characteristics), is easy to process, and gives the sole material a higher resilience.
[0131] By comparing Example 2 with Comparative Example 3, it can be seen that the modified silica provided in the present invention utilizes chemical and physical modification methods in sequence, which further improves the dispersibility of silica in the rubber matrix compared to the blending modification, strengthens the interface effect between silica and the rubber matrix, and improves the strength, wear resistance and anti-slip performance of the material.
[0132] Comparison between Example 3 and Comparative Examples 4 and 5 further verifies the technical advantage of the method combining chemical modification with physical modification. There are limitations to the performance improvement by relying solely on chemical modification or physical modification. The present invention relies on the chemical modification in the first step to first form chemical grafting, and then relies on the physical modification in the second step to form a hydrogen bond physical interaction with the hydroxyl groups on the surface of the silica that do not participate in the chemical grafting, thereby forming a physical coating effect, thereby improving the interface effect between the silica and the rubber matrix. The silica particles are evenly dispersed in the rubber matrix, which has a positive effect on improving the strength, wear resistance and anti-slip performance of the rubber material.
[0133] It should be noted that there are many testing standards for footwear. When the domestic and foreign standards used for some indicators are different, the test data of the same indicator will vary greatly. For example, for anti-slip testing, GB / T3903.6 whole shoe (sole) anti-slip test method, ASTMF 1677 hand-held elbow anti-slip test method, ASTMF 489-96James anti-slip test method, HG / T 3780-2005 footwear static anti-slip test method and other test methods have different test methods. The results of the test for different materials of the soles will be very different; generally speaking, the friction coefficient measured by GB / T3903.6 is relatively low among all test methods. When the friction coefficient of rubber is measured at about 0.12 according to GB / T3903.6, the corresponding ASTMF 1677 may be measured at about 0.6, and ASTMF 489-96James or HG / T 3780-2005 may be measured at about 0.75.
[0134] All tests of the present invention adopt GB / T series, which can comprehensively reflect the performance of various indicators of the sole.
[0135] The above is only a preferred embodiment of the present invention, and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment, it is not used to limit the present invention. Any technician familiar with this patent can make some changes or modify the technical contents suggested above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the solution of the present invention.
Claims
1. A wear-resistant and non-slip rubber composite material, characterized in that: The composition comprises, by mass fraction, 10-50 parts of superpolymerized natural rubber, 30-80 parts of rare earth butadiene rubber, 5-20 parts of polar rubber, 3-8 parts of zinc oxide, 0.5-3 parts of stearic acid, 10-90 parts of modified silica, 0.5-5 parts of antioxidant, 0.5-20 parts of plasticizer, 1-5 parts of accelerator and 1-5 parts of sulfur; the sum of the mass fractions of superpolymerized natural rubber, rare earth butadiene rubber and polar rubber is 100 parts; the modified silica is firstly chemically modified by an ethanol solution of a silane coupling agent, and then physically modified by an ethanol solution of at least one of polyethylene glycol, diethanolamine, triethanolamine, butanediamine and tetramethylenetetramine.
2. The wear-resistant and anti-slip rubber composite material according to claim 1, characterized in that: The polar rubber is one or more of nitrile rubber, carboxyl nitrile and hydrogenated nitrile rubber. The acrylonitrile content in the polar rubber is 10-50%, the Mooney viscosity ML (1+4) at 100° C. is 30-100, and the molecular weight is 500,000-1,000,000.
3. The wear-resistant and anti-slip rubber composite material according to claim 1, characterized in that: The cis structure content in rare earth butadiene rubber is >96%, the Mooney viscosity ML (1+4) at 100°C is 40-80, and the molecular weight is 400,000-800,000.
4. The wear-resistant and non-slip rubber composite material according to claim 1, characterized in that: The rubber hydrocarbon content in the hyperpolymerized natural rubber is 97-99%, the non-rubber component content is 1-3%, the Mooney viscosity ML (1+4) at 100°C is 40-90, and the molecular weight is 1.5 million to 2.5 million.
5. The wear-resistant and anti-slip rubber composite material according to claim 1, characterized in that: The specific modification method of modified silica includes the following steps: S1. Add the powder of white carbon black into a high-speed stirring mixer with electric heating and vacuuming functions, set the stirring speed of the mixer to 100-2000rpm, spray the ethanol dispersion of silane coupling agent with a concentration of 5-50wt% onto the white carbon black powder by using an atomizing device, and control the amount of coupling agent to be 2-15wt% of the mass of white carbon black; then vacuum the high-speed stirrer, turn on the heating, set the temperature to 100-150°C, the reaction time to 10-60min, release the pressure after stirring, and set the temperature to 30-70°C; S2. Spraying an ethanol dispersion of at least one of polyethylene glycol, diethanolamine, triethanolamine, butanediamine and tetramethylenetetramine onto the chemically modified silica using an atomizing device, stirring and mixing for 5 to 30 minutes, setting the rotation speed to 100 to 2000 rpm, and vacuuming to remove the ethanol solvent after sufficient mixing to obtain modified silica.
6. The wear-resistant and non-slip rubber composite material according to claim 1 or 5, characterized in that: The silane coupling agent is at least one of bis-[γ-(triethoxysilyl)propyl]tetrasulfide, bis-[γ-(triethoxysilyl)propyl]disulfide, γ-mercaptopropyltrimethoxysilane, γ-mercaptopropylethoxybis-(propyl-hexaethoxysiloxane), γ-mercaptopropyltriethoxysilane, γ-aminopropyltriethoxysilane, γ-methacryloxypropyltrimethoxysilane and γ-glycidoxypropyltrimethoxysilane.
7. The wear-resistant and anti-slip rubber composite material according to claim 1, characterized in that: The antioxidant is at least one of antioxidant 1010, antioxidant 1076, antioxidant 264, antioxidant SP, antioxidant MB, antioxidant 168, antioxidant 445, antioxidant 405, and microcrystalline wax.
8. The wear-resistant and non-slip rubber composite material according to claim 1, characterized in that: The plasticizer is at least one of naphthenic oil, epoxidized soybean oil, paraffin oil, coumarone resin, terpene resin, rosin resin and petroleum resin.
9. The wear-resistant and non-slip rubber composite material according to claim 1, characterized in that: The accelerator is at least one of accelerator M, accelerator DM, accelerator CZ, accelerator NOBS, accelerator TMTD, accelerator TBzTD, and accelerator D.
10. A method for preparing a wear-resistant and non-slip rubber composite material, characterized in that: The method for preparing the wear-resistant and non-slip rubber composite material according to any one of claims 1 to 9 comprises the following steps: S1. According to the formula of the rubber composite material, weigh the corresponding components, put the superpolymerized natural rubber, rare earth butadiene rubber and polar rubber into the internal mixer respectively, set the initial temperature of the internal mixer to 60-90°C, control the speed of the internal mixer to 50-100rpm, and mix for 1-5min; S2, adding modified white carbon black, zinc oxide, stearic acid, antioxidant and plasticizer into an internal mixer twice, mixing for 2 to 5 minutes, and discharging the rubber when the temperature of the rubber reaches 120 to 150°C, discharging the rubber by an open mixer, and leaving the mixer for 24 hours to obtain a mixed rubber sheet; S3, adding accelerator and sulfur to the mixed film by using an open mill, mixing evenly and then producing the film for standby use; S4. Cut the corresponding size according to the outsole sample, hot-press and mold it on a flat vulcanizer to prepare the sample.
Citation Information
Cited By
Preparation method of rubber outsole with extremely wear resistance and high wet skid resistance
CN116535749A
Anti-skid and wear-resistant light conveying belt and preparation method thereof
CN120441896A
Polyurethane resin, polyurethane synthetic leather and preparation method and application thereof
CN121319323A
High-strength rope based on polyester fiber composite material and manufacturing method thereof
CN121760093A