Low-temperature thermal decomposition resin emulsion and preparation method thereof

By preparing polypropylene carbonate resin emulsion, the challenges posed by high-temperature thermal decomposition materials to matrix materials and processing technology have been solved, achieving a combination of low-temperature thermal decomposition and environmentally friendly treatment, thus expanding the application possibilities of the material.

CN118956135APending Publication Date: 2024-11-15CHONGQING POLYCOMP INT
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411306606.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The use of existing thermally decomposable materials at high temperatures poses challenges to the matrix materials and processing technology, and traditional materials are difficult to meet the requirements of low-temperature thermal decomposition.

Method used

A low-temperature thermal decomposition resin emulsion composed of polypropylene carbonate resin, polypropylene carbonate polyol, sodium 3-carboxybenzenesulfonate, and nonionic emulsifier is prepared by melt blending, shear emulsification, and vacuum distillation, optimizing the raw material formulation to achieve low-temperature thermal decomposition.

Benefits of technology

A resin emulsion with excellent low-temperature thermal decomposition performance was prepared, which reduced the thermal decomposition temperature, improved the stability and biodegradability of the emulsion, and reduced the environmental treatment cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005049665060000011
    Figure BDA0005049665060000011
  • Figure BDA0005049665060000031
    Figure BDA0005049665060000031
  • Figure BDA0005049665060000041
    Figure BDA0005049665060000041
Patent Text Reader

Abstract

The invention belongs to the field of chemical materials, and particularly relates to a low-temperature thermal decomposition resin emulsion and a preparation method thereof. The low-temperature thermal decomposition resin emulsion provided by the invention is prepared from the following raw materials in parts by weight: 30 to 50 parts of polypropylene carbonate, 1 to 15 parts of polypropylene carbonate polyol, 0.1 to 5 parts of sodium 3-carboxybenzenesulfonate, 0.5 to 8 parts of an emulsifier, 0 to 20 parts of a cosolvent and 50 to 70 parts of water. According to the invention, the raw material formula of the resin emulsion is optimally designed, so that the resin emulsion with excellent low-temperature thermal decomposition performance is obtained, and the resin emulsion is biodegradable and low in environment-friendly treatment cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of chemical materials, and in particular relates to a low-temperature thermal decomposition resin emulsion and a preparation method thereof. Background Art

[0002] In many fields such as special glass fiber material coating, ceramic parts, chips, electronic circuit boards, electronic and electrical components, etc., under certain process conditions, it is necessary to coat the base material with polymers for protection, support, bonding, etc., in order to meet the process requirements of product production, processing, and molding. Then, under specific conditions, the polymers are removed under heating conditions. Therefore, there is an urgent need for high-performance low-temperature thermal decomposition emulsion materials.

[0003] At present, traditional thermal decomposition materials used in the above-mentioned fields include methyl cellulose, ethyl cellulose, polyvinyl alcohol (butyral), acrylic resin, styrene resin, vinyl acetate, etc. The degumming temperature is greater than 400-500°C or the burn-out temperature is greater than 900-1300°C. Excessively high temperatures pose severe challenges to the base material and subsequent processing technology. Summary of the invention

[0004] In view of this, the object of the present invention is to provide a low-temperature thermal decomposition resin emulsion and a preparation method thereof. The resin emulsion provided by the present invention has excellent low-temperature thermal decomposition performance and is environmentally friendly and degradable.

[0005] The present invention provides a low-temperature thermal decomposition resin emulsion, and the preparation raw materials include, by weight:

[0006]

[0007] Preferably, the number average molecular weight of the polypropylene carbonate is 10,000 to 40,000.

[0008] Preferably, the number average molecular weight of the polypropylene carbonate polyol is 2000-6000.

[0009] Preferably, the emulsifier is a nonionic emulsifier and / or an anionic emulsifier.

[0010] Preferably, the emulsifier is one or more of ethylene oxide propylene oxide block polyethers, alkyl alcohol ethers, alkyl alcohol block polyethers, alkylphenol polyoxyethylene ethers, alkyl alcohol polyoxyethylene ethers, aromatic polyethers, alkyl alcohol ether sulfates, alkyl alcohol ether phosphates and alkyl alcohol ether carboxylates.

[0011] Preferably, the co-solvent is one or more of acetone, butanone, ethyl acetate and benzene.

[0012] The present invention provides a method for preparing the low-temperature thermal decomposition resin emulsion described in the above technical solution, comprising the following steps:

[0013] a) melt-blending polypropylene carbonate resin, polypropylene carbonate polyol and sodium 3-carboxybenzenesulfonate to react to obtain a graft mixture;

[0014] b) The grafted mixture, emulsifier, cosolvent and water are mixed and sheared to obtain a low-temperature thermal decomposition resin emulsion.

[0015] Preferably, in step a), the temperature of the melt blending is 160-260° C.; and the time of the melt blending is 2-5 hours.

[0016] Preferably, in step b), the temperature of the shear emulsification is 150-200° C.; the pressure of the shear emulsification is 0.3-1.8 MPa; and the time of the shear emulsification is 0.5-2 h.

[0017] Preferably, the method further comprises: c) performing reduced pressure distillation on the low-temperature thermal decomposition resin emulsion to recover the co-solvent therein.

[0018] Compared with the prior art, the present invention provides a low-temperature thermal decomposition resin emulsion and a preparation method thereof. In terms of weight, the raw materials for preparing the low-temperature thermal decomposition resin emulsion provided by the present invention include: 30 to 50 parts of polypropylene carbonate, 1 to 15 parts of polypropylene carbonate polyol, 0.1 to 5 parts of sodium 3-carboxybenzenesulfonate, 0.5 to 8 parts of emulsifier, 0 to 20 parts of cosolvent, and 50 to 70 parts of water. The present invention optimizes the raw material formula of the resin emulsion to obtain a resin emulsion with excellent low-temperature thermal decomposition performance, and the resin emulsion is biodegradable and has low environmental protection treatment cost. DETAILED DESCRIPTION

[0019] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0020] The present invention provides a low-temperature thermal decomposition resin emulsion, and the preparation raw materials include, by weight:

[0021]

[0022] In the resin emulsion provided by the present invention, among the raw materials for preparation, the polypropylene carbonate is white, light yellow particles or powder prepared by catalytic polymerization of carbon dioxide and propylene oxide as raw materials, and the number average molecular weight is preferably 10000-40000, specifically 10000, 15000, 20000, 25000, 30000, 35000 or 40000, wherein the thermal degradation temperature is lower at a lower molecular weight, and the film-forming strength of the emulsion is improved at a higher molecular weight, and it can be flexibly selected according to application requirements.

[0023] In the resin emulsion provided by the present invention, the content of the polypropylene carbonate in the preparation raw materials can specifically be 30 parts by weight, 31 parts by weight, 32 parts by weight, 33 parts by weight, 34 parts by weight, 35 parts by weight, 36 parts by weight, 37 parts by weight, 38 parts by weight, 39 parts by weight, 40 parts by weight, 41 parts by weight, 42 parts by weight, 43 parts by weight, 44 parts by weight, 45 parts by weight, 46 parts by weight, 47 parts by weight, 48 parts by weight, 49 parts by weight or 50 parts by weight.

[0024] In the resin emulsion provided by the present invention, among the raw materials for preparation, the polypropylene carbonate polyol is a colorless, transparent or slightly yellow liquid prepared by catalytic polymerization of carbon dioxide and propylene oxide as raw materials, and the number average molecular weight is preferably 2000-6000, specifically 2000, 2500, 3000, 3500, 4000, 4500, 5000, 5500 or 6000.

[0025] In the resin emulsion provided by the present invention, the content of the polypropylene carbonate polyol in the preparation raw materials can specifically be 1 weight part, 2 weight parts, 3 weight parts, 4 weight parts, 5 weight parts, 6 weight parts, 7 weight parts, 8 weight parts, 9 weight parts, 10 weight parts, 11 weight parts, 12 weight parts, 13 weight parts, 14 weight parts or 15 weight parts.

[0026] In the resin emulsion provided by the present invention, in the preparation raw materials, the molecular structure of the sodium 3-carboxybenzenesulfonate is as follows:

[0027]

[0028] In the resin emulsion provided by the present invention, the content of sodium 3-carboxybenzenesulfonate in the preparation raw materials can be specifically 0.1 weight parts, 0.3 weight parts, 0.5 weight parts, 0.7 weight parts, 1 weight parts, 1.2 weight parts, 1.5 weight parts, 1.7 weight parts, 2 weight parts, 2.3 weight parts, 2.5 weight parts, 2.7 weight parts, 3 weight parts, 3.2 weight parts, 3.5 weight parts, 3.7 weight parts, 4 weight parts, 4.2 weight parts, 4.5 weight parts, 4.7 weight parts or 5 weight parts.

[0029] In the resin emulsion provided by the present invention, in the preparation raw materials, the emulsifier is preferably a nonionic emulsifier and / or an anionic emulsifier, and more preferably one or more of ethylene oxide propylene oxide block polyether, alkyl alcohol ether, alkyl alcohol block polyether, alkylphenol polyoxyethylene ether, alkyl alcohol polyoxyethylene ether, aryl-containing polyether, alkyl alcohol ether sulfate, alkyl alcohol ether phosphate and alkyl alcohol ether carboxylate; wherein, the brand of the ethylene oxide propylene oxide block polyether is preferably one or more of P105, F68 and P108; the alkyl alcohol polyoxyethylene ether is preferably isomeric fatty alcohol polyoxyethylene ether, and its brand is preferably 3400. In the specific embodiment provided by the present invention, the emulsifier is preferably ethylene oxide propylene oxide block polyether and isomeric fatty alcohol polyoxyethylene ether, and the mass ratio of the ethylene oxide propylene oxide block polyether to the isomeric fatty alcohol polyoxyethylene ether is preferably 3: (0.5-5), and more preferably 3: (1-2).

[0030] In the resin emulsion provided by the present invention, the content of the emulsifier in the preparation raw materials can specifically be 0.5 weight parts, 1 weight parts, 1.5 weight parts, 2 weight parts, 2.5 weight parts, 3 weight parts, 3.5 weight parts, 4 weight parts, 4.5 weight parts, 5 weight parts, 5.5 weight parts, 6 weight parts, 6.5 weight parts, 7 weight parts, 7.5 weight parts or 8 weight parts.

[0031] In the resin emulsion provided by the present invention, in the preparation raw materials, the co-solvent is preferably one or more of acetone, butanone, ethyl acetate and benzene. Among them, acetone is the most preferred, followed by butanone, and then ethyl acetate.

[0032] In the resin emulsion provided by the present invention, the content of the co-solvent in the preparation raw materials can specifically be 0, 1 weight part, 2 weight parts, 3 weight parts, 4 weight parts, 5 weight parts, 6 weight parts, 7 weight parts, 8 weight parts, 9 weight parts, 10 weight parts, 11 weight parts, 12 weight parts, 13 weight parts, 14 weight parts, 15 weight parts, 16 weight parts, 17 weight parts, 18 weight parts, 19 weight parts or 20 weight parts.

[0033] In the resin emulsion provided by the present invention, in the preparation raw materials, the water is preferably deionized water; the content of the water in the preparation raw materials can specifically be 50 parts by weight, 51 parts by weight, 52 parts by weight, 53 parts by weight, 54 parts by weight, 55 parts by weight, 56 parts by weight, 57 parts by weight, 58 parts by weight, 59 parts by weight, 60 parts by weight, 61 parts by weight, 62 parts by weight, 63 parts by weight, 64 parts by weight, 65 parts by weight, 66 parts by weight, 67 parts by weight, 68 parts by weight, 69 parts by weight or 70 parts by weight.

[0034] The present invention also provides a method for preparing the low-temperature thermal decomposition resin emulsion described in the above technical solution, comprising the following steps:

[0035] a) melt-blending polypropylene carbonate resin, polypropylene carbonate polyol and sodium 3-carboxybenzenesulfonate to react to obtain a graft mixture;

[0036] b) The grafted mixture, emulsifier, cosolvent and water are mixed and sheared to obtain a low-temperature thermal decomposition resin emulsion.

[0037] In the preparation method provided by the present invention, in step a), liquid polypropylene carbonate polyol is introduced to reduce the resin melt viscosity and mixing temperature on the one hand, and to increase the terminal hydroxyl content of the resin system on the other hand, which is conducive to the esterification reaction between the terminal hydroxyl group and the carboxyl group in sodium 3-carboxybenzenesulfonate, thereby grafting the hydrophilic group of sodium sulfonate with a hydrophilic function.

[0038] In the preparation method provided by the present invention, in step a), the melt blending is preferably carried out under nitrogen protection; the temperature of the melt blending is preferably 160-260°C, specifically 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, 220°C, 230°C, 240°C, 250°C or 260°C; the time of the melt blending is preferably 2-5h, specifically 2h, 2.5h, 3h, 3.5h, 4h, 4.5h or 5h.

[0039] In the preparation method provided by the present invention, in step b), the introduction of an emulsifier can further reduce the viscosity of the resin system, so that the polypropylene carbonate resin can maintain a fluid state even at a temperature above 80° C., which is beneficial to reducing the emulsification temperature of the polypropylene carbonate resin, solving the problems of foaming and demulsification during the emulsification process, and ensuring the emulsification effect; the introduction of a co-solvent is beneficial to ensuring the emulsification effect, and can significantly improve the stability of the final emulsion product.

[0040] In the preparation method provided by the present invention, in step b), the temperature of the shear emulsification is preferably 150-200°C, specifically 150°C, 155°C, 160°C, 165°C, 170°C, 175°C, 180°C, 185°C, 190°C, 195°C or 200°C; the pressure of the shear emulsification is preferably 0.3-1.8MPa, specifically 0.3MPa, 0.4MPa, 0.5MPa, 0.6MPa, 0.7MPa, 0.8MPa , 0.9MPa, 1MPa, 1.1MPa, 1.2MPa, 1.3MPa, 1.4MPa, 1.5MPa, 1.6MPa, 1.7MPa or 1.8MPa; the shear emulsification time is preferably 0.5-2h, specifically 0.5h, 0.6h, 0.7h, 0.8h, 0.9h, 1h, 1.1h, 1.2h, 1.3h, 1.4h, 1.5h, 1.6h, 1.7h, 1.8h, 1.9h or 2h.

[0041] In the preparation method provided by the present invention, it is preferred to further include: c) subjecting the low-temperature thermal decomposition resin emulsion to reduced pressure distillation to recover the co-solvent therein.

[0042] In the preparation method provided by the present invention, in a specific embodiment, the preparation method of the low-temperature thermal decomposition resin emulsion more specifically comprises the following steps:

[0043] (1) Stirring and heating polypropylene carbonate resin (granules or powder) and polypropylene carbonate polyol (liquid) to 160-260° C. under nitrogen protection until they are in a molten state, adding sodium 3-carboxybenzenesulfonate to the molten state for a certain period of time, wherein the terminal hydroxyl groups in the resin react with the carboxyl groups of the sodium 3-carboxybenzenesulfonate to form grafts, thereby obtaining a grafted mixture;

[0044] (2) maintaining the fluidity of the grafted mixture obtained in step (1) and adding a certain amount of emulsifier before cooling, and further stirring and mixing to make it uniform;

[0045] (3) Keep stirring and cool down to below 100° C., then add a certain amount of cosolvent and water to the resin mixture obtained in step (2), seal and pressurize and heat to 150-200° C., while gradually increasing the shear stirring rate and keeping the temperature for 0.5-2 hours to complete emulsification;

[0046] (4) recovering the co-solvent in the emulsion by vacuum distillation, and cooling and discharging the material to obtain a resin emulsion without the co-solvent.

[0047] In the above specific preparation steps provided by the present invention, in step (1), the time for adding sodium 3-carboxybenzenesulfonate and mixing thoroughly is 2 to 5 hours.

[0048] In the above specific preparation steps provided by the present invention, in step (2), the grafted mixture has a certain fluidity above 160° C. because polypropylene carbonate polyol with a relatively lower molecular weight is added, and the temperature is kept above 160° C. and the fluidity is maintained, and a certain amount of emulsifier is added before cooling, and the mixture is further stirred and mixed evenly. At this time, due to the addition of an emulsifier with a relatively lower molecular weight, the temperature at which the system maintains fluidity can be further reduced.

[0049] In the above-mentioned specific preparation steps provided by the present invention, in step (3), the co-solvent and water can also be pressurized. That is, after the resin mixture obtained in step (2) is cooled to 150-200°C, the co-solvent and water can be added into the closed high-pressure reactor by high-pressure feeding, thereby eliminating the cooling and heating process, but the equipment requirements are higher.

[0050] In the above specific preparation steps provided by the present invention, in step (4), it is preferred to use a reduced pressure distillation method to recover the co-solvent in the mixed liquid, and the mixed liquid is subjected to reduced pressure distillation at 40 to 70° C. to recover the co-solvent. In addition, the present invention can also use other reasonable recovery methods for recovery, and in some embodiments, the co-solvent may not be recovered.

[0051] The technical solution provided by the present invention optimizes the raw material formula of the resin emulsion to obtain a resin emulsion with excellent low-temperature thermal decomposition performance, and the resin emulsion is biodegradable and has low environmental protection treatment cost. More specifically, the technical solution of the present invention has the following advantages:

[0052] 1. The main resin raw materials used in the present invention are polypropylene carbonate resin and polypropylene carbonate polyol, which are prepared by catalytic polymerization of carbon dioxide and propylene oxide. The raw materials can fully utilize a large amount of CO 2 resources and can reduce CO in the atmosphere 2 emissions, improve environmental quality, and help mitigate the greenhouse effect.

[0053] 2. The present invention introduces liquid polypropylene carbonate polyol, which reduces the melt viscosity and mixing temperature of the resin on the one hand, and increases the terminal hydroxyl content of the resin system on the other hand, which is beneficial to the esterification reaction between the terminal hydroxyl group and the carboxyl group in sodium 3-carboxybenzenesulfonate, thereby grafting the hydrophilic group of sodium sulfonate with a hydrophilic function, effectively improving the stability of the emulsion.

[0054] 3. The present invention preferably introduces a nonionic emulsifier in a molten state, which can further reduce the viscosity of the resin system, so that the polypropylene carbonate resin can maintain a fluid state at a relatively low temperature, which is beneficial to reduce the emulsification temperature of the polypropylene carbonate resin, solves the problems of foaming and demulsification during the emulsification process, and ensures the emulsification effect.

[0055] 4. The present invention preferably adopts a grafting combined with pressurized emulsification method to prepare the emulsion, which significantly reduces the use of co-solvents in the preparation process. This method is used for the first time to prepare a stable emulsion for polypropylene carbonate, and can emulsify PPC resins of different molecular weights, greatly expanding the possibility of using PPC resin as an emulsion.

[0056] 5. The emulsion product prepared by the present invention has excellent emulsion shear stability and storage stability, and has great application potential when used as a glass fiber film-forming agent.

[0057] For the purpose of greater clarity, the invention is described in detail through the following embodiments.

[0058] Example 1

[0059] Step (1): 50 parts by weight of a polypropylene carbonate resin (particles) with a number average molecular weight of 10,000 and 5 parts by weight of a polypropylene carbonate polyol (liquid) with a number average molecular weight of 6,000 are stirred and heated to 150-160° C. under nitrogen protection until they are molten, 0.5 parts by weight of sodium 3-carboxybenzenesulfonate are added to the mixture while maintaining the molten state, and the mixture is stirred and mixed thoroughly, and the mixture is kept warm and stirred for 2 hours to obtain a grafted mixture.

[0060] Step (2): The grafted mixture was kept at a temperature above 160° C. and maintained fluidity, and 5 parts by weight of ethylene oxide propylene oxide block polyether emulsifier P105 (BASF) was added before cooling, and further stirred and mixed thoroughly.

[0061] Step (3): the mixture obtained above is cooled to 50°C, and then 5 parts by weight of the auxiliary solvent acetone and 50 parts by weight of deionized water are added, and then the mixture is heated, pressurized and stirred in a sealed manner, and the temperature is set at 150-160°C for shear stirring for 1 hour to complete pressurized emulsification, and the pressure is 0.4-0.6 MPa, and then the temperature is reduced and the pressure is released.

[0062] Step (4): Recover the co-solvent in the mixed liquid by vacuum distillation. After the mixed liquid is subjected to vacuum distillation at 50° C. to recover the co-solvent, the mixture is cooled and discharged to obtain a low-temperature thermal decomposition aliphatic polycarbonate emulsion.

[0063] Example 2

[0064] Step (1): 40 parts by weight of a polypropylene carbonate resin (particles) with a number average molecular weight of 20,000 and 10 parts by weight of a polypropylene carbonate polyol (liquid) with a number average molecular weight of 4,000 are stirred and heated to 170-180° C. under nitrogen protection until they are molten, 2 parts by weight of sodium 3-carboxybenzenesulfonate are added to the mixture while maintaining the molten state, and the mixture is stirred and mixed thoroughly, and the mixture is kept warm and stirred for 3 hours to obtain a grafted mixture.

[0065] Step (2): The grafted mixture is kept at a temperature above 180° C. and fluidity is maintained. Before cooling, 3 parts by weight of ethylene oxide propylene oxide block polyether emulsifier F68 (BASF) and 2 parts by weight of isomeric fatty alcohol polyoxyethylene ether 3400 (Solvay) are added, and the mixture is further stirred and mixed thoroughly.

[0066] Step (3): The mixture obtained above is cooled to 70°C, and then 10 parts by weight of the auxiliary solvent acetone and 60 parts by weight of deionized water are added, and then the mixture is heated, pressurized and stirred in a sealed manner, and the temperature is set at 170-180°C for 2 hours to complete pressurized emulsification at 0.8-1.0 MPa, and then the temperature is reduced and the pressure is released.

[0067] Step (4): Recover the co-solvent in the mixed liquid by vacuum distillation. After the mixed liquid is subjected to vacuum distillation at 50° C. to recover the co-solvent, the mixture is cooled and discharged to obtain a low-temperature thermal decomposition aliphatic polycarbonate emulsion.

[0068] Example 3

[0069] Step (1): 30 parts by weight of a polypropylene carbonate resin (particles) with a number average molecular weight of 40,000 and 15 parts by weight of a polypropylene carbonate polyol (liquid) with a number average molecular weight of 2,000 are stirred and heated to 190-200° C. under nitrogen protection until they are molten, 3 parts by weight of sodium 3-carboxybenzenesulfonate are added to the mixture while maintaining the molten state, and the mixture is stirred and mixed thoroughly, and the mixture is kept warm and stirred for 4 hours to obtain a grafted mixture.

[0070] Step (2): The grafted mixture is kept at a temperature above 180° C. and fluidity is maintained, and before cooling, 6 parts by weight of ethylene oxide propylene oxide block polyether emulsifier P108 (BASF) and 2 parts by weight of isomeric fatty alcohol polyoxyethylene ether 3400 (Solvay) are added, and further stirred and mixed thoroughly.

[0071] Step (3): The mixture obtained above is cooled to 80°C, and then 10 parts by weight of the auxiliary solvent ethyl acetate and 70 parts by weight of deionized water are added, and then the mixture is heated, pressurized and stirred in a sealed manner, and the temperature is set at 180-190°C for shear stirring for 2 hours to complete pressurized emulsification at 1.0-1.3 MPa, and then the temperature is reduced and the pressure is released.

[0072] Step (4): Recover the co-solvent in the mixed liquid by vacuum distillation. After the mixed liquid is subjected to vacuum distillation at 70° C. to recover the co-solvent, the mixture is cooled and discharged to obtain a low-temperature thermal decomposition aliphatic polycarbonate emulsion.

[0073] Performance Testing

[0074] The emulsion products prepared in Examples 1 to 3 were tested, and the results are shown in Table 1:

[0075] Table 1 Product performance indicators

[0076]

[0077] In Table 1, the preparation method of the emulsion film is: the emulsion is dried at 120°C for 2 hours to prepare the resin film; the test method of the decomposition temperature of the emulsion film is: using thermogravimetric analysis (TGA) to test, that is, under program-controlled temperature, the mass of the sample is measured as the temperature and time change to determine the thermal decomposition temperature, the test conditions are nitrogen atmosphere, temperature range 25 ~ 800°C, heating rate 10°C / min, the initial decomposition temperature is judged as the initial weight loss greater than 5% / min, and the final decomposition temperature is judged as the final weight loss less than 2% / min.

[0078] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A low-temperature thermal decomposition resin emulsion, characterized in that: In parts by weight, the raw materials for preparation include:

2. The low-temperature thermal decomposition resin emulsion according to claim 1, characterized in that The number average molecular weight of the polypropylene carbonate is 10,000 to 40,000.

3. The low-temperature thermal decomposition resin emulsion according to claim 1, characterized in that The number average molecular weight of the polypropylene carbonate polyol is 2000-6000.

4. The low-temperature thermal decomposition resin emulsion according to claim 1, characterized in that The emulsifier is a nonionic emulsifier and / or an anionic emulsifier.

5. The low-temperature thermal decomposition resin emulsion according to claim 4, characterized in that: The emulsifier is one or more of ethylene oxide and propylene oxide block polyethers, alkyl alcohol ethers, alkyl alcohol block polyethers, alkylphenol polyoxyethylene ethers, alkyl alcohol polyoxyethylene ethers, aromatic polyethers, alkyl alcohol ether sulfates, alkyl alcohol ether phosphates and alkyl alcohol ether carboxylates.

6. The low-temperature thermal decomposition resin emulsion according to claim 1, characterized in that The co-solvent is one or more of acetone, butanone, ethyl acetate and benzene.

7. A method for preparing a low-temperature thermally decomposable resin emulsion according to any one of claims 1 to 6, characterized in that: The following steps are involved: a) melt-blending polypropylene carbonate resin, polypropylene carbonate polyol and sodium 3-carboxybenzenesulfonate to react to obtain a graft mixture; b) The grafted mixture, emulsifier, cosolvent and water are mixed and sheared to obtain a low-temperature thermal decomposition resin emulsion.

8. The preparation method according to claim 7, characterized in that: In step a), the temperature of the melt blending is 160 to 260° C.; and the time of the melt blending is 2 to 5 hours.

9. The preparation method according to claim 7, characterized in that: In step b), the temperature of the shear emulsification is 150-200° C.; the pressure of the shear emulsification is 0.3-1.8 MPa; and the time of the shear emulsification is 0.5-2 h.

10. The preparation method according to claim 7, characterized in that: Also includes: c) subjecting the low-temperature thermal decomposition resin emulsion to reduced pressure distillation to recover the co-solvent therein.