Modified polyacrylonitrile copolymer adhesive as well as preparation method and application thereof

By modifying polyacrylonitrile copolymer adhesive, combining flexible acrylates and functional reaction monomers, the problem of PVDF is solved in the environment and the adhesion and softness of the positive electrode material of lithium-ion battery is improved. It realizes environmentally friendly and sustainable high-performance battery adhesive replacement.

CN118956302AActive Publication Date: 2024-11-15BLUE OCEAN & BLACK STONE TECH CO LTD (FUJIAN)

Patent Information

Application Number
CN202411137389.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-15
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

Existing lithium-ion battery positive electrode adhesives mainly use polyvinylidene fluoride (PVDF), which is difficult to degrade in the environment and has high cost, and has a potential threat to the environment and human health. At the same time, the high glass of polyacrylonitrile The transformation temperature results in insufficient flexibility and cannot meet the process requirements of high-performance batteries.

Method used

Using modified polyacrylonitrile copolymer adhesive, the polymerization of flexible acrylate monomers and functional reaction monomers is introduced to prepare the adhesive with good adhesion and softness, reducing the glass transition temperature, suitable for Lithium-ion battery cathode material, replacing traditional PVDF adhesive.

Benefits of technology

Achieve environmentally friendly and sustainable adhesive replacement, reduce costs, improve the stability and softness of the battery positive electrode material, meet industrial production and application needs, and surpass the adhesion and softness performance of traditional PVDF adhesives .

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of battery adhesives, and discloses a modified polyacrylonitrile copolymer adhesive, which is prepared from the following raw materials in parts by weight: 40 to 60 parts of acrylonitrile, 30 to 45 parts of flexible acrylate monomer, 10 to 30 parts of functional reaction monomer, 0.2 to 0.5 part of surfactant and 0.1 to 0.15 part of initiator. The weight of the acrylonitrile is not less than 40% of the total mass of the acrylonitrile, the flexible acrylate monomer and the functional reaction monomer. The adhesive with good adhesive force and high softness can be prepared, and has a good prospect in the application of a battery positive electrode.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of battery adhesives, and in particular to a modified polyacrylonitrile copolymer adhesive and a preparation method and application thereof. Background Art

[0002] Lithium-ion batteries are widely used in portable electronic devices, electric vehicles and energy storage systems due to their high energy density, long cycle life and low self-discharge rate. In the manufacturing process of lithium-ion batteries, the choice of binder for electrode materials has an important influence on the performance and life of the battery. The binder not only improves the mechanical strength of the electrode, but also ensures good contact between the active material and the current collector, ensuring the electrochemical performance of the battery during the charge and discharge process.

[0003] At present, the positive electrode binder of lithium-ion batteries mainly adopts polyvinylidene fluoride (PVDF). Although PVDF itself has good chemical stability, its persistence in the environment may lead to the problem of difficult degradation. PVDF is a fluorine-containing material with a high price. If proper protective measures are not taken during the use and handling of PVDF, it may release harmful fluorides, posing a potential threat to the environment and human health. Although PVDF does not directly belong to perfluorinated and polyfluoroalkyl substances (PFAS), as a fluorinated polymer, its application and treatment are still affected by PFAS-related policies. The EU's strict restrictions and phase-out policies on PFAS reflect its cautious attitude towards the overall use of fluorinated materials. This has prompted the industry to look for more environmentally friendly and sustainable alternative materials or improve the use and treatment methods of existing materials to meet increasingly stringent environmental standards.

[0004] Polyacrylonitrile (PAN) is a polymer material with excellent mechanical properties, chemical stability and heat resistance, but the hardness of the pole pieces prepared from it is relatively high and cannot meet production needs. PAN is a highly polar polymer with good affinity with electrolytes and electrochemical stability. Using PAN to replace polyvinylidene fluoride (PVDF) can increase the polarity of electrode active materials and reduce material costs. However, the glass transition temperature of PAN homopolymer (Tg≈85°C) is high and its flexibility is insufficient at room temperature, which cannot fully meet the process requirements for preparing high-performance batteries. Therefore, modifying polyacrylonitrile copolymers to prepare adhesives suitable for batteries remains a research focus that needs to be urgently addressed. Summary of the invention

[0005] In the first aspect, the present application provides a modified polyacrylonitrile copolymer adhesive. In the technical solution of the present application, based on acrylonitrile, flexible acrylic ester monomers and functional monomers are introduced. The functional monomers have specific functional groups. The three undergo polymerization reaction under the action of an initiator. The obtained copolymer can be applied to lithium-ion battery positive electrode adhesives, and the softness, adhesion and dispersion properties of the obtained adhesive can meet the requirements. In addition, the present invention realizes a high-cost replacement for PVDF by selecting raw materials such as acrylic esters and acrylonitrile, reduces the cost of adhesives, and is suitable for industrial production and application.

[0006] This application adopts the following technical solutions: A modified polyacrylonitrile copolymer adhesive comprises raw materials including 40-60 parts of acrylonitrile, 30-45 parts of flexible acrylic ester monomers, 10-30 parts of functional reaction monomers, 0.2-0.5 parts of surfactants and 0.1-0.15 parts of initiators by weight, wherein the weight of the acrylonitrile is not less than 40% of the total weight of the acrylonitrile, the flexible acrylic ester monomers and the functional reaction monomers, and the functional groups of the functional reaction monomers include one or more of hydroxyl, amide, sulfonate, ether and morpholine.

[0007] By adopting the above technical scheme, in this scheme, acrylonitrile, flexible acrylic ester monomers and functional reaction monomers are copolymerized, and the amount of acrylonitrile is controlled to obtain a modified acrylonitrile copolymer. The adhesive prepared on the basis of acrylonitrile has good adhesion and oil solubility, and by introducing flexible monomers, the softness and dispersion performance of the obtained adhesive can be adjusted, thereby improving the performance of the adhesive; and the functional reaction monomer has a specific functional group, which can also further improve the adhesion and dispersion performance of the adhesive.

[0008] Optionally, the acrylic monomer includes one or more of ethyl acrylate, propyl acrylate, butyl acrylate, hexyl acrylate, octyl acrylate, 2-ethylhexyl acrylate, isobutyl acrylate, isooctyl acrylate and lauryl acrylate.

[0009] By adopting the above technical solution, the above-mentioned flexible acrylic monomer is polymerized with acrylonitrile, so that the glass transition temperature of the copolymer can be lower than -50°C, so that the binder is in a highly elastic state at room temperature and exhibits softness, which is conducive to its application in positive electrode materials.

[0010] Optionally, the functional monomer is selected from a mixture of ethylene glycol methyl ether acrylate, acrylamide and acryloylmorpholine.

[0011] By adopting the above technical solution, the monomers are selected from the synergistic effect of the above different functional groups, and the obtained adhesive has better adhesion, which makes the positive electrode material have better stability when applied to the positive electrode material.

[0012] Optionally, the flexible acrylic monomer is selected from a mixture of isooctyl acrylate, butyl acrylate and ethyl acrylate.

[0013] By adopting the above technical solution, the prepared polymer has better softness, which is beneficial to the application of positive electrode materials.

[0014] Optionally, the initiator is selected from one or a combination of more than one of benzoyl peroxide, sodium p-toluene sulfite, tert-butyl hydroperoxide, N,N-dihydroxypropyl p-toluidine, ethylenediamine, azobisisobutyronitrile, sodium persulfate, ammonium persulfate, and sodium bisulfite.

[0015] By adopting the above technical solution, the above initiators can further initiate the polymerization reaction of the monomers, thereby preparing the modified polyacrylonitrile copolymer in the present application.

[0016] Optionally, the surfactant is selected from one of alkylbenzene sulfonate, sodium alkyl sulfate, and alkyl ether surfactants, or a combination of several thereof.

[0017] In a second aspect, the present application provides a method for preparing the modified polyacrylonitrile copolymer adhesive in the above scheme.

[0018] A method for preparing a modified polyacrylonitrile copolymer adhesive comprises the following steps: (1) dividing acrylonitrile into two parts, adding a surfactant, the first part of acrylonitrile, a flexible acrylate monomer and a functional reaction monomer into water and passing nitrogen to deoxygenate, mixing the raw materials uniformly, and then raising the temperature to a first temperature; (2) the initiator is divided into three parts, the first part of the initiator is dissolved in water, and then added dropwise to the solution obtained in step (1) to carry out a heat preservation reaction; then the second part of the initiator is dissolved in water and the second part of acrylonitrile is added to the above reaction solution, and the temperature is raised to the second temperature and a heat preservation reaction is carried out; then the third part of the initiator is added to the above reaction solution and the temperature is kept for reaction; (3) after the reaction is completed, the temperature is lowered and the material is discharged to obtain a modified polyacrylonitrile copolymer.

[0019] By adopting the above technical scheme, after distributed reaction, and after heating and heat preservation, the modified polyacrylonitrile copolymer in this scheme can be prepared, which is applied to the adhesive of battery positive electrode material and has good adhesion and softness.

[0020] Optionally, the first temperature is 60-75°C, and the second temperature is 70-80°C.

[0021] In a third aspect, the present application provides an application of the modified polyacrylonitrile copolymer adhesive of the above scheme, wherein the modified polyacrylonitrile copolymer adhesive is used for mixing with an active material and a conductive agent and then applied to a positive electrode plate of a lithium-ion battery.

[0022] In summary, the present application includes at least one of the following beneficial effects: 1. In the technical solution of the present application, acrylonitrile copolymer is used as the main body of the adhesive, which has good adhesion, and flexible acrylic esters are introduced into the copolymer, which gives the copolymer a lower glass transition temperature while maintaining the adhesion of the acrylonitrile copolymer, so that the adhesive is in a highly elastic state at room temperature, showing softness, which is beneficial to the stability of the battery positive electrode material. In addition, the functional reaction monomer has a specific functional group, which can improve the adhesive adhesion while also improving the dispersion performance of the adhesive. DETAILED DESCRIPTION

[0023] The performance of the battery depends largely on the electrode, and optimizing the battery structure is conducive to promoting the development of high-performance batteries. The positive electrode of the battery is composed of active materials, binders and conductive agents. The role of the binder is to use the active material and the conductive agent to be tightly combined and fixed on the current collector.

[0024] At present, the positive electrode adhesive of lithium-ion batteries mainly uses polyvinylidene fluoride (PVDF), but with the increasing requirements of environmental protection and other issues, it has become a trend to replace traditional polyvinylidene fluoride (PVDF) with adhesives such as polyacrylonitrile. However, for adhesives, sufficient adhesion is required while also requiring good softness. Although polyacrylonitrile has good adhesion to active materials and current collectors, it is below the glass transition temperature at room temperature and has high crystallinity. Therefore, the pole piece prepared using polyacrylonitrile as an adhesive has the problem of poor flexibility.

[0025] In order to solve the above technical problems, the first aspect of the present invention provides a modified polyacrylonitrile copolymer adhesive, which is prepared from raw materials including 40-60 parts of acrylonitrile, 30-45 parts of flexible acrylic ester monomers, 10-30 parts of functional reaction monomers, 0.2-0.5 parts of surfactants and 0.1-0.15 parts of initiators, by weight, the weight of the acrylonitrile is not less than 40% of the total mass of the acrylonitrile, the flexible acrylic ester monomers and the functional reaction monomers, and the functional groups of the functional reaction monomers include one or more of hydroxyl, amide, sulfonate, ether and morpholine.

[0026] Functional reaction monomers are monomers that can be copolymerized with acrylonitrile monomers, such as a mixture of one or more selected from ethylene glycol methyl ether acrylate, acrylamide, sodium allyl sulfonate, acryloyl morpholine, and 2-hydroxyethyl acrylate. Under the action of these functional groups, the emulsification effect is improved to a certain extent, the copolymerization effect of the oil-soluble monomer is improved, and the polymer itself can be given better adhesion.

[0027] In the technical solution of the present application, flexible acrylic acid esters and functional reaction monomers are introduced on the basis of acrylonitrile monomer, which can maintain the good adhesion of acrylonitrile while giving the copolymer a lower glass transition temperature. The glass transition temperature of the obtained copolymer is lower than -50°C, so that the adhesive is in a highly elastic state at room temperature, showing softness, which is beneficial to the stability of the use of the battery positive electrode material. In addition, the content of acrylonitrile monomer is not less than 40%, so that the modified polyacrylonitrile copolymer can be well dissolved in N-methylpyrrolidone solvent for application in the application of battery positive electrode sheets.

[0028] The initiator of the present application is selected from one or more of benzoyl peroxide, sodium p-toluene sulfite, tert-butyl hydroperoxide, N,N-dihydroxypropyl p-toluidine, ethylenediamine, azobisisobutyronitrile, sodium persulfate, ammonium persulfate, sodium bisulfite, as long as it can initiate the polymerization reaction. The amount of the initiator is 0.1-0.15 parts, that is, 0.1, 0.12, 0.13, 0.15, etc. can be selected.

[0029] The surfactant in the present application is selected from one or a combination of alkylbenzene sulfonate, sodium alkyl sulfate, and alkyl ether surfactants, which can promote more uniform distribution of the monomer in water, such as sodium dodecyl sulfate, etc. The proportion of the surfactant is 0.2-0.5 parts, that is, 0.2, 0.3, 0.35, 0.4, 0.5, etc. can be selected.

[0030] Example 1 In 800 parts of water, add 0.2 parts of sodium dodecyl sulfate, then add 40 parts of acrylonitrile, 30 parts of butyl acrylate, 30 parts of butyl acrylate, 10 parts of ethylene glycol methyl ether acrylate and 10 parts of acrylamide, pass nitrogen to deoxygenate, stir and mix evenly, and raise the temperature of the reactor to 60-75°C.

[0031] Add 0.08 parts of ammonium persulfate to 40 parts of water and stir to mix evenly, add initiator solution dropwise to the above liquid, complete the addition within 1-2 hours, keep warm and react for 2-3 hours after the addition is completed, then add 0.02 parts of ammonium persulfate (dissolved in 10 parts of water) and 10 parts of acrylonitrile, heat to 70-80°C and keep warm for 2-4 hours, then add 0.02 parts of ammonium persulfate, keep warm at 70-80°C for 1 hour, then cool and stop the reaction, and discharge the material when the temperature in the autoclave drops below 40°C to obtain a modified polyacrylonitrile copolymer.

[0032] Example 2 In 800 parts of water, add 0.2 parts of sodium dodecyl sulfate, then add 40 parts of acrylonitrile, 30 parts of butyl acrylate, 10 parts of sodium allyl sulfonate and 10 parts of acryloylmorpholine, pass nitrogen to deoxygenate, stir and mix evenly, and raise the temperature of the reactor to 60-75°C.

[0033] Add 0.08 parts of sodium persulfate into 40 parts of water and stir to mix evenly, add initiator solution dropwise into the above liquid, complete the addition within 1-2 hours, keep warm and react for 2-3 hours after the addition is completed, then add 0.02 parts of ammonium persulfate (dissolved in 10 parts of water) and 10 parts of acrylonitrile, heat to 70-80°C and keep warm for 2-4 hours, then add 0.02 parts of ammonium persulfate, keep warm at 70-80°C for 1 hour, then cool and stop the reaction, and discharge the material when the temperature in the kettle drops below 40°C.

[0034] Example 3 In 800 parts of water, add 0.2 parts of sodium dodecyl sulfate, then add 40 parts of acrylonitrile, 25 parts of isooctyl acrylate, 5 parts of ethylene glycol methyl ether acrylate, and 10 parts of acrylamide, pass nitrogen to deoxygenate, stir and mix evenly, and raise the temperature of the reactor to 60-75°C.

[0035] Add 0.08 parts of ammonium persulfate to 40 parts of water and stir to mix evenly, add initiator solution dropwise to the above liquid, complete the addition within 1-2 hours, keep warm and react for 2-3 hours after the addition is completed, then add 0.02 parts of ammonium persulfate (dissolved in 10 parts of water) and 20 parts of acrylonitrile, heat to 70-80℃ and keep warm for 2-4 hours, then add 0.02 parts of ammonium persulfate, keep warm at 70-80℃ for 1h, then cool and stop the reaction, and discharge the material when the temperature in the kettle drops below 40℃.

[0036] Example 4 In 800 parts of water, add 0.2 parts of sodium dodecyl sulfate, then add 30 parts of acrylonitrile, 35 parts of isooctyl acrylate, 10 parts of sodium allyl sulfonate, and 15 parts of 2-hydroxyethyl acrylate, pass nitrogen to deoxygenate, stir and mix evenly, and raise the temperature of the reactor to 60-75°C.

[0037] Add 0.08 parts of sodium persulfate into 40 parts of water and stir to mix evenly, add initiator solution dropwise into the above liquid, complete the addition within 1-2 hours, keep warm and react for 2-3 hours after the addition is completed, then add 0.02 parts of ammonium persulfate (dissolved in 10 parts of water) and 10 parts of acrylonitrile, heat to 70-80°C and keep warm for 2-4 hours, then add 0.02 parts of ammonium persulfate, keep warm at 70-80°C for 1 hour, then cool and stop the reaction, and discharge the material when the temperature in the kettle drops below 40°C.

[0038] Example 5 In 800 parts of water, add 0.2 parts of sodium dodecyl sulfate, then add 30 parts of acrylonitrile, 15 parts of isooctyl acrylate, 15 parts of butyl acrylate, 10 parts of ethyl acrylate, 5 parts of ethylene glycol methyl ether acrylate, 10 parts of acrylamide, and 5 parts of acryloylmorpholine; deoxygenate with nitrogen, stir and mix evenly, and raise the temperature of the reactor to 60-75°C.

[0039] Add 0.1 parts of sodium persulfate into 40 parts of water and stir to mix evenly, add initiator solution dropwise into the above liquid, complete the addition within 1-2 hours, keep warm and react for 2-3 hours after the addition is completed, then add 0.02 parts of ammonium persulfate (dissolved in 10 parts of water) and 10 parts of acrylonitrile, heat to 70-80℃ and keep warm for 2-4 hours, then add 0.02 parts of ammonium persulfate, keep warm at 70-80℃ for 1 hour, then cool and stop the reaction, and discharge the material when the temperature in the kettle drops below 40℃.

[0040] Comparative Example 1 The difference between this comparative example and Example 3 is that equal amounts of isooctyl acrylate are used to replace ethylene glycol methyl ether acrylate and acrylamide, and the rest of the preparation processes are the same.

[0041] Comparative Example 2 The difference between this comparative example and Example 3 is that an equal amount of acrylonitrile is used to replace isooctyl acrylate, and the rest of the preparation processes are the same.

[0042] Application Example The modified polyacrylonitrile copolymer adhesive prepared in the embodiment of the present application is used for lithium ion battery positive electrode after being mixed with active materials and conductive agents, and the amount of the adhesive used accounts for 1-2% of the total mass of the adhesive, conductive agent and active materials.

[0043] Performance Testing Adhesion test: positive electrode lithium manganese oxide slurry was prepared. By weight, the modified polyacrylonitrile copolymer adhesive obtained in this application accounted for 1.3 parts, the oily CNT slurry accounted for 1.0 parts, and the positive electrode lithium manganese oxide material accounted for 97.7 parts. The slurry was prepared using NMP (N-methylpyrrolidone). The slurry was coated on aluminum foil (thickness 18μm) using a flat coater, and the coating surface density was 2g / cm 2; Use an electric roller machine to roll the pole piece, compacting 2.85g / cm 3 The adhesion of the obtained electrodes was tested respectively (unit: N / m) according to the masking tape sticking and peeling method.

[0044] Softness: The electrode is prepared according to the above method, and the softness of the electrode is tested using a softness tester (unit: mN); the smaller the value obtained by the test, the better the softness.

[0045] The test values ​​of Examples 1-5, Comparative Examples 1-2 and commercial PVDF products are shown in the following table: Adhesion(N / m) Softness(mN) Example 1 7.3 790 Example 2 6.3 871 Example 3 8.1 849 Example 4 8 645 Example 5 8.3 665 Comparative Example 1 5.8 620 Comparative Example 2 6.8 990 PVDF products on the market 6.9 537 In the scheme of the present application, by comparing Example 3 with Comparative Example 1, it can be seen that the adhesion of the adhesive can be improved under the action of the functional reaction monomer, and by comparing Example 3 with Comparative Example 2, it can be seen that the acrylic monomer can improve the good softness of the adhesive. The market requirements for battery positive electrode adhesives are generally adhesion ≥ 6N / m and softness ≤ 800mN. In the embodiments of the present application, especially Examples 4 and 5, not only the market requirements are met, but also the adhesion and softness have surpassed PVDF. Therefore, the modified polyacrylonitrile copolymer adhesive obtained in the present application has a good prospect for replacing PVDF for battery positive electrode adhesives.

[0046] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. A modified polyacrylonitrile copolymer adhesive, characterized in that: The raw materials include 40-60 parts of acrylonitrile, 30-45 parts of flexible acrylic ester monomers, 10-30 parts of functional reaction monomers, 0.2-0.5 parts of surfactants and 0.1-0.15 parts of initiators by weight. The weight of the acrylonitrile is not less than 40% of the total weight of the acrylonitrile, the flexible acrylic ester monomers and the functional reaction monomers. The functional groups of the functional reaction monomers include one or more of hydroxyl, amide, sulfonate, ether and morpholine.

2. A modified polyacrylonitrile copolymer adhesive according to claim 1, characterized in that: The acrylic monomers include one or more of ethyl acrylate, propyl acrylate, butyl acrylate, hexyl acrylate, octyl acrylate, 2-ethylhexyl acrylate, isobutyl acrylate, isooctyl acrylate and lauryl acrylate.

3. The modified polyacrylonitrile copolymer adhesive according to claim 1, characterized in that: The functional reaction monomer is selected from a mixture of ethylene glycol methyl ether acrylate, acrylamide and acryloyl morpholine.

4. A modified polyacrylonitrile copolymer adhesive according to claim 2, characterized in that: The flexible acrylic monomer is selected from a mixture of isooctyl acrylate, butyl acrylate and ethyl acrylate.

5. The modified polyacrylonitrile copolymer adhesive according to claim 1, characterized in that: The initiator is selected from one or a combination of benzoyl peroxide, sodium p-toluene sulfite, tert-butyl hydroperoxide, N,N-dihydroxypropyl p-toluidine, ethylenediamine, azobisisobutyronitrile, sodium persulfate, ammonium persulfate, and sodium bisulfite.

6. The modified polyacrylonitrile copolymer adhesive according to claim 1, characterized in that: The surfactant is selected from one or a combination of alkylbenzene sulfonate, sodium alkyl sulfate, and alkyl ether surfactants.

7. A method for preparing a modified polyacrylonitrile copolymer adhesive according to any one of claims 1 to 6, characterized in that: The following steps are included (1) acrylonitrile is divided into two parts, a surfactant, the first part of acrylonitrile, a flexible acrylate monomer and a functional reaction monomer are added into water and nitrogen is passed through to deoxygenate the water, the raw materials are mixed evenly, and then the temperature is raised to a first temperature; (2) the initiator is divided into three parts, the first part of the initiator is dissolved in water, and then added dropwise to the solution obtained in step (1) to carry out a heat-insulating reaction; then the second part of the initiator is dissolved in water and the second part of acrylonitrile is added to the above reaction solution, and the temperature is raised to the second temperature and the temperature is kept for reaction; then the third part of the initiator is added to the above reaction solution and the temperature is kept for reaction; (3) After the reaction is completed, the temperature is lowered and the material is discharged to obtain a modified polyacrylonitrile copolymer.

8. The method for preparing a modified polyacrylonitrile copolymer adhesive according to claim 7, characterized in that: The first temperature is 60-75°C, and the second temperature is 70-80°C.

9. An application of the modified polyacrylonitrile copolymer adhesive according to any one of claims 1 to 6, characterized in that: The modified polyacrylonitrile copolymer adhesive is used for applying to a positive electrode plate of a lithium ion battery after being mixed with an active material and a conductive agent.

Citation Information

Patent Citations

  • Acrylonitrile copolymer adhesive and application thereof in lithium ion batteries

    CN106220779A

  • Water-based composite binder for battery electrode, preparation method of water-based composite binder and battery electrode

    CN114204022A

  • Anode fluoride-free binder material as well as preparation method and application thereof

    CN117777904A

  • Heteroatom-rich adhesive as well as preparation method and application thereof

    CN118085772A

  • Adhesive sheet for battery and lithium ion battery

    JP2020074308A

Cited By

  • High-viscosity high-stripping-degree acrylonitrile resin as well as preparation method and application thereof