Green and environment-friendly preparation method of calcium sulfonate

By using additives such as oleic amide and polymethyl methacrylate in the calcium sulfonate preparation process to replace traditional carcinogenic solvents, the problem of excessive use of carcinogenic solvents and chlorophenol in the preparation of calcium sulfonate is solved, and high temperature is achieved The improvement of cleanliness, wear resistance and coagulation reduction performance has promoted the green development of chemical industry.

CN118956466APending Publication Date: 2024-11-15XINXIANG RICHFUL LUBE ADDITIVE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411193347.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

There are problems in the existing calcium sulfonate preparation process that use too much carcinogenic solvents and contain chlorine and phenols, and compatibility problems are prone to occur during the compounding process, which is costly and poorly effective.

Method used

Using oleic acid amides to replace calcium chloride and alkyl phenols and other additives, reduce the use of carcinogenic solvents by controlling reaction conditions and ventilation parameters, improve micelle stability and alkalinity, and combine small molecule carboxylic acid and polymethyl methacrylic acid. Ester, calcium sulfonate free of chlorine and phenol is prepared, with high temperature purity, wear resistance and coagulation reduction properties.

Benefits of technology

It has achieved green and environmentally friendly preparation of calcium sulfonate, reduced the use of carcinogenic solvents, improved the anti-wear and coagulation performance of the product, and conformed to the green development concept of chemical industry, stable physical and chemical indicators of the product, excellent oil solubility and colloid stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118956466A_ABST
    Figure CN118956466A_ABST
Patent Text Reader

Abstract

The invention discloses a green and environment-friendly preparation method of calcium sulfonate, which comprises the following steps: adding solvent oil, a main accelerant, base oil and sulfonic acid into a reaction flask, and uniformly stirring; controlling the temperature of the reaction liquid to be 50-90 DEG C under the condition of condensation reflux, starting to carry out neutralization reaction timing after adding inorganic calcium, and adding an auxiliary accelerant A after 10-60 minutes so as to continuously react for 5-30 minutes; the method comprises the following steps: controlling the temperature at 50-85 DEG C under a condensation reflux condition, adding inorganic calcium, water and a promoter B at a first ventilation node, and starting to introduce CO2; when the gas is introduced to a second node, supplementing inorganic calcium, water and an auxiliary accelerant B; when ventilation is conducted to a third node, inorganic calcium and water are supplemented till ventilation is finished; removing alcohol and water in the reaction liquid, and filtering or centrifuging to remove solid residues; and distilling under reduced pressure to obtain a finished product. The product prepared by the invention is small in residue amount, good in oil solubility and colloid stability, and excellent in high-temperature detergency, wear resistance and pour point depressing property, and conforms to the concept of green development.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lubricating oil additives, and in particular to a green and environmentally friendly preparation method of calcium sulfonate. Background Art

[0002] When the equipment is operated under extreme conditions such as high temperature and high pressure, the insoluble matter of lubricating oil oxidation is not conducive to the normal operation of the engine, and the acidic substances corrode the engine surface. The acid neutralization, washing, dispersing and solubilizing effects of calcium sulfonate can better solve such problems, achieving the purpose of slowing down the decline of oil products and keeping the engine clean.

[0003] The overbasing reaction of calcium sulfonate includes neutralization and carbonation. The neutralization reaction is mainly the process of sulfonic acid reacting with inorganic calcium to form neutral calcium sulfonate; the carbonation reaction is the process of inorganic calcium generating nano-scale calcium carbonate (also containing a small amount of calcium hydroxide, etc.) particles and being wrapped by neutral calcium sulfonate to form a stable colloid. The main problem to be overcome in the synthesis of calcium sulfonate is to select suitable additives to promote the stable occurrence of the reaction. Common additives include ammonia, alkylphenols, small molecule carboxylic acids, fatty acids, calcium chloride or surfactants.

[0004] Application No. CN201611207154.3 discloses a method for preparing a super-high base synthetic magnesium sulfonate, using small molecule organic acid, saturated fatty acid, and low-carbon alcohol as an auxiliary system to obtain a magnesium sulfonate with no skinning, low precipitation value, and low turbidity. Application No. CN201711327170.0 discloses a method for preparing a super-high base synthetic alkylbenzene calcium sulfonate, using alcohols, dodecylphenol or sulfide alkylphenol calcium, amine substances, calcium chloride, and acid substances as an auxiliary system to obtain a calcium sulfonate with a calcium content of about 22%. Application No. CN102295971A discloses a high base heavy alkylbenzene calcium sulfonate detergent and a preparation method thereof, using low-carbon alcohol, calcium chloride, ethylenediamine, ammonia water, etc. as an auxiliary system to prepare a high base, low viscosity, and clear and stable calcium sulfonate. Application No. CN201210390215.X discloses a synthetic alkylbenzene calcium sulfonate type lubricating oil detergent and a production process, using methanol and sulfur-bridged alkylphenol calcium as auxiliary agents to produce calcium sulfonate with a TBN of 20 to 300 mgKOH / g. Application No. US07188517 discloses a method for preparing high-base calcium sulfonate, using ethylenediamine as an auxiliary agent, which improves the utilization rate of raw materials and reduces solid waste.

[0005] The defects of the existing preparation process of calcium sulfonate are:

[0006] 1. The calcium sulfonate prepared by the existing process contains chlorine and phenol, which is not conducive to the normal operation of equipment, the healthy growth of animals and plants, and the long-term coexistence of humans and nature.

[0007] 2. Xylene and toluene, which are widely used in the existing calcium sulfonate synthesis process, are listed as Class III carcinogens by the International Agency for Research on Cancer (IARC).

[0008] 3. In the existing lubricant single agent compounding process, different single agents are directly mixed at the same time, which is prone to compatibility problems, high costs and poor benefits.

[0009] According to statistics, the energy consumed by friction and wear accounts for about 23% of the world's total energy, and mechanical failures account for about 80%; the use of anti-friction materials is an important material to maintain the efficient and long-life operation of mechanical systems. In recent years, some cutting-edge research has increasingly valued the application of oleamide lubricants. Methacrylates have a good effect on improving the low-temperature flow properties of diesel engine oils, etc. In the future, the research and development of calcium sulfonates at home and abroad will develop in the direction of chlorine-free, phenol-free and reduced use of harmful solvents. The new synthesis process of calcium alkylbenzene sulfonate should significantly reduce the use of carcinogenic solvents, organically combine detergents, friction reducers and pour point depressants, and the product does not contain chlorine and phenol, and has good high-temperature detergency, anti-wear and pour point depressant properties, promoting the sustainable development of green chemical industry. Summary of the invention

[0010] In view of the deficiencies in the prior art, the present invention provides a green and environmentally friendly preparation method of calcium sulfonate, which avoids excessive use of carcinogenic solvents, replaces additives such as calcium chloride and alkylphenol with oleic acid amide and the like, increases the stability and alkalinity of micelles, solves the problems of calcium sulfonate containing chlorine and phenol, and improves the anti-wear and de-condensation properties of calcium sulfonate; the prepared calcium sulfonate has low slag amount, good oil solubility and colloid stability, and excellent high-temperature cleaning performance, anti-wear performance and de-condensation performance, which is in line with the concept of green development of chemical industry.

[0011] The invention discloses a green and environmentally friendly preparation method of calcium sulfonate, comprising:

[0012] Step 1, add solvent oil, primary accelerator, base oil and sulfonic acid into a reaction bottle and stir evenly;

[0013] Step 2: Under condensation reflux conditions, the reaction liquid temperature is controlled at 50-90° C., and after adding inorganic calcium, the neutralization reaction timing is started. After 10-60 minutes, the co-promoter A is added and the reaction is continued for 5-30 minutes;

[0014] Step 3, under the condition of condensation reflux, control the temperature at 50-85°C, add inorganic calcium, water and booster B at the first ventilation node and start to introduce CO2; when ventilation reaches the second node, add inorganic calcium, water and booster B; when ventilation reaches the third node, add inorganic calcium and water until the ventilation ends;

[0015] Step 4: raising the temperature to 90-130° C. under a vacuum pressure of 0-0.05 MPa to remove alcohol and water from the reaction solution, and removing solid residue by filtering or centrifugation;

[0016] Step 5: subject the centrifuged sample or the filtered sample to vacuum distillation at 0 to -0.1 MPa and 150 to 250° C. to obtain a finished product.

[0017] As a further improvement of the present invention, in step 1, by weight, there are 70 to 200 parts of solvent oil, 10 to 50 parts of primary accelerator, 50 to 150 parts of base oil, and 10 to 100 parts of sulfonic acid.

[0018] As a further improvement of the present invention, in step 1,

[0019] The solvent oil includes at least one of alkanes and alkanols;

[0020] The primary accelerator includes at least one of a monohydric alcohol and a polyhydric alcohol;

[0021] The base oil comprises at least one of 100N, 150SN, 150N, 150SN, 150BS, 500N and 500SN;

[0022] The sulfonic acid includes at least one of long-chain alkylbenzene sulfonic acid, heavy alkylbenzene sulfonic acid and petroleum sulfonic acid.

[0023] As a further improvement of the present invention, the solvent oil is undecane and / or n-nonanol, the main accelerator is methanol, the base oil is 150N, the sulfonic acid is long-chain alkylbenzene sulfonic acid and heavy alkylbenzene sulfonic acid, and the weight ratio of the long-chain alkylbenzene sulfonic acid to the heavy alkylbenzene sulfonic acid is (1-10):(1-10).

[0024] As a further improvement of the present invention, in step 2,

[0025] The inorganic calcium comprises at least one of calcium oxide and calcium hydroxide, and the amount of the inorganic calcium added is 3 to 15 parts by weight;

[0026] The booster A is a small molecule acid, which includes one or more of formic acid, acetic acid, propionic acid, butyric acid, etc.; the amount of booster A added is 1 to 10 parts by weight.

[0027] As a further improvement of the present invention, in step 3, the ventilation rate of CO2 is constant and the rate is 10-150mL / min, preferably 50-150mL / min; the total ventilation volume of CO2 is 13.5-16L, the ventilation volume to the first node is 0% of the total ventilation volume, the ventilation volume to the second node is 20%-30% of the total ventilation volume, and the ventilation volume to the third node is 47%-60% of the total ventilation volume.

[0028] As a further improvement of the present invention, in step 3,

[0029] The inorganic calcium comprises at least one of calcium oxide and calcium hydroxide, and the amount of inorganic calcium added for the first time and the amount of inorganic calcium added twice thereafter are both 7 to 20 parts by weight;

[0030] The amount of water added for the first time and the amount of water added twice thereafter are both 2 to 15 parts by weight;

[0031] The auxiliary promoter B includes at least one of oleic acid amide, diethylenetriamine oleate, triethylenetetramine oleate and polymethyl methacrylate. The initial addition amount and the subsequent additional addition amount of the auxiliary promoter B are both 1 to 15 parts by weight.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] The present invention prepares synthetic alkylbenzene calcium sulfonate by using solvent oils such as nonanol, small molecule carboxylic acid, oleic acid amide and polymethyl methacrylate, thereby reducing the impact of traditional solvent oils such as toluene and xylene on health and the environment, achieving significant green transformation and performance optimization, and improving the anti-wear properties and pour point depression characteristics of the product by means of the friction reduction properties of oleic acid amide and the pour point depression properties of polymethyl methacrylate. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is a flow chart of the green and environmentally friendly preparation method of calcium sulfonate disclosed in the present invention;

[0035] Figure 2 This is a picture of the wear spots of the base oil;

[0036] Figure 3 This is the wear spot picture of Example 4. DETAILED DESCRIPTION

[0037] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] The present invention is further described in detail below in conjunction with the accompanying drawings:

[0039] like Figure 1 As shown, the present invention provides a green and environmentally friendly preparation method of calcium sulfonate, comprising:

[0040] Step 1, weighing: add the preset weight of solvent oil, main accelerator, and base oil to the reaction bottle in sequence and stir evenly mechanically, then add sulfonic acid and continue stirring for 5 to 10 minutes; wherein,

[0041] By weight, the addition amount of each component is: 70-200 parts of solvent oil, 10-50 parts of primary accelerator, 50-150 parts of base oil, and 10-100 parts of sulfonic acid;

[0042] The solvent oil is at least one of alkanes and alkanols, preferably undecane and / or n-nonanol;

[0043] The main accelerator is at least one of a monohydric alcohol and a polyhydric alcohol, such as one or more of methanol, ethanol, propanol, isopropanol, ethylene glycol, glycerol and sucrose, etc., preferably the main accelerator is methanol;

[0044] The base oil includes one or more of 100N, 150SN, 150N, 150SN, 150BS, 500N and 500SN, preferably 150N;

[0045] The sulfonic acid comprises at least one of long-chain alkylbenzene sulfonic acid, heavy alkylbenzene sulfonic acid and petroleum sulfonic acid. Preferably, the sulfonic acid is long-chain alkylbenzene sulfonic acid and heavy alkylbenzene sulfonic acid, and the weight ratio of the long-chain alkylbenzene sulfonic acid to the heavy alkylbenzene sulfonic acid is (1-10):(1-10), that is, 5-50 parts of long-chain alkylbenzene sulfonic acid and 5-50 parts of heavy alkylbenzene sulfonic acid.

[0046] Step 2, neutralization reaction: Under condensation reflux conditions, the reaction liquid temperature is controlled at 50-90°C, and the neutralization reaction timing is started after the addition of inorganic calcium. After 10-60 minutes, the co-promoter A is added and the reaction is continued for 5-30 minutes. The end of the reaction is judged to be pH ≥ 8; wherein,

[0047] The inorganic calcium comprises at least one of calcium oxide and calcium hydroxide, and the amount of the inorganic calcium added is 3 to 15 parts by weight;

[0048] The co-promoter A is various small molecule acids, preferably one or more of formic acid, acetic acid, propionic acid, butyric acid, etc.; by weight, the amount of co-promoter A added is 1 to 10 parts; that is, 1 to 10 parts of formic acid, 1 to 10 parts of acetic acid, 1 to 10 parts of propionic acid, and 1 to 10 parts of butyric acid.

[0049] Step 3, carbonation reaction: under condensation reflux conditions, control the temperature at 50-85°C, add 7-20 parts of inorganic calcium, 2-15 parts of water and 1-15 parts of promoter B at the first ventilation node and start to introduce CO2, the gas rate of CO2 is 10-150mL / min; when ventilation reaches the second node, add 7-20 parts of inorganic calcium, 2-15 parts of water and 1-15 parts of promoter B, and the reaction temperature and gas rate remain unchanged; when ventilation reaches the third node, add 7-20 parts of inorganic calcium and 2-15 parts of water, and the reaction temperature and gas rate remain unchanged; until the ventilation ends; wherein,

[0050] The ventilation rate of CO2 is constant and the ventilation rate is preferably 50-150 mL / min; the total ventilation volume of CO2 is 13.5-16 L, the ventilation volume to the first node is 0% of the total ventilation volume, the ventilation volume to the second node is 20%-30% of the total ventilation volume, and the ventilation volume to the third node is 47%-60% of the total ventilation volume;

[0051] The inorganic calcium comprises at least one of calcium oxide and calcium hydroxide, and the auxiliary promoter B comprises at least one of oleamide, diethylenetriamine oleate, triethylenetetramine oleate and polymethyl methacrylate, preferably oleamide and / or polymethyl methacrylate; in terms of weight, the amount of oleamide added each time is 3 to 15 parts, and the amount of polymethyl methacrylate added each time is 1 to 10 parts; it is further preferred that the auxiliary promoter B added for the first time and the auxiliary promoter B added subsequently can be the same or different components, such as the auxiliary promoter B added for the first time is polymethacrylate, and the auxiliary promoter B added subsequently is oleamide or polymethyl methacrylate; or, the auxiliary promoter B added for the first time is oleamide, and the auxiliary promoter B added subsequently is polymethacrylate or oleamide.

[0052] Step 4, de-alcoholization water: the vacuum is set at 0~-0.05MPa, the temperature is raised to 90~130℃, and the alcohol and water in the reaction solution are removed.

[0053] Step 5, filtration or centrifugation: remove solid residue by sedimentation, centrifugation or filtration.

[0054] Step 6, vacuum distillation: remove components such as solvent oil from the centrifuged or filtered sample at 0 to -0.1 MPa and 150 to 250° C. to obtain a finished product.

[0055] Embodiment 1:

[0056] Add 130 parts of n-nonanol, 15 parts of methanol, 70 parts of 150N, 25 parts of long-chain alkylbenzene sulfonic acid, 25 parts of heavy alkylbenzene sulfonic acid and 8 parts of calcium oxide to a 500ml four-necked flask. After reacting at 60°C for 40 minutes, add 3 parts of acetic acid and continue to react for 15 minutes. After the reaction, the pH of the reaction solution is ≥10. Lower the reaction temperature to 50°C, add 5 parts of oleamide, 14 parts of calcium oxide and 3 parts of water, and control the CO2 introduction rate to be constant at 110mL / min; when ventilated to 4.5L, add 3 parts of oleamide, 13 parts of calcium oxide and 3 parts of water, and the reaction temperature and CO2 introduction rate remain unchanged; when ventilated to 9.5L, add 12 parts of calcium oxide and 3 parts of water, the reaction temperature and CO2 introduction rate remain unchanged, ventilate to 15L to stop the reaction, and detect DBN=18mgKOH / g. Under -0.03MPa conditions, the alcohol water is dealcoholized to 130°C, and the material is translucent and brownish red. Then the finished product is obtained by precipitation, centrifugal removal of slag, and reduced pressure distillation to remove the solvent in the material.

[0057] Embodiment 2:

[0058] Add 150 parts of undecane, 20 parts of methanol, 70 parts of 150N, 30 parts of long-chain alkylbenzene sulfonic acid, 20 parts of heavy alkylbenzene sulfonic acid and 8 parts of calcium oxide to a 500ml four-necked flask in sequence. After reacting at 60°C for 40 minutes, add 3 parts of acetic acid and continue to react for 15 minutes. After the reaction, the pH of the reaction solution is ≥10. Lower the reaction temperature to 50°C, add 3 parts of polymethyl methacrylate, 14 parts of calcium oxide and 3 parts of water, and control the CO2 introduction rate to be constant at 110mL / min; when ventilated to 4.5L, add 2 parts of polymethyl methacrylate, 13 parts of calcium oxide and 3 parts of water, and the reaction temperature and CO2 introduction rate remain unchanged; when ventilated to 9.5L, add 12 parts of calcium oxide and 3 parts of water, and the reaction temperature and CO2 introduction rate remain unchanged. Ventilate to 15L to stop the reaction, and detect DBN=26mgKOH / g. Under -0.03MPa conditions, dealcoholate water to 130°C, and the material is translucent and brownish red. Then the finished product is obtained by precipitation, centrifugal removal of slag, and reduced pressure distillation to remove the solvent in the material.

[0059] Embodiment 3:

[0060] Add 150 parts of n-nonanol, 15 parts of methanol, 70 parts of 150N, 45 parts of long-chain alkylbenzene sulfonic acid, 15 parts of heavy alkylbenzene sulfonic acid and 8 parts of calcium oxide to a 500ml four-necked flask. After reacting at 60℃ for 40min, add 2 parts of formic acid and continue to react for 15min. After the reaction, the pH of the reaction solution is ≥10. Lower the reaction temperature to 50℃, add 5 parts of oleamide, 14 parts of calcium oxide and 3 parts of water, and control the CO2 introduction rate to be constant at 110mL / min; when ventilated to 4.0L, add 3 parts of oleamide, 13 parts of calcium oxide and 3 parts of water, and the reaction temperature and CO2 introduction rate remain unchanged; when ventilated to 9.0L, add 12 parts of calcium oxide and 3 parts of water, the reaction temperature and CO2 introduction rate remain unchanged, ventilate to 15L to stop the reaction, and detect DBN=15mgKOH / g. Under -0.03MPa conditions, the water is dealcoholized to 130℃, and the material is translucent and brownish red. Then the finished product is obtained by precipitation, centrifugal removal of slag, and reduced pressure distillation to remove the solvent in the material.

[0061] Embodiment 4:

[0062] Add 130 parts of undecane, 20 parts of methanol, 70 parts of 150N, 15 parts of long-chain alkylbenzene sulfonic acid, 50 parts of heavy alkylbenzene sulfonic acid and 8 parts of calcium oxide to a 500ml four-necked flask in sequence. After reacting at 60℃ for 40min, add 2 parts of formic acid and continue to react for 15min. After the reaction, the pH of the reaction solution is ≥10. Lower the reaction temperature to 50℃, add 3 parts of polymethyl methacrylate, 14 parts of calcium oxide and 3 parts of water, and control the CO2 introduction rate to be constant at 110mL / min; when ventilated to 4.5L, add 3 parts of oleamide, 13 parts of calcium oxide and 3 parts of water, and the reaction temperature and CO2 introduction rate remain unchanged; when ventilated to 9.5L, add 12 parts of calcium oxide and 3 parts of water, and the reaction temperature and CO2 introduction rate remain unchanged. Ventilate to 15L to stop the reaction, and detect DBN=20mgKOH / g. Under -0.03MPa conditions, the water is dealcoholized to 130℃, and the material is translucent and brownish red. Then the finished product is obtained by precipitation, centrifugal removal of slag, and reduced pressure distillation to remove the solvent in the material.

[0063] Comparative Example 1 (without adding oil amide)

[0064] The synthetic alkylbenzene sulfonate prepared in this comparative example is basically the same as the relevant operation of Example 1, except that the oleic acid amide in Example 1 is replaced with n-nonanol of the same mass. The difference during the experiment is that the reaction liquid turns white when the aeration reaches 15L, and the detection DBN=78mgKOH / g.

[0065] Comparative Example 2 (without acetic acid)

[0066] The synthetic alkylbenzene sulfonate calcium prepared in this comparative example is basically the same as the relevant operation of Example 1, except that the acetic acid in Example 1 is replaced with n-nonanol of the same mass. The difference during the experiment is that the reaction solution is in a jelly state when the aeration reaches 15L.

[0067] Comparative Example 3 (without adding polymethyl methacrylate)

[0068] The synthetic alkylbenzene sulfonate prepared in this comparative example is basically the same as the relevant operation of Example 2, except that the polymethyl methacrylate in Example 2 is replaced with an equal mass of undecane. The difference during the experiment is that the reaction liquid turns white when the aeration reaches 15L, and the detected DBN is 86mgKOH / g.

[0069] 1. Physical and chemical indicators

[0070] The physical and chemical data of the above-mentioned Examples 1-4, Comparative Examples 1-3 and commercially available T106D are shown in Table 1.

[0071] Table 1

[0072]

[0073]

[0074] Note: During the preparation process of Comparative Example 2, the reaction solution was in a jelly state, indicating that the experiment failed. Therefore, there is no test data for Comparative Example 2 in Table 1.

[0075] Results and analysis:

[0076] 1) As shown in Table 1, Examples 1 to 4 do not contain chlorine and phenol, and the base value, viscosity, Ca content and S content fluctuate slightly, reflecting that the process of the present invention is stable and the results are controllable;

[0077] 2) Without the addition of oleamide or polymethyl methacrylate, TBN, viscosity, and Ca content decreased significantly, and the centrifugal residue rate increased significantly. There was a phenomenon of calcium loss in the late stage of the reaction, which was related to the instability of micelles in the late stage of the reaction. This shows that the addition of oleamide or polymethyl methacrylate helps to improve the stability of micelles, which is conducive to the stable reaction and the product reaching the standard and being stable.

[0078] 3) If acetic acid is not added, calcium loss and gelation occur in the later stage of the reaction, reflecting that in the absence of small molecule carboxylic acids, the stability of the micelles decreases significantly, which is not conducive to the stable progress of the reaction and the formation of products.

[0079] 2. Oil solubility and colloid stability

[0080] Examples 1 to 4 and commercially available samples were prepared into 50% samples with kerosene and placed at high temperature of 80°C for three months to observe their colloidal stability; samples were prepared into 25% samples with three types of oils and placed for three months to observe their oil solubility. The results are shown in Table 2.

[0081] Table 2

[0082]

[0083]

[0084] Results and analysis:

[0085] As shown in Table 2, in terms of oil solubility, after being placed at room temperature for three months, the samples of Examples 1 to 4 showed no abnormality, which was better than the commercially available T106D; in terms of colloid stability, after being placed at 80°C for three months, the samples of the examples showed no abnormality, which was better than the commercially available T106D. By comparing the results, the quality of the present invention in terms of oil solubility and colloid stability is excellent, which is higher than the quality of the products currently circulating in the market. This is mainly related to the selection of appropriate additives, solvents and other reaction parameters in the present invention, and the appropriate process route ensures that the product has excellent oil solubility and colloid stability.

[0086] 3. Performance evaluation

[0087] The detergency performance was evaluated by testing the examples and the commercially available T106D coke plate (base oil 500SN); the anti-wear performance was evaluated by the four-ball method (base oil 150N), and the pour point depression effect was evaluated by measuring the pour point (base oil 150N). The results are shown in Table 3.

[0088] Table 3

[0089]

[0090] Results and analysis:

[0091] 1) The rubber weights of Examples 1 to 4 and the commercially available T106D are all less than the base oil, indicating that the presence of calcium sulfonate can significantly improve the high-temperature detergency of the oil; the rubber weights of Examples 1 to 4 are all less than 15 mg, and the rubber weights of the commercially available T106D are all greater than 17 mg, reflecting that the samples of the examples have better high-temperature detergency than the commercially available T106D.

[0092] 2) The wear spot diameters of the embodiment and the commercially available T106D are significantly reduced compared with the base oil, indicating that calcium sulfonate has certain anti-wear properties; the wear spot diameter of the embodiment is significantly reduced compared with the commercially available T106D, and has better anti-wear properties, reflecting that the friction reduction properties of oleic acid amide improve the anti-wear and friction reduction capabilities of calcium sulfonate; the wear spot diameter of embodiment 2 is larger than that of other embodiments, which is mainly related to the absence of oleic acid amide with friction reduction properties in embodiment 2; wherein, the wear spot image of the base oil is as shown in FIG. Figure 2 As shown, the wear spot image of Example 4 is as follows Figure 3 shown.

[0093] 3) Compared with the base oil and other calcium sulfonate samples, Examples 2 and 4 have lower pour points. There is almost no significant difference between the pour points of other calcium sulfonate samples and the base oil. This is mainly due to the introduction of polymethyl methacrylate, which significantly reduces the pour point of the oil.

[0094] 4) Data analysis shows that the introduction of additives such as oleamide and polymethyl methacrylate not only improves the stability of micelles and promotes the stable occurrence of the reaction, but also significantly improves the anti-wear properties of calcium sulfonate oil and reduces the freezing point of the oil.

[0095] The advantages of the present invention are:

[0096] Compared with the traditional synthesis process, the present invention uses solvent oils such as nonanol, small molecule carboxylic acids, oleic acid amide and polymethyl methacrylate to prepare synthetic alkylbenzene sulfonate, thereby reducing the impact of traditional solvent oils such as toluene and xylene on health and the environment, achieving significant green transformation and performance optimization, and improving the product's anti-wear properties and de-condensation characteristics by virtue of the friction-reducing properties of oleic acid amide and the de-condensation properties of polymethyl methacrylate.

[0097] It is specifically reflected in the following aspects:

[0098] 1. Application of environmentally friendly reagents. The present invention adopts a safer and more environmentally friendly solvent system, and abandons the chloride and phenol salt additives that may be introduced in the traditional process;

[0099] 2. Improvement of product quality. In terms of physical and chemical properties, the product of the present invention has stable physical and chemical indicators, extremely low centrifugal residue content, and achieves zero detection of chlorine and phenol content;

[0100] 3. The performance is more competitive. The product of the present invention is higher in oil solubility, colloid stability, high temperature detergency, wear resistance and pour point reduction properties than the high-end T106D product on the market, providing solid technical support for improving engine operating efficiency and extending equipment service life;

[0101] 4. Significant improvement in comprehensive benefits. The present invention is not limited to technical innovation, but also aims to comprehensively promote environmental protection, product quality improvement and market application potential.

[0102] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A green and environmentally friendly preparation method of calcium sulfonate, characterized in that: include: Step 1, add solvent oil, primary accelerator, base oil and sulfonic acid into a reaction bottle and stir evenly; Step 2: Under condensation reflux conditions, the reaction liquid temperature is controlled at 50-90° C., and after adding inorganic calcium, the neutralization reaction timing is started. After 10-60 minutes, the co-promoter A is added and the reaction is continued for 5-30 minutes; Step 3, under the condition of condensation reflux, control the temperature at 50-85°C, add inorganic calcium, water and booster B at the first ventilation node and start to introduce CO2; when ventilation reaches the second node, add inorganic calcium, water and booster B; when ventilation reaches the third node, add inorganic calcium and water until the ventilation ends; Step 4: raising the temperature to 90-130° C. under a vacuum pressure of 0-0.05 MPa to remove alcohol and water from the reaction solution, and removing solid residue by filtering or centrifugation; Step 5: subject the centrifuged sample or the filtered sample to vacuum distillation at 0 to -0.1 MPa and 150 to 250° C. to obtain a finished product.

2. The green and environmentally friendly preparation method of calcium sulfonate as claimed in claim 1, characterized in that, In step 1, by weight, there are 70 to 200 parts of solvent oil, 10 to 50 parts of primary accelerator, 50 to 150 parts of base oil, and 10 to 100 parts of sulfonic acid.

3. The green and environmentally friendly preparation method of calcium sulfonate as claimed in claim 1 or 2, characterized in that, In step 1, The solvent oil includes at least one of alkanes and alkanols; The primary accelerator includes at least one of a monohydric alcohol and a polyhydric alcohol; The base oil comprises at least one of 100N, 150SN, 150N, 150SN, 150BS, 500N and 500SN; The sulfonic acid includes at least one of long-chain alkylbenzene sulfonic acid, heavy alkylbenzene sulfonic acid and petroleum sulfonic acid.

4. The green and environmentally friendly preparation method of calcium sulfonate as claimed in claim 3, characterized in that, The solvent oil is undecane and / or n-nonanol, the main accelerator is methanol, the base oil is 150N, the sulfonic acid is long-chain alkylbenzene sulfonic acid and heavy alkylbenzene sulfonic acid, and the weight ratio of the long-chain alkylbenzene sulfonic acid to the heavy alkylbenzene sulfonic acid is (1-10):(1-10).

5. The green and environmentally friendly preparation method of calcium sulfonate as claimed in claim 1, characterized in that, In step 2, The inorganic calcium comprises at least one of calcium oxide and calcium hydroxide, and the amount of the inorganic calcium added is 3 to 15 parts by weight; The booster A is a small molecule acid, which includes one or more of formic acid, acetic acid, propionic acid, butyric acid, etc.; the amount of booster A added is 1 to 10 parts by weight.

6. The green and environmentally friendly preparation method of calcium sulfonate as claimed in claim 1, characterized in that, In step 3, the ventilation rate of CO2 is constant and the rate is 10-150mL / min, preferably 50-150mL / min; the total ventilation volume of CO2 is 13.5-16L, the ventilation volume to the first node is 0% of the total ventilation volume, the ventilation volume to the second node is 20%-30% of the total ventilation volume, and the ventilation volume to the third node is 47%-60% of the total ventilation volume.

7. The green and environmentally friendly preparation method of calcium sulfonate as claimed in claim 1, characterized in that, In step 3, The inorganic calcium comprises at least one of calcium oxide and calcium hydroxide, and the amount of inorganic calcium added for the first time and the amount of inorganic calcium added twice thereafter are both 7 to 20 parts by weight; The amount of water added for the first time and the amount of water added twice thereafter are both 2 to 15 parts by weight; The auxiliary promoter B includes at least one of oleic acid amide, diethylenetriamine oleate, triethylenetetramine oleate and polymethyl methacrylate. The initial addition amount and the subsequent additional addition amount of the auxiliary promoter B are both 1 to 15 parts by weight.