Treatment method for improving structure and performance of hypoeutectic Al-Mg2Si alloy

By performing electrical pulse melt treatment on Al-Mg2Si alloy, refine the grains and uniformly distribute eutectic structure, the problem of degradation of alloy mechanical properties is solved, and the hardness and corrosion resistance of the alloy are significantly improved, which is suitable for industrial production.

CN118957326AActive Publication Date: 2024-11-15LIAONING UNIVERSITY OF TECHNOLOGY

Patent Information

Application Number
CN202411069615.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-15
Estimated Expiration
2044-08-06

AI Technical Summary

Technical Problem

The Mg2Si particles generated by the Al-Mg2Si alloy during conventional casting are too large, resulting in a decrease in the mechanical properties of the alloy, and it is difficult to control the solidification structure and dendrite segregation of the alloy, affecting the mechanical properties.

Method used

By performing electrical pulse melt treatment on subeutectic Al-Mg2Si alloy, the electrical pulse processing parameters, such as pulse voltage, frequency and time, the grain size of α-Al is refined, and the α-Al+Mg2Si eutectic structure is uniformly distributed. , improve dendrites segregation in solidified structure.

Benefits of technology

The performance of the alloy is significantly improved, including improving hardness, corrosion resistance and tensile properties, forming high-quality ingots, suitable for the industrial production of large-scale alloys.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957326A_ABST
    Figure CN118957326A_ABST
Patent Text Reader

Abstract

The invention provides a treatment method for improving the structure and performance of a hypoeutectic Al-Mg2Si alloy, and belongs to the technical field of metal material treatment. The treatment method provided by the invention comprises the following steps: carrying out electric pulse treatment on a hypoeutectic Al-Mg2Si alloy melt; the technological parameters of the electric pulse treatment are as follows: the pulse voltage is 300V-700V, the pulse frequency is 22Hz, and the pulse treatment time is 30s. According to the method, the electric pulse treatment is introduced into the hypoeutectic Al-Mg2Si alloy melt, and the high-quality cast ingot is prepared. On one hand, due to electromagnetic force and pulse oscillation generated by a pulse electromagnetic field, heterogeneous atomic clusters in liquid metal are reduced, similar atomic clusters are increased, and therefore the purpose of refining an alloy solidification structure is achieved, on the other hand, solute atoms are promoted to diffuse under the action of electric pulses, the segregation degree of a second phase is remarkably improved, and therefore the performance of the alloy is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal material processing, and in particular to a processing method for improving the structure and performance of a hypoeutectic Al-Mg2Si alloy. Background Art

[0002] As an intermetallic compound, Mg2Si has many excellent properties such as high strength, high hardness, high wear resistance, high melting point and high elastic modulus. In Al-Mg2Si alloy, Mg2Si as the strengthening phase of the alloy has an important influence on the mechanical properties of the alloy. At present, there are great potential advantages in new structural materials, which can be used in many fields, such as power generation, refrigeration and even military, aerospace, automobiles, etc. However, conventional casting of Al-Mg2Si alloy will cause the size of intermetallic Mg2Si to increase, forming an undesirable coarse skeleton shape. At this time, the coarse and irregularly shaped particles will split the matrix, generate crack sources, and seriously reduce the mechanical properties of the alloy. Therefore, the key to the preparation of Al-Mg2Si alloy is to control the shape and size of Mg2Si particles generated in the Al matrix and improve the dendrite segregation in the solidification structure, which directly affects the mechanical properties of the alloy. Therefore, controlling the material structure and properties from the metallurgical source has an important role and practical significance. Summary of the invention

[0003] Based on the above content, the purpose of the present invention is to provide a processing method for improving the structure and properties of hypoeutectic Al-Mg2Si alloy. The present invention improves the structure of hypoeutectic Al-Mg2Si alloy, refines the grain size of α-Al, reduces the size of α-Al+Mg2Si eutectic structure and makes it evenly distributed, improves dendrite segregation in solidification structure, and thus improves the performance of hypoeutectic Al-Mg2Si alloy by performing electric pulse melt treatment on hypoeutectic Al-Mg2Si alloy and adjusting the electric pulse treatment parameters.

[0004] In order to achieve the above-mentioned purpose, the present invention provides the following technical scheme: a processing method for improving the structure and properties of hypoeutectic Al-Mg2Si alloy, wherein the hypoeutectic Al-Mg2Si alloy melt is subjected to electric pulse treatment; the process parameters of the electric pulse treatment are: pulse voltage of 300V to 700V, pulse frequency of 22Hz, and pulse treatment time of 30s.

[0005] In some embodiments of the present invention, the pulse voltage is 300 V, the pulse frequency is 22 Hz, and the pulse time is 30 s.

[0006] In some embodiments of the present invention, the hypoeutectic Al-Mg2Si alloy melt comprises 93% Al, 5% Mg and 2% Si by mass percentage.

[0007] The Mg content in Al-based alloys is generally 0.8% to 1.2%, and the Si content is generally 0.4% to 0.8%. The strength and hardness of the obtained Al-based alloys are low, and the corrosion resistance is poor. The present invention adds a higher content of Mg and Si elements to the Al-Mg2Si alloy. The Mg element can reduce the eutectic point of the alloy and improve the corrosion resistance. The addition of Si elements can improve the fluidity of the alloy and improve the mechanical properties. If the content of Mg and Si elements is too much, it will reach the level of eutectic alloy, which deviates from the purpose of the present invention to improve the hypoeutectic alloy, and too much Mg and Si elements will have the opposite effect.

[0008] In some embodiments of the present invention, electric pulse treatment is performed when the temperature of the hypoeutectic Al-Mg2Si alloy melt is 720-750°C.

[0009] In some embodiments of the present invention, after the electric pulse treatment, a heat preservation step is also included.

[0010] In some embodiments of the present invention, the insulation temperature is 740° C. and the time is 5 minutes.

[0011] In some embodiments of the present invention, after the insulation is completed, a casting step is also included.

[0012] The casting temperature will affect the performance of the alloy. When the casting temperature is high, the cooling rate is slow, the supercooling degree is small, and the atomic clusters grow during the solidification process, making the alloy structure coarse after forming and the performance is low. When the casting temperature is low, the cooling rate is fast and the supercooling degree is large, which will inhibit the growth of atomic clusters during the solidification process, making the structure after solidification finer, and can improve the performance of the alloy. Therefore, the preferred alloy melt temperature during casting in the present invention is 740°C (casting is performed after keeping at 740°C for 5 minutes, that is, the temperature of the alloy melt during casting is 740°C).

[0013] The present invention discloses the following technical effects:

[0014] The present invention introduces electric pulse treatment into the hypoeutectic Al-Mg2Si alloy melt to prepare high-quality ingots. On the one hand, due to the electromagnetic force and pulse oscillation generated by the pulse electromagnetic field, heterogeneous atomic clusters in the liquid metal are reduced and homogeneous atomic clusters are increased, thereby achieving the purpose of refining the alloy solidification structure. On the other hand, the action of the electric pulse promotes the diffusion of solute atoms, significantly improves the segregation degree of the second phase, and thus improves the performance of the alloy.

[0015] The method of the present invention for performing electric pulse treatment on a hypoeutectic Al-Mg2Si alloy in a melt stage is suitable for large-scale alloy treatment and is more conducive to industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0017] Figure 1 Schematic diagram of the microstructure of Al-Mg2Si alloy prepared by Comparative Example 1 and Examples 1-5 of the present invention, wherein (a) is Comparative Example 1, (b) is Example 1, (c) is Example 2, (d) is Example 3, (e) is Example 4, and (f) is Example 5.

[0018] Figure 2 This is a diagram of the average grain size of the Al-Mg2Si alloy prepared in Comparative Example 1 and Examples 1-5 of the present invention.

[0019] Figure 3 The second phase area fraction diagram of the Al-Mg2Si alloy prepared in Comparative Example 1 and Examples 1-5 of the present invention.

[0020] Figure 4 XRD diagram of the Al-Mg2Si alloy prepared in Comparative Example 1 and Examples 1-5 of the present invention.

[0021] Figure 5 These are scanning electron microscope images of Al-Mg2Si alloys prepared in Comparative Example 1 and Examples 1-5, wherein (a) is Comparative Example 1, (b) is Example 1, (c) is Example 2, (d) is Example 3, (e) is Example 4, and (f) is Example 5.

[0022] Figure 6 The scanning electron microscope dot scan images are of the Al-Mg2Si alloys prepared in Comparative Example 1 and Examples 1-5, wherein (a) is Comparative Example 1, (b) is Example 1, (c) is Example 2, (d) is Example 3, (e) is Example 4, and (f) is Example 5.

[0023] Figure 7 The hardness variation diagram of the Al-Mg2Si alloy prepared in Comparative Example 1 and Examples 1-5.

[0024] Figure 8 Graph showing changes in tensile properties of Al-Mg2Si alloys prepared in Comparative Example 1 and Examples 1-5.

[0025] Fig. 9 Polarization curves (a) and Nyquist diagrams (b) of Al-Mg2Si alloy samples under different pulse voltages.

[0026] Fig.10 These are three-dimensional morphologies of Al-Mg2Si alloys after corrosion prepared in Comparative Example 1 and Examples 1-5, wherein (a) is Comparative Example 1, (b) is Example 1, (c) is Example 2, (d) is Example 3, (e) is Example 4, and (f) is Example 5. DETAILED DESCRIPTION

[0027] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0028] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0029] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0030] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.

[0031] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0032] The invention provides a processing method for improving the structure and performance of a hypoeutectic Al-Mg2Si alloy, wherein the hypoeutectic Al-Mg2Si alloy melt is subjected to electric pulse treatment; the process parameters of the electric pulse treatment are: a pulse voltage of 300V to 700V, a pulse frequency of 22Hz, and a pulse treatment time of 30s.

[0033] The present invention improves the microstructure of the hypoeutectic Al-Mg2Si alloy, refines the grain size of α-Al, reduces the size of the α-Al+Mg2Si eutectic structure, and makes it evenly distributed, improves the dendrite segregation in the solidified structure, and thus improves the performance of the hypoeutectic Al-Mg2Si alloy by performing an electric pulse melt treatment on the hypoeutectic Al-Mg2Si alloy and adjusting the electric pulse treatment parameters. The specific steps are as follows:

[0034] Step 1. Melting Al-Mg2Si alloy: weigh raw materials Al, master alloy Al-22Si and Mg according to the mass ratio, heat Al and master alloy Al-22Si to 750°C until they are completely melted, wrap metal Mg with aluminum foil, press metal Mg into the metal melt with a bell jar, put it into a furnace and keep it warm for 5 minutes (the insulation temperature is 750°C) after the metal Mg is completely melted, then bury the refining agent (the amount of the refining agent is 0.5wt% of the Al-Mg2Si alloy ingot) in the metal melt with a bell jar for about 2-3 minutes, remove the slag on the surface of the melt, and then put it back into the resistance furnace and keep it warm for 5 minutes (the insulation temperature is 750°C) to obtain Al-Mg2Si alloy melt;

[0035] Step 2. Electric pulse treatment: The Al-Mg2Si alloy melt obtained in step 1 is subjected to electric pulse treatment, and after the treatment, it is placed in a furnace and kept at 740°C for 5 minutes; wherein the pulse voltage is 300V to 700V, the pulse frequency is 22Hz, and the pulse treatment time is 30s;

[0036] Step 3. Casting: Cast the sample obtained in step 2 into a mold to cast the alloy melt to obtain a processed Al-Mg2Si alloy sample.

[0037] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the content of the present invention is not limited to the following embodiments.

[0038] The refining agent used in the examples is a commonly used refining agent in the art and is obtained through commercial channels.

[0039] In the embodiments and comparative examples, each component in the alloy melt was weighed according to the mass ratio (Table 1);

[0040] Among them, the content of each element is as follows: Al: 93%, Mg: 5%, Si: 2%;

[0041] The burning loss rate of each element is: Al: 2%, Mg: 25%, Al-22Si: 1%;

[0042] Table 1 Alloy chemical composition (wt.%)

[0043]

[0044] Example 1

[0045] Step 1. Melting Al-Mg2Si alloy: weighed Al and intermediate alloy Al-22Si are put into a graphite crucible, the graphite crucible is put into a resistance furnace and heated to 750°C until it is completely melted, the metal Mg is wrapped with aluminum foil, the metal Mg is pressed into the metal melt by a bell jar, and after the metal Mg is completely melted, it is put into the furnace at 750°C for 5 minutes, and then a refining agent (the amount of the refining agent is 0.5wt% of the Al-Mg2Si alloy ingot) is buried in the metal melt with a bell jar for about 3 minutes, and then the slag on the surface of the melt is removed, and then it is put back into the resistance furnace and kept at 750°C for 5 minutes to obtain an Al-Mg2Si alloy melt;

[0046] Step 2. Electric pulse treatment: insert a metal electrode into a crucible, and perform electric pulse treatment on the Al-Mg2Si alloy melt obtained in step 1. After the treatment, put it into a furnace and keep it at 740°C for 5 minutes; wherein the pulse voltage is 300V, the pulse frequency is 22Hz, and the pulse treatment time is 30s;

[0047] Step 3. Casting: Cast the sample obtained in step 2 into a mold to cast the alloy melt to obtain an Al-Mg2Si alloy sample.

[0048] Example 2

[0049] The preparation method of the Al-Mg2Si alloy sample in this embodiment is the same as that in Embodiment 1, except that the pulse voltage is 400V.

[0050] Example 3

[0051] The preparation method of the Al-Mg2Si alloy sample in this embodiment is the same as that in Embodiment 1, except that the pulse voltage is 500V.

[0052] Example 4

[0053] The preparation method of the Al-Mg2Si alloy sample in this embodiment is the same as that in Embodiment 1, except that the pulse voltage is 600V.

[0054] Example 5

[0055] The preparation method of the Al-Mg2Si alloy sample in this embodiment is the same as that in Embodiment 1, except that the pulse voltage is 700V.

[0056] Comparative Example 1

[0057] The preparation method of the Al-Mg2Si alloy sample in this comparative example is the same as that in Example 1, except that the step of electric pulse treatment is omitted.

[0058] Figure 1 Schematic diagram of the microstructure of the Al-Mg2Si alloy prepared in Examples 1-5 and Comparative Example 1. Figure 1 (a) is the alloy solidification structure of the original sample without electric pulse treatment (Comparative Example 1). It can be seen that the eutectic α-Al+Mg2Si structure presents a coarse lamellar structure, and the primary α-Al presents a coarse dendrite structure; Figure 1 (b) is the alloy solidification structure when the pulse voltage is 300V (Example 1). It can be seen that when the pulse voltage is 300V, the α-Al and α-Al+Mg2Si structures are significantly refined, and the grains are evenly distributed; Figure 1 (c) is the alloy solidification structure when the pulse voltage is 400V (Example 2). Compared with the untreated alloy solidification structure (Comparative Example 1), the α-Al structure is significantly refined, and the α-Al+Mg2Si structure is slightly refined; Figure 1 (d) is the alloy solidification structure when the pulse voltage is 500V (Example 3). Compared with the solidification structure of the original sample (Comparative Example 1), the α-Al+Mg2Si structure is more obviously refined, and the α-Al is slightly coarser than when the pulse voltage is 300V (Example 1); Figure 1 (e) is the alloy solidification structure when the pulse voltage is 600V (Example 4). Compared with the original sample (Comparative Example 1), the α-Al is obviously refined and the α-Al+Mg2Si structure is refined; Figure 1 (f) is the alloy solidification structure when the pulse voltage is 700V (Example 5). Compared with the original sample (Comparative Example 1), the α-Al and α-Al+Mg2Si structures are both refined. Therefore, when the pulse voltage is 300V, the alloy solidification structure refinement effect is most significant. When the pulse voltage is 500V, 600V and 700V, the organizational difference is not large.

[0059] Figure 2 The figure is a graph showing the average grain size of the Al-Mg2Si alloy prepared in Comparative Example 1 and Examples 1-5 of the present invention. Figure 2It can be seen that when the pulse voltage increases from 0V to 300V, the average grain size of α-Al and Mg2Si decreases sharply. When the pulse voltage increases from 300V to 700V, the average grain size of α-Al and Mg2Si first increases and then tends to be stable. The average grain sizes of α-Al and eutectic α-Al+Mg2Si structures of the untreated sample are 150.39μm and 155.74μm, respectively. When the pulse voltage is 300V, the average grain sizes of α-Al and eutectic α-Al+Mg2Si are 110.89μm and 93.35μm, respectively; when the pulse voltage is 400V, the average grain sizes of α-Al and eutectic α-Al+Mg2Si are 127.98μm and 110.11μm, respectively; when the pulse voltage is 400V, the average grain sizes of α-Al and eutectic α-Al+Mg2Si are 127.98μm and 110.11μm, respectively. When the pulse voltage is 500V, the average grain sizes of α-Al and eutectic α-Al+Mg2Si are 132.31μm and 125.96μm, respectively; when the pulse voltage is 600V, the average grain sizes of α-Al and eutectic α-Al+Mg2Si are 131.29μm and 122.37μm, respectively; when the pulse voltage is 700V, the average grain sizes of α-Al and eutectic α-Al+Mg2Si are 133.65μm and 126.27μm, respectively. The average grain sizes of α-Al and Mg2Si of the untreated sample are 1.36 times and 1.67 times that of the pulse voltage of 300V. Therefore, when the pulse voltage is 300V, the grains are the finest.

[0060] Figure 3 The second phase area fraction diagram of the Al-Mg2Si alloy prepared in Comparative Example 1 and Examples 1-5 of the present invention. Figure 3 It can be seen that with the continuous increase of pulse voltage, the second phase area fraction (Acre) of the alloy solidification structure first increases, then decreases, and then increases. When the pulse voltage is 300V, the second phase area fraction is 40.47%; when the pulse voltage is 400V, the second phase area fraction is 43.53%; when the pulse voltage is 500V, the second phase area fraction is 44.71%; when the pulse voltage is 600V, the second phase area fraction is 44.33%; when the pulse voltage is 700V, the second phase area fraction is 45.18%. The second phase area fractions of the samples with pulse voltage are better than those of the untreated samples. The second phase area fraction of the untreated sample is 46.58%, which is 1.15 times that of the pulse voltage of 300V. Therefore, when the pulse voltage is 300V, the second phase area fraction is the smallest.

[0061] Figure 4The XRD diagram of the Al-Mg2Si alloy prepared in Comparative Example 1 and Examples 1-5 of the present invention. The position of the diffraction peak of the XRD curve of the Al-Mg2Si alloy did not change before and after the electric pulse treatment, and both were composed of α-Al and Mg2Si phases. It can be determined that only α (Al) and Mg2Si phases exist in the alloy structure, and no new diffraction peaks appear, that is, there is no increase or decrease in other elements. However, after the electric pulse treatment, the diffraction peak intensity and diffraction angle 2θ of the α (Al) and η (Mg2Si) phases change, from which it can be seen that the electric pulse treatment promotes the process of crystal nucleation.

[0062] Figure 5 This is a scanning electron microscope image of the Al-Mg2Si alloy prepared in Comparative Example 1 and Examples 1-5 of the present invention. Figure 5 (a) is a scan of an untreated sample (Comparative Example 1). Figure 5 (b) is a surface scan of a sample with a pulse voltage of 300 V (Example 1). Figure 5 (c) is a surface scan of a sample with a pulse voltage of 400 V (Example 2), Figure 5 (d) is a surface scan of the sample with a pulse voltage of 500 V (Example 3). Figure 5 (e) is a surface scan of a sample with a pulse voltage of 600 V (Example 4), Figure 5 (f) is a surface scan of the sample with a pulse voltage of 700 V (Example 5). Overall, Al, Mg, and Si elements are evenly distributed, with most of Mg and Si distributed on the grain boundaries and only a small amount of Mg and Si elements distributed on the Al matrix.

[0063] Figure 6 Scanning electron microscope dot scan images of Al-Mg2Si alloys prepared in Comparative Example 1 and Examples 1-5 of the present invention, wherein (a) is Comparative Example 1, (b) is Example 1, (c) is Example 2, (d) is Example 3, (e) is Example 4, and (f) is Example 5. Figure 6 In the figure, the plane black area is the α-Al matrix, and the white and black strips are the Mg2Si phase. α-Al and Mg2Si phases are distributed in (a)-(f). In (a), there is a coarse lamellar eutectic α-Al+Mg2Si structure, and the Mg2Si phase is in a coarse block. In (b), the eutectic α-Al+Mg2Si structure is the finest and evenly distributed, and the Mg2Si phase is obviously refined and in the form of thin strips. In (c)-(d), the size of the eutectic α-Al+Mg2Si structure gradually increases, and the Mg2Si also increases accordingly.

[0064] right Figure 6The α-Al matrix and Mg2Si phase in the casting were scanned to determine their element contents as shown in Tables 2 and 3. The results show that with the increase of the pulse voltage, the Al content in the α-Al matrix does not change much, the Mg content gradually increases, and the Si content gradually decreases. With the decrease of the casting temperature, the Al content in the Mg2Si phase gradually increases, and the Mg content first decreases, then increases, and then decreases. The Si content first increases, then decreases, and then increases.

[0065] Table 2 SEM point scanning results of α-Al matrix under different pulse voltages (Wt%)

[0066]

[0067] Table 3 SEM point scanning results of Mg2Si under different pulse voltages (Wt%)

[0068]

[0069]

[0070] Figure 7 The hardness change diagram of the Al-Mg2Si alloy prepared in Comparative Example 1 and Examples 1-5. As the pulse voltage increases, the microhardness of the Al-Mg2Si alloy shows a trend of first increasing, then decreasing, and then increasing again. When the pulse voltage is 300V (Example 1), the hardness of the alloy is 82.65HV 0.2 When the pulse voltage is 400V (Example 2), the hardness of the alloy is 84.20HV 0.2 When the pulse voltage is 500V (Example 3), the hardness of the alloy is 87.70HV 0.2 When the pulse voltage is 600V (Example 4), the hardness of the alloy is 86.50HV 0.2 When the pulse voltage is 700V (Example 5), the hardness of the alloy is 87.80HV 0.2 The alloy hardness of the untreated sample (Comparative Example 1) is 75.75HV 0.2 When the pulse voltage is 700V, the maximum hardness is 87.80HV 0.2 , which is 1.16 times that of the untreated sample. Therefore, the hardness is maximum when the pulse voltage is 700V.

[0071] like Figure 8The tensile properties of Al-Mg2Si alloys prepared in Comparative Example 1 and Examples 1-5 are shown in Figure 1. The tensile strength decreases rapidly and then stabilizes with the increase of the pulse voltage, and the elongation decreases rapidly and then increases with the increase of the pulse voltage. The tensile strength and elongation of the untreated sample (Comparative Example 1) are 161.28 MPa and 1.43%, respectively. When the pulse voltage is 300V (Example 1), the tensile strength of the alloy is 261.01MPa and the elongation is 5.87%; when the pulse voltage is 400V (Example 2), the tensile strength of the alloy is 224.23MPa and the elongation is 3.14%; when the pulse voltage is 500V (Example 3), the tensile strength of the alloy is 211.15MPa and the elongation is 2.66%; when the pulse voltage is 600V (Example 4), the tensile strength of the alloy is 213.01MPa and the elongation is 2.79%; when the pulse voltage is 700V (Example 5), the tensile strength of the alloy is 212.12MPa and the elongation is 3.52%. When the pulse voltage is 300V, the tensile strength of the alloy is the largest, which is 1.22 times and 3.06 times the tensile strength and elongation of the untreated alloy sample, respectively. Therefore, when the pulse voltage is 300V, the tensile strength and elongation are the best.

[0072] Polarization curves of Al-Mg2Si alloy samples under different pulse voltages are shown in Figure 2. Fig. 9 As shown in (a). It can be seen that under different pulse voltages, the cathode polarization curve of Al-Mg2Si alloy is relatively smooth, and there is a large passivation zone at the anode, indicating that the polarization rate and resistance are poor during the electrode reaction. The self-corrosion potential of the untreated sample (Comparative Example 1) is Ecorr = -1.4474V, and the self-corrosion current density is Icorr = 1.544×10 -3 A / cm 2 When the pulse voltage is 300 V (Example 1), the self-corrosion potential of the alloy is Ecorr = -1.2056 V, and the self-corrosion current density is Icorr = 5.740 × 10 -6 A / cm 2 When the pulse voltage is 400 V (Example 2), the self-corrosion potential of the alloy is Ecorr = -1.3430 V, and the self-corrosion current density is Icorr = 9.820 × 10 -5 A / cm 2 When the pulse voltage is 500 V (Example 3), the self-corrosion potential of the alloy is Ecorr = -1.0052 V, and the self-corrosion current density is Icorr = 5.776 × 10 -4 A / cm 2 When the pulse voltage is 600 V (Example 4), the self-corrosion potential of the alloy is Ecorr = -1.3525 V, and the self-corrosion current density is Icorr = 1.537 × 10 -4A / cm 2 When the pulse voltage is 700 V (Example 5), the self-corrosion potential of the alloy is Ecorr = -1.3544 V, and the self-corrosion current density is Icorr = 1.629 × 10 -4 A / cm 2 .

[0073] In the Nyquist diagram, the smaller the impedance arc diameter is, the greater the corrosion rate is. Fig. 9 As shown in (b), when no electric pulse is applied (Comparative Example 1), the impedance arc diameter of the Al-Mg2Si alloy is a minimum of 1074, and when the electric pulse is 300V (Example 1), the impedance arc diameter is a maximum of 3007.

[0074] The electrochemical parameters of the alloy under different pulse voltages are shown in Table 4.

[0075] Table 4 Electrochemical parameters of alloys at different casting temperatures

[0076]

[0077] Fig.10 The three-dimensional morphology of the alloy after corrosion under different pulse voltages is mainly pitting. Among them, (a) is the average corrosion pit depth after electrochemical corrosion when it is untreated (Comparative Example 1), which is 18.646μm. (b) is the average corrosion pit depth after electrochemical corrosion when the pulse voltage is 300V (Example 1), which is 13.686μm. (c) is the average corrosion pit depth after electrochemical corrosion when the pulse voltage is 400V (Example 2), which is 14.172μm. (d) is the average corrosion pit depth after electrochemical corrosion when the pulse voltage is 500V (Example 3), which is 24.615μm. (e) is the average corrosion pit depth after electrochemical corrosion when the pulse voltage is 600V (Example 4), which is 15.722μm. (f) is the average corrosion pit depth after electrochemical corrosion when the pulse voltage is 300V (Example 5), which is 26.892μm. The average corrosion pit depth of the untreated sample after electrochemical corrosion is 18.646 μm, which is 1.36 times that when the pulse voltage is 300 V. It can be seen that the corrosion resistance is best when the pulse voltage is 300 V.

[0078] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for improving the structure and properties of a hypoeutectic Al-Mg2Si alloy, characterized in that: The hypoeutectic Al-Mg2Si alloy melt is subjected to electric pulse treatment; the process parameters of the electric pulse treatment are: pulse voltage of 300V to 700V, pulse frequency of 22Hz, and pulse treatment time of 30s.

2. The method for improving the structure and properties of hypoeutectic Al-Mg2Si alloy according to claim 1, characterized in that: In terms of mass percentage, the hypoeutectic Al-Mg2Si alloy melt contains 93% Al, 5% Mg and 2% Si.

3. The method for improving the structure and properties of hypoeutectic Al-Mg2Si alloy according to claim 1, characterized in that: When the temperature of the hypoeutectic Al-Mg2Si alloy melt is 720-750° C., electric pulse treatment is performed.

4. The method for improving the structure and properties of hypoeutectic Al-Mg2Si alloy according to claim 1, characterized in that: After the electric pulse treatment, the method further includes a step of keeping warm.

5. The method for improving the structure and properties of hypoeutectic Al-Mg2Si alloy according to claim 4, characterized in that: The insulation temperature is 740° C. and the insulation time is 5 minutes.

6. The method for improving the structure and properties of hypoeutectic Al-Mg2Si alloy according to claim 4, characterized in that: After the heat preservation is completed, a casting step is also included.

Citation Information

Patent Citations

  • Deterioration method for cast aluminum silicon magnesium automobile hub alloy

    CN107058819A

  • Treatment method for improving wear resistance and corrosion resistance of Al-Mg-Si alloy

    CN113278823A

  • Corrosion-resistant 5083 aluminum alloy and preparation method thereof

    CN115637359A

  • Aluminum alloy sheet having excellent pulse laser weldability

    JP2006104580A

  • A method for controlling the casting defect of Al-Si-Mg alloy through grain refinement and improving the cooling speed by using hydropulse

    KR1020130011208A

Cited By

  • Preparation method of metal material with multiphase heterostructure

    CN119501036A