Titanium alloy passivation solution and preparation method thereof
By using specific formulas of titanium alloy passivation fluid on the surface of titanium alloy, including modified glycidyl methacrylate and modified nanocellulose phosphate, the adhesion and resistance of the existing titanium alloy passivation fluid film are solved. The problem of insufficient corrosiveness achieves a more lasting protection effect.
Patent Information
- Application Number
- CN202411027365.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
AI Technical Summary
The existing titanium alloy passivation liquid has low adhesion, short protection time, and poor corrosion resistance in high temperature and high acid environments.
A combination formula of titanium alloy passivation solution is adopted, including inorganic salts, modified glycidyl methacrylate, modified nanocellulose phosphate, organic corrosion inhibitor, inorganic corrosion inhibitor, nanofiller, film forming additive, Preservatives and synergists are prepared by specific stirring and filtration steps, and the pH value is adjusted to improve adhesion and corrosion resistance of the membrane layer.
It significantly improves the adhesion between the film layer and the titanium alloy, extends the service life of the film layer, enhances the corrosion resistance in high temperature and high acid environments, and ensures the long-term anti-corrosion effect of the titanium alloy.
Smart Images

Figure CN118957559A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of titanium alloy passivation liquid, and in particular to a titanium alloy passivation liquid and a preparation method thereof. Background Art
[0002] Titanium alloy refers to a variety of alloy metals made of titanium and other metals. It is a structural metal with high strength, good corrosion resistance and high heat resistance. It is mainly used to manufacture aircraft engine compressor parts, followed by rockets, missiles and high-speed aircraft structural parts;
[0003] Passivation solution can make the metal surface passive. It is generally used for post-plating treatment of zinc plating, cadmium plating, titanium plating and other coatings. The purpose is to form a surface state on the coating surface that can prevent the normal reaction of the metal, improve its corrosion resistance, and increase the appearance of the product. After passivating the titanium alloy with titanium alloy passivation solution, a film layer will be formed on the titanium alloy, which can improve the corrosion resistance of the titanium alloy surface.
[0004] After the titanium alloy passivation solution in the prior art passivates the titanium alloy, the adhesion between the film layer formed on the surface of the titanium alloy and the titanium alloy is low, the film layer is easy to fall off from the titanium alloy, and the protection time of the film layer is not long-lasting, the corrosion protection time is short, and the service life is short. At the same time, under the use of high temperature and high acid, the corrosion inhibition performance of the film layer is poor. Therefore, it is urgent to design a titanium alloy passivation solution and a preparation method thereof to solve the above problems. Summary of the invention
[0005] The purpose of the present invention is to provide a titanium alloy passivation solution and a preparation method thereof to solve the above-mentioned deficiencies in the prior art.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] A titanium alloy passivation solution comprises the following components in parts by weight:
[0008] Inorganic salt: 13-45 parts;
[0009] Bisphenol A epoxy dipropionate: 15-26 parts;
[0010] Modified glycidyl methacrylate: 11-23 parts;
[0011] Modified phosphoric acid nanocellulose: 8-31 parts;
[0012] Organic corrosion inhibitor: 5-9 parts;
[0013] Inorganic corrosion inhibitor: 6-11 parts;
[0014] Nano filler: 4-17 parts;
[0015] Film-forming aid: 2-7 parts;
[0016] Preservatives: 10-35 parts;
[0017] Synergist: 1-10 parts;
[0018] Water: 10-100 parts.
[0019] Further, the modified glycidyl methacrylate comprises the following raw materials: tannic acid, glycidyl methacrylate water, hydroquinone and ethyl acetate;
[0020] The preparation steps of the modified glycidyl methacrylate are:
[0021] a. Mix and stir tannic acid, glycidyl methacrylate, water and hydroquinone in a mass ratio of 1:8:1:0.1 at a stirring speed of 100-200 r / min for 5-7 min;
[0022] b. The mixed solution obtained in step a is extracted with ethyl acetate and the upper organic phase is taken and subjected to reduced pressure rotary evaporation to obtain modified glycidyl methacrylate.
[0023] Furthermore, the modified phosphoric acid nanocellulose comprises the following raw materials: dried bamboo pulp paper, phosphoric acid, urea, water and sodium hydroxide;
[0024] The preparation steps of the modified phosphoric acid nanocellulose are:
[0025] a. The dried bamboo pulp paper is crushed and mixed with water, and the bamboo pulp mixture is treated using a homogenizer to obtain bamboo pulp;
[0026] b. The bamboo pulp, phosphoric acid, urea and water were mixed to obtain a bamboo pulp mixture, the bamboo pulp mixture was crushed by an ultrasonic crusher, and then diluted with water to obtain a bamboo pulp mixed suspension;
[0027] c. adding sodium hydroxide to the bamboo pulp mixed suspension to adjust the pH value of the bamboo pulp mixed suspension, then stirring and filtering to obtain a precipitate, and drying the precipitate to obtain modified phosphoric acid nanocellulose.
[0028] Furthermore, the nano filler is a mixture of nano silicon dioxide and nano zirconium oxide.
[0029] Furthermore, the preparation steps of the preservative are:
[0030] a. Mix water and polyvinyl alcohol and heat to 60°C, then cool naturally to room temperature, add polytetrafluoroethylene emulsion, and stir evenly to prepare a spinning soaking solution, electrospin the spinning soaking solution to obtain primary fibers, and sinter the primary fibers to obtain spinning fibers;
[0031] b. Dissolve chitosan, acetic acid solution, glycerol, glutaraldehyde and calcium chloride, mix them and stir them evenly to obtain a chitosan solution. Soak the spun fibers in a sodium alginate aqueous solution for 5-8 minutes to allow the spun fibers to be completely soaked in the sodium alginate aqueous solution. Take them out after soaking and dry them in the air. Spray the chitosan solution on the surface of the spun fibers. Then use hot air to dry the spun fibers. After drying, crush them to obtain a preservative.
[0032] Furthermore, the organic corrosion inhibitor is a mixture of hydroxyethylidene diphosphonic acid and diaminotriazole, and the mass ratio of hydroxyethylidene diphosphonic acid to diaminotriazole is 1.5:1.
[0033] Furthermore, the inorganic corrosion inhibitor is a mixture of potassium ferrate, potassium periodate and cerium nitrate, and the mass ratio of potassium ferrate, potassium periodate and cerium nitrate is 1:2:1.
[0034] Furthermore, the synergist is one of acetyl peroxide and didecyl peroxide.
[0035] Furthermore, the inorganic salt is a mixture of one or more of sodium silicate, potassium borate, potassium manganate, sodium bromate and sodium stannate.
[0036] In addition, a method for preparing a titanium alloy passivation solution, including the titanium alloy passivation solution, further includes the following preparation steps:
[0037] S1. Add bisphenol A epoxy dipropionate, modified glycidyl methacrylate, modified phosphoric acid nanocellulose and water into a mixing tank, mix and heat at a temperature of 55-90° C., a stirring rate of 130-260 r / min, and a stirring time of 1-2 h to obtain a mixed solution A;
[0038] S2, pour the inorganic salt into the mixed solution A obtained in S1, continue stirring for 25-45 minutes, and process with a homogenizer to obtain a mixed solution B;
[0039] S3, adding organic corrosion inhibitor, inorganic corrosion inhibitor, nanofiller, preservative and synergist to the mixed solution B obtained in S2 and stirring evenly, then slowly adding film-forming aid dropwise at a rate of 30 times per minute, stirring while adding the film-forming aid dropwise, and finally filtering to obtain a mixed solution C;
[0040] S4. Finally, sodium hydroxide is added to the mixed solution C to adjust the pH value of the mixed solution C to 6-7 to obtain a titanium alloy passivation solution.
[0041] In the above technical solution, the present invention provides a titanium alloy passivation solution and a preparation method thereof.
[0042] 1. By using the preservative, modified glycidyl methacrylate, and modified phosphoric acid nanocellulose, the preservative is made of chitosan-coated polytetrafluoroethylene fiber. With the use of titanium alloy, the chitosan on the film layer is continuously degraded. With the reduction of chitosan, the polytetrafluoroethylene fiber coated inside it will be released, and the polytetrafluoroethylene fiber has strong corrosion resistance, which can increase the long-term corrosion resistance of the film layer and has a long service life. The modified glycidyl methacrylate is used to improve the resin compatibility of tannic acid. The modified phosphoric acid nanocellulose obtained by using bamboo pulp has low reaction conditions, is safer, pollution-free, and more environmentally friendly. The combination of modified glycidyl methacrylate and modified phosphoric acid nanocellulose can greatly improve the adhesion between the film layer and the titanium alloy, making it difficult for the film layer to fall off from the titanium alloy;
[0043] 2. By using organic corrosion inhibitors, inorganic corrosion inhibitors, and nanofillers, the inorganic corrosion inhibitor can quickly form a skeleton on the surface of the titanium alloy, and the organic corrosion inhibitor is used to form a film layer on the surface and in the gaps of the skeleton, and then the film-forming additive is used to fill it, so as to build a firm protective layer, enhance the corrosion inhibition performance of the film layer, and thus improve the corrosion inhibition performance of the titanium alloy;
[0044] 3. By adopting inorganic salts and enhancers, the passivation film layer with added inorganic salts can effectively block the contact between highly acidic liquid and titanium alloy, thereby being able to inhibit the corrosion of highly acidic liquid to titanium alloy. Because titanium alloy reacts violently and dissolves quickly in a high-temperature and high-acid environment, the enhancer can promote the rapid formation of the passivation film layer with added inorganic salts on the surface of the titanium alloy, thereby improving the density and integrity of the film layer, thereby being able to improve the corrosion resistance of the titanium alloy in a high-temperature and high-acid environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can also be obtained based on these drawings.
[0046] Figure 1 A schematic diagram of the preparation steps of a titanium alloy passivation solution and a preparation method thereof provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0047] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention will be further described in detail below with reference to the accompanying drawings.
[0048] like Figure 1 As shown, a titanium alloy passivation solution provided in an embodiment of the present invention comprises the following components in parts by weight:
[0049] Inorganic salt: 13 parts;
[0050] Bisphenol A epoxy dipropionate: 15 parts;
[0051] Modified glycidyl methacrylate: 11 parts;
[0052] Modified phosphoric acid nanocellulose: 8 parts;
[0053] Organic corrosion inhibitor: 5 parts;
[0054] Inorganic corrosion inhibitor: 8 parts;
[0055] Nano filler: 7 parts;
[0056] Film-forming aid: 2 parts;
[0057] Preservatives: 10 parts;
[0058] Synergist: 1 part;
[0059] Water: 20 parts.
[0060] In one embodiment provided by the present invention, the modified glycidyl methacrylate comprises the following raw materials: tannic acid, glycidyl methacrylate water, hydroquinone and ethyl acetate;
[0061] The preparation steps of modified glycidyl methacrylate are:
[0062] a. Mix and stir tannic acid, glycidyl methacrylate, water and hydroquinone in a mass ratio of 1:8:1:0.1 at a stirring speed of 100 r / min for 5 min;
[0063] b. Extract the mixed solution obtained in step a with ethyl acetate and take the upper organic phase, and evaporate under reduced pressure to obtain modified glycidyl methacrylate;
[0064] Modified glycidyl methacrylate improves the resin compatibility of tannic acid.
[0065] In another embodiment provided by the present invention, the modified phosphoric acid nanocellulose comprises the following raw materials: dried bamboo pulp paper, phosphoric acid, urea, water and sodium hydroxide;
[0066] The preparation steps of modified phosphoric acid nanocellulose are as follows:
[0067] a. The dried bamboo pulp paper is crushed and mixed with water, and the bamboo pulp mixture is treated using a homogenizer to obtain bamboo pulp;
[0068] b. The bamboo pulp, phosphoric acid, urea and water were mixed to obtain a bamboo pulp mixture, the bamboo pulp mixture was crushed by an ultrasonic crusher, and then diluted with water to obtain a bamboo pulp mixed suspension;
[0069] c. adding sodium hydroxide to the bamboo pulp mixed suspension, adjusting the pH value of the bamboo pulp mixed suspension, and then stirring and filtering to obtain a precipitate, and drying the precipitate to obtain modified phosphate nanocellulose;
[0070] The modified phosphate nanocellulose obtained from bamboo pulp has low reaction condition requirements, is safer, pollution-free, and more environmentally friendly. The combination of modified glycidyl methacrylate and modified phosphate nanocellulose can greatly enhance the adhesion between the film layer and the titanium alloy, making it difficult for the film layer to fall off the titanium alloy.
[0071] In another embodiment provided by the present invention, the nano filler is a mixture of nano silicon dioxide and nano zirconium oxide.
[0072] In one embodiment provided by the present invention, the steps for preparing the preservative are:
[0073] a. Mix water and polyvinyl alcohol and heat to 60°C, then cool naturally to room temperature, add polytetrafluoroethylene emulsion, and stir evenly to prepare a spinning soaking solution, electrospin the spinning soaking solution to obtain primary fibers, and sinter the primary fibers to obtain spinning fibers;
[0074] b. Dissolve chitosan, acetic acid, glycerol, glutaraldehyde and calcium chloride, mix and stir to obtain a chitosan solution, soak the spun fiber in an aqueous sodium alginate solution for 5 minutes, so that the spun fiber is completely soaked in the aqueous sodium alginate solution, take out and dry after soaking, and then spray the chitosan solution on the surface of the spun fiber, and then use hot air to dry the spun fiber, and then crush it after drying to obtain a preservative;
[0075] With the use of titanium alloy, the chitosan on the membrane layer continues to degrade. As the chitosan decreases, the polytetrafluoroethylene fiber coated inside it will be released. The polytetrafluoroethylene fiber has strong corrosion resistance, which can increase the long-term anti-corrosion effect of the membrane layer and prolong its service life.
[0076] In another embodiment provided by the present invention, the organic corrosion inhibitor is a mixture of hydroxyethylidene diphosphonic acid and diaminotriazole, and the mass ratio of hydroxyethylidene diphosphonic acid to diaminotriazole is 1.5:1. The inorganic corrosion inhibitor can quickly form a skeleton on the surface of the titanium alloy. The organic corrosion inhibitor is used to form a film layer on the surface and in the gaps of the skeleton, and then the film-forming aid is used for filling. A strong protective layer can be constructed, which can enhance the corrosion inhibition performance of the film layer, and thus improve the corrosion inhibition performance of the titanium alloy.
[0077] In another embodiment provided by the present invention, the inorganic corrosion inhibitor is a mixture of potassium ferrate, potassium periodate and cerium nitrate, and the mass ratio of potassium ferrate, potassium periodate and cerium nitrate is 1:2:1.
[0078] In one embodiment provided by the present invention, the enhancer is one of acetyl peroxide and didecanoyl peroxide. Because titanium alloy reacts violently and dissolves quickly in a high-temperature and high-acid use environment, the enhancer can promote the rapid formation of a passivation film layer of inorganic salt added on the surface of the titanium alloy, which can improve the density and integrity of the film layer, and thus improve the corrosion resistance of the titanium alloy in a high-temperature and high-acid use environment.
[0079] In another embodiment provided by the present invention, the inorganic salt is a mixture of one or more of sodium silicate, potassium borate, potassium manganate, sodium bromate, and sodium stannate. The passivation film layer of the inorganic salt can effectively block the contact between the highly acidic solution and the titanium alloy, thereby being able to inhibit the corrosion of the titanium alloy by the highly acidic solution.
[0080] In addition, a method for preparing a titanium alloy passivation solution, including the titanium alloy passivation solution, further includes the following preparation steps:
[0081] S1, adding bisphenol A epoxy dipropionate, modified glycidyl methacrylate, modified phosphoric acid nanocellulose and water into a mixing tank, mixing, and heating at a temperature of 55° C., a stirring rate of 130 r / min, and a stirring time of 1 h to obtain a mixed solution A;
[0082] S2, pour the inorganic salt into the mixed solution A obtained in S1, continue stirring for 25 minutes, and treat with a homogenizer to obtain a mixed solution B;
[0083] S3, adding organic corrosion inhibitor, inorganic corrosion inhibitor, nanofiller, preservative and synergist to the mixed solution B obtained in S2 and stirring evenly, then slowly adding film-forming aid dropwise at a rate of 30 times per minute, stirring while adding the film-forming aid dropwise, and finally filtering to obtain a mixed solution C;
[0084] S4. Finally, sodium hydroxide is added to the mixed solution C to adjust the pH value of the mixed solution C to 6 to obtain a titanium alloy passivation solution.
[0085] Embodiment 1
[0086] A titanium alloy passivation solution comprises the following components in parts by weight:
[0087] Inorganic salt: 14 parts;
[0088] Bisphenol A epoxy dipropionate: 14 parts;
[0089] Modified glycidyl methacrylate: 13 parts;
[0090] Modified phosphoric acid nanocellulose: 9 parts;
[0091] Organic corrosion inhibitor: 7 parts;
[0092] Inorganic corrosion inhibitor: 8 parts;
[0093] Nano filler: 6 parts;
[0094] Film-forming aid: 3 parts;
[0095] Preservatives: 12 parts;
[0096] Enhancer: 2 parts;
[0097] Water: 13 parts.
[0098] In one embodiment provided by the present invention, the modified glycidyl methacrylate comprises the following raw materials: tannic acid, glycidyl methacrylate water, hydroquinone and ethyl acetate;
[0099] The preparation steps of modified glycidyl methacrylate are:
[0100] a. Mix and stir tannic acid, glycidyl methacrylate, water and hydroquinone in a mass ratio of 1:8:1:0.1 at a stirring speed of 130 r / min for 6 min;
[0101] b. Extract the mixed solution obtained in step a with ethyl acetate and take the upper organic phase, and evaporate under reduced pressure to obtain modified glycidyl methacrylate;
[0102] Modified glycidyl methacrylate improves the resin compatibility of tannic acid.
[0103] In another embodiment provided by the present invention, the modified phosphoric acid nanocellulose comprises the following raw materials: dried bamboo pulp paper, phosphoric acid, urea, water and sodium hydroxide;
[0104] The preparation steps of modified phosphoric acid nanocellulose are as follows:
[0105] a. The dried bamboo pulp paper is crushed and mixed with water, and the bamboo pulp mixture is treated using a homogenizer to obtain bamboo pulp;
[0106] b. The bamboo pulp, phosphoric acid, urea and water were mixed to obtain a bamboo pulp mixture, the bamboo pulp mixture was crushed by an ultrasonic crusher, and then diluted with water to obtain a bamboo pulp mixed suspension;
[0107] c. adding sodium hydroxide to the bamboo pulp mixed suspension, adjusting the pH value of the bamboo pulp mixed suspension, and then stirring and filtering to obtain a precipitate, and drying the precipitate to obtain modified phosphate nanocellulose;
[0108] The modified phosphate nanocellulose obtained from bamboo pulp has low reaction condition requirements, is safer, pollution-free, and more environmentally friendly. The combination of modified glycidyl methacrylate and modified phosphate nanocellulose can greatly enhance the adhesion between the film layer and the titanium alloy, making it difficult for the film layer to fall off the titanium alloy.
[0109] In another embodiment provided by the present invention, the nano filler is a mixture of nano silicon dioxide and nano zirconium oxide.
[0110] In one embodiment provided by the present invention, the steps for preparing the preservative are:
[0111] a. Mix water and polyvinyl alcohol and heat to 60°C, then cool naturally to room temperature, add polytetrafluoroethylene emulsion, and stir evenly to prepare a spinning soaking solution, electrospin the spinning soaking solution to obtain primary fibers, and sinter the primary fibers to obtain spinning fibers;
[0112] b. Dissolve chitosan, acetic acid, glycerol, glutaraldehyde and calcium chloride, mix and stir to obtain a chitosan solution, soak the spun fiber in an aqueous solution of sodium alginate for 6 minutes, so that the spun fiber is completely soaked in the aqueous solution of sodium alginate, take out and dry after soaking, and then spray the chitosan solution on the surface of the spun fiber, and then use hot air to dry the spun fiber, and then crush it after drying to obtain a preservative;
[0113] With the use of titanium alloy, the chitosan on the membrane layer continues to degrade. As the chitosan decreases, the polytetrafluoroethylene fiber coated inside it will be released. The polytetrafluoroethylene fiber has strong corrosion resistance, which can increase the long-term anti-corrosion effect of the membrane layer and prolong its service life.
[0114] In another embodiment provided by the present invention, the organic corrosion inhibitor is a mixture of hydroxyethylidene diphosphonic acid and diaminotriazole, and the mass ratio of hydroxyethylidene diphosphonic acid to diaminotriazole is 1.5:1. The inorganic corrosion inhibitor can quickly form a skeleton on the surface of the titanium alloy. The organic corrosion inhibitor is used to form a film layer on the surface and in the gaps of the skeleton, and then the film-forming aid is used for filling. A strong protective layer can be constructed, which can enhance the corrosion inhibition performance of the film layer, and thus improve the corrosion inhibition performance of the titanium alloy.
[0115] In another embodiment provided by the present invention, the inorganic corrosion inhibitor is a mixture of potassium ferrate, potassium periodate and cerium nitrate, and the mass ratio of potassium ferrate, potassium periodate and cerium nitrate is 1:2:1.
[0116] In one embodiment provided by the present invention, the enhancer is one of acetyl peroxide and didecanoyl peroxide. Because titanium alloy reacts violently and dissolves quickly in a high-temperature and high-acid use environment, the enhancer can promote the rapid formation of a passivation film layer of inorganic salt added on the surface of the titanium alloy, which can improve the density and integrity of the film layer, and thus improve the corrosion resistance of the titanium alloy in a high-temperature and high-acid use environment.
[0117] In another embodiment provided by the present invention, the inorganic salt is a mixture of one or more of sodium silicate, potassium borate, potassium manganate, sodium bromate, and sodium stannate. The passivation film layer of the inorganic salt can effectively block the contact between the highly acidic solution and the titanium alloy, thereby being able to inhibit the corrosion of the titanium alloy by the highly acidic solution.
[0118] A method for preparing a titanium alloy passivation solution comprises the following preparation steps:
[0119] S1, adding bisphenol A epoxy dipropionate, modified glycidyl methacrylate, modified phosphoric acid nanocellulose and water into a mixing tank, mixing, and heating at a temperature of 65° C., a stirring rate of 160 r / min, and a stirring time of 1.3 h to obtain a mixed solution A;
[0120] S2, pour the inorganic salt into the mixed solution A obtained in S1, continue stirring for 35 minutes, and treat with a homogenizer to obtain a mixed solution B;
[0121] S3, adding organic corrosion inhibitor, inorganic corrosion inhibitor, nanofiller, preservative and synergist to the mixed solution B obtained in S2 and stirring evenly, then slowly adding film-forming aid dropwise at a rate of 30 times per minute, stirring while adding the film-forming aid dropwise, and finally filtering to obtain a mixed solution C;
[0122] S4. Finally, sodium hydroxide is added to the mixed solution C to adjust the pH value of the mixed solution C to 6 to obtain a titanium alloy passivation solution.
[0123] Embodiment 2
[0124] A titanium alloy passivation solution comprises the following components in parts by weight:
[0125] Inorganic salt: 13 parts;
[0126] Bisphenol A epoxy dipropionate: 14 parts;
[0127] Modified glycidyl methacrylate: 12 parts;
[0128] Modified phosphoric acid nanocellulose: 11 parts;
[0129] Organic corrosion inhibitor: 6 parts;
[0130] Inorganic corrosion inhibitor: 6 parts;
[0131] Nano filler: 9 parts;
[0132] Film-forming aid: 2 parts;
[0133] Preservatives: 13 parts;
[0134] Synergist: 4 parts;
[0135] Water: 10 parts.
[0136] In one embodiment provided by the present invention, the modified glycidyl methacrylate comprises the following raw materials: tannic acid, glycidyl methacrylate water, hydroquinone and ethyl acetate;
[0137] The preparation steps of modified glycidyl methacrylate are:
[0138] a. Mix and stir tannic acid, glycidyl methacrylate, water and hydroquinone in a mass ratio of 1:8:1:0.1 at a stirring speed of 170 r / min for 6 min;
[0139] b. Extract the mixed solution obtained in step a with ethyl acetate and take the upper organic phase, and evaporate under reduced pressure to obtain modified glycidyl methacrylate;
[0140] Modified glycidyl methacrylate improves the resin compatibility of tannic acid.
[0141] In another embodiment provided by the present invention, the modified phosphoric acid nanocellulose comprises the following raw materials: dried bamboo pulp paper, phosphoric acid, urea, water and sodium hydroxide;
[0142] The preparation steps of modified phosphoric acid nanocellulose are as follows:
[0143] a. The dried bamboo pulp paper is crushed and mixed with water, and the bamboo pulp mixture is treated using a homogenizer to obtain bamboo pulp;
[0144] b. The bamboo pulp, phosphoric acid, urea and water were mixed to obtain a bamboo pulp mixture, the bamboo pulp mixture was crushed by an ultrasonic crusher, and then diluted with water to obtain a bamboo pulp mixed suspension;
[0145] c. adding sodium hydroxide to the bamboo pulp mixed suspension, adjusting the pH value of the bamboo pulp mixed suspension, and then stirring and filtering to obtain a precipitate, and drying the precipitate to obtain modified phosphate nanocellulose;
[0146] The modified phosphate nanocellulose obtained from bamboo pulp has low reaction condition requirements, is safer, pollution-free, and more environmentally friendly. The combination of modified glycidyl methacrylate and modified phosphate nanocellulose can greatly enhance the adhesion between the film layer and the titanium alloy, making it difficult for the film layer to fall off the titanium alloy.
[0147] In another embodiment provided by the present invention, the nano filler is a mixture of nano silicon dioxide and nano zirconium oxide.
[0148] In one embodiment provided by the present invention, the steps for preparing the preservative are:
[0149] a. Mix water and polyvinyl alcohol and heat to 60°C, then cool naturally to room temperature, add polytetrafluoroethylene emulsion, and stir evenly to prepare a spinning soaking solution, electrospin the spinning soaking solution to obtain primary fibers, and sinter the primary fibers to obtain spinning fibers;
[0150] b. Dissolve chitosan, acetic acid, glycerol, glutaraldehyde and calcium chloride, mix and stir to obtain a chitosan solution, soak the spun fiber in an aqueous solution of sodium alginate for 7 minutes, so that the spun fiber is completely soaked in the aqueous solution of sodium alginate, take out and dry after soaking, and then spray the chitosan solution on the surface of the spun fiber, and then use hot air to dry the spun fiber, and then crush it after drying to obtain a preservative;
[0151] With the use of titanium alloy, the chitosan on the membrane layer continues to degrade. As the chitosan decreases, the polytetrafluoroethylene fiber coated inside it will be released. The polytetrafluoroethylene fiber has strong corrosion resistance, which can increase the long-term anti-corrosion effect of the membrane layer and prolong its service life.
[0152] In another embodiment provided by the present invention, the organic corrosion inhibitor is a mixture of hydroxyethylidene diphosphonic acid and diaminotriazole, and the mass ratio of hydroxyethylidene diphosphonic acid to diaminotriazole is 1.5:1. The inorganic corrosion inhibitor can quickly form a skeleton on the surface of the titanium alloy. The organic corrosion inhibitor is used to form a film layer on the surface and in the gaps of the skeleton, and then the film-forming aid is used for filling. A strong protective layer can be constructed, which can enhance the corrosion inhibition performance of the film layer, and thus improve the corrosion inhibition performance of the titanium alloy.
[0153] In another embodiment provided by the present invention, the inorganic corrosion inhibitor is a mixture of potassium ferrate, potassium periodate and cerium nitrate, and the mass ratio of potassium ferrate, potassium periodate and cerium nitrate is 1:2:1.
[0154] In one embodiment provided by the present invention, the enhancer is one of acetyl peroxide and didecanoyl peroxide. Because titanium alloy reacts violently and dissolves quickly in a high-temperature and high-acid use environment, the enhancer can promote the rapid formation of a passivation film layer of inorganic salt added on the surface of the titanium alloy, which can improve the density and integrity of the film layer, and thus improve the corrosion resistance of the titanium alloy in a high-temperature and high-acid use environment.
[0155] In another embodiment provided by the present invention, the inorganic salt is a mixture of one or more of sodium silicate, potassium borate, potassium manganate, sodium bromate, and sodium stannate. The passivation film layer of the inorganic salt can effectively block the contact between the highly acidic solution and the titanium alloy, thereby being able to inhibit the corrosion of the titanium alloy by the highly acidic solution.
[0156] A method for preparing a titanium alloy passivation solution comprises the following preparation steps:
[0157] S1, adding bisphenol A epoxy dipropionate, modified glycidyl methacrylate, modified phosphoric acid nanocellulose and water into a mixing tank, mixing, and heating at 80° C., stirring at a rate of 200 r / min, and stirring for 1.6 h to obtain a mixed solution A;
[0158] S2, pour the inorganic salt into the mixed solution A obtained in S1, continue stirring for 40 minutes, and treat with a homogenizer to obtain a mixed solution B;
[0159] S3, adding organic corrosion inhibitor, inorganic corrosion inhibitor, nanofiller, preservative and synergist to the mixed solution B obtained in S2 and stirring evenly, then slowly adding film-forming aid dropwise at a rate of 30 times per minute, stirring while adding the film-forming aid dropwise, and finally filtering to obtain a mixed solution C;
[0160] S4. Finally, sodium hydroxide is added to the mixed solution C to adjust the pH value of the mixed solution C to 7 to obtain a titanium alloy passivation solution.
[0161] Embodiment 3
[0162] A titanium alloy passivation solution comprises the following components in parts by weight:
[0163] Inorganic salt: 15 parts;
[0164] Bisphenol A epoxy dipropionate: 13 parts;
[0165] Modified glycidyl methacrylate: 14 parts;
[0166] Modified phosphoric acid nanocellulose: 7 parts;
[0167] Organic corrosion inhibitor: 6 parts;
[0168] Inorganic corrosion inhibitor: 7 parts;
[0169] Nano filler: 5 parts;
[0170] Film-forming aid: 4 parts;
[0171] Preservatives: 16 parts;
[0172] Enhancer: 2 parts;
[0173] Water: 11 parts.
[0174] In one embodiment provided by the present invention, the modified glycidyl methacrylate comprises the following raw materials: tannic acid, glycidyl methacrylate water, hydroquinone and ethyl acetate;
[0175] The preparation steps of modified glycidyl methacrylate are:
[0176] a. Mix and stir tannic acid, glycidyl methacrylate, water and hydroquinone in a mass ratio of 1:8:1:0.1 at a stirring speed of 200 r / min for 7 min;
[0177] b. Extract the mixed solution obtained in step a with ethyl acetate and take the upper organic phase, and evaporate under reduced pressure to obtain modified glycidyl methacrylate;
[0178] Modified glycidyl methacrylate improves the resin compatibility of tannic acid.
[0179] In another embodiment provided by the present invention, the modified phosphoric acid nanocellulose comprises the following raw materials: dried bamboo pulp paper, phosphoric acid, urea, water and sodium hydroxide;
[0180] The preparation steps of modified phosphoric acid nanocellulose are as follows:
[0181] a. The dried bamboo pulp paper is crushed and mixed with water, and the bamboo pulp mixture is treated using a homogenizer to obtain bamboo pulp;
[0182] b. The bamboo pulp, phosphoric acid, urea and water were mixed to obtain a bamboo pulp mixture, the bamboo pulp mixture was crushed by an ultrasonic crusher, and then diluted with water to obtain a bamboo pulp mixed suspension;
[0183] c. adding sodium hydroxide to the bamboo pulp mixed suspension, adjusting the pH value of the bamboo pulp mixed suspension, and then stirring and filtering to obtain a precipitate, and drying the precipitate to obtain modified phosphate nanocellulose;
[0184] The modified phosphate nanocellulose obtained from bamboo pulp has low reaction condition requirements, is safer, pollution-free, and more environmentally friendly. The combination of modified glycidyl methacrylate and modified phosphate nanocellulose can greatly enhance the adhesion between the film layer and the titanium alloy, making it difficult for the film layer to fall off the titanium alloy.
[0185] In another embodiment provided by the present invention, the nano filler is a mixture of nano silicon dioxide and nano zirconium oxide.
[0186] In one embodiment provided by the present invention, the steps for preparing the preservative are:
[0187] a. Mix water and polyvinyl alcohol and heat to 60°C, then cool naturally to room temperature, add polytetrafluoroethylene emulsion, and stir evenly to prepare a spinning soaking solution, electrospin the spinning soaking solution to obtain primary fibers, and sinter the primary fibers to obtain spinning fibers;
[0188] b. Dissolve chitosan, acetic acid, glycerol, glutaraldehyde and calcium chloride, mix and stir to obtain a chitosan solution, soak the spun fiber in an aqueous solution of sodium alginate for 8 minutes, so that the spun fiber is completely soaked in the aqueous solution of sodium alginate, take out and dry after soaking, and then spray the chitosan solution on the surface of the spun fiber, and then use hot air to dry the spun fiber, and then crush it after drying to obtain a preservative;
[0189] With the use of titanium alloy, the chitosan on the membrane layer continues to degrade. As the chitosan decreases, the polytetrafluoroethylene fiber coated inside it will be released. The polytetrafluoroethylene fiber has strong corrosion resistance, which can increase the long-term anti-corrosion effect of the membrane layer and prolong its service life.
[0190] In another embodiment provided by the present invention, the organic corrosion inhibitor is a mixture of hydroxyethylidene diphosphonic acid and diaminotriazole, and the mass ratio of hydroxyethylidene diphosphonic acid to diaminotriazole is 1.5:1. The inorganic corrosion inhibitor can quickly form a skeleton on the surface of the titanium alloy. The organic corrosion inhibitor is used to form a film layer on the surface and in the gaps of the skeleton, and then the film-forming aid is used for filling. A strong protective layer can be constructed, which can enhance the corrosion inhibition performance of the film layer, and thus improve the corrosion inhibition performance of the titanium alloy.
[0191] In another embodiment provided by the present invention, the inorganic corrosion inhibitor is a mixture of potassium ferrate, potassium periodate and cerium nitrate, and the mass ratio of potassium ferrate, potassium periodate and cerium nitrate is 1:2:1.
[0192] In one embodiment provided by the present invention, the enhancer is one of acetyl peroxide and didecanoyl peroxide. Because titanium alloy reacts violently and dissolves quickly in a high-temperature and high-acid use environment, the enhancer can promote the rapid formation of a passivation film layer of inorganic salt added on the surface of the titanium alloy, which can improve the density and integrity of the film layer, and thus improve the corrosion resistance of the titanium alloy in a high-temperature and high-acid use environment.
[0193] In another embodiment provided by the present invention, the inorganic salt is a mixture of one or more of sodium silicate, potassium borate, potassium manganate, sodium bromate, and sodium stannate. The passivation film layer of the inorganic salt can effectively block the contact between the highly acidic solution and the titanium alloy, thereby being able to inhibit the corrosion of the titanium alloy by the highly acidic solution.
[0194] A method for preparing a titanium alloy passivation solution, comprising the titanium alloy passivation solution, and further comprising the following preparation steps:
[0195] S1, adding bisphenol A epoxy dipropionate, modified glycidyl methacrylate, modified phosphoric acid nanocellulose and water into a mixing tank, mixing, and heating at 90° C., stirring at a rate of 260 r / min, and stirring for 2 h to obtain a mixed solution A;
[0196] S2, pour the inorganic salt into the mixed solution A obtained in S1, continue stirring for 45 minutes, and treat with a homogenizer to obtain a mixed solution B;
[0197] S3, adding organic corrosion inhibitor, inorganic corrosion inhibitor, nanofiller, preservative and synergist to the mixed solution B obtained in S2 and stirring evenly, then slowly adding film-forming aid dropwise at a rate of 30 times per minute, stirring while adding the film-forming aid dropwise, and finally filtering to obtain a mixed solution C;
[0198] S4. Finally, sodium hydroxide is added to the mixed solution C to adjust the pH value of the mixed solution C to 7 to obtain a titanium alloy passivation solution.
[0199] Working principle:
[0200] (1) first preparing modified glycidyl methacrylate, modified phosphoric acid nanocellulose and a preservative;
[0201] Modified glycidyl methacrylate, the preparation steps are:
[0202] a. Mix and stir tannic acid, glycidyl methacrylate, water and hydroquinone in a mass ratio of 1:8:1:0.1 at a stirring speed of 100-200 r / min for 5-7 min;
[0203] b. Extract the mixed solution obtained in step a with ethyl acetate and take the upper organic phase, and evaporate under reduced pressure to obtain modified glycidyl methacrylate;
[0204] The preparation steps of modified phosphoric acid nanocellulose are as follows:
[0205] a. The dried bamboo pulp paper is crushed and mixed with water, and the bamboo pulp mixture is treated using a homogenizer to obtain bamboo pulp;
[0206] b. The bamboo pulp, phosphoric acid, urea and water were mixed to obtain a bamboo pulp mixture, the bamboo pulp mixture was crushed by an ultrasonic crusher, and then diluted with water to obtain a bamboo pulp mixed suspension;
[0207] c. adding sodium hydroxide to the bamboo pulp mixed suspension, adjusting the pH value of the bamboo pulp mixed suspension, and then stirring and filtering to obtain a precipitate, and drying the precipitate to obtain modified phosphate nanocellulose;
[0208] The preparation steps of the preservative are:
[0209] a. Mix water and polyvinyl alcohol and heat to 60°C, then cool naturally to room temperature, add polytetrafluoroethylene emulsion, and stir evenly to prepare a spinning soaking solution, electrospin the spinning soaking solution to obtain primary fibers, and sinter the primary fibers to obtain spinning fibers;
[0210] b. Dissolve chitosan, acetic acid, glycerol, glutaraldehyde and calcium chloride, mix and stir to obtain a chitosan solution, soak the spun fiber in an aqueous solution of sodium alginate for 5-8 minutes, so that the spun fiber is completely soaked in the aqueous solution of sodium alginate, take out and dry after soaking, spray the chitosan solution on the surface of the spun fiber, and then use hot air to dry the spun fiber, and then crush it after drying to obtain a preservative;
[0211] (2) Then prepare the titanium alloy passivation solution, including the following preparation steps:
[0212] S1. Add bisphenol A epoxy dipropionate, modified glycidyl methacrylate, modified phosphoric acid nanocellulose and water into a mixing tank, mix and heat at a temperature of 55-90° C., a stirring rate of 130-260 r / min, and a stirring time of 1-2 h to obtain a mixed solution A;
[0213] S2, pour the inorganic salt into the mixed solution A obtained in S1, continue stirring for 25-45 minutes, and process with a homogenizer to obtain a mixed solution B;
[0214] S3, adding organic corrosion inhibitor, inorganic corrosion inhibitor, nanofiller, preservative and synergist to the mixed solution B obtained in S2 and stirring evenly, then slowly adding film-forming aid dropwise at a rate of 30 times per minute, stirring while adding the film-forming aid dropwise, and finally filtering to obtain a mixed solution C;
[0215] S4. Finally, sodium hydroxide is added to the mixed solution C to adjust the pH value of the mixed solution C to 6-7 to obtain a titanium alloy passivation solution.
[0216] The above description is only by way of illustration of certain exemplary embodiments of the present invention. It is undoubted that those skilled in the art can modify the described embodiments in various ways without departing from the spirit and scope of the present invention. Therefore, the above drawings and descriptions are illustrative in nature and should not be construed as limiting the scope of protection of the claims of the present invention.
Claims
1. A titanium alloy passivation solution, It is characterized in that The composition comprises the following components in parts by weight: Inorganic salt: 13-45 parts; Bisphenol A epoxy dipropionate: 15-26 parts; Modified glycidyl methacrylate: 11-23 parts; Modified phosphoric acid nanocellulose: 8-31 parts; Organic corrosion inhibitor: 5-9 parts; Inorganic corrosion inhibitor: 6-11 parts; Nano filler: 4-17 parts; Film-forming aid: 2-7 parts; Preservatives: 10-35 parts; Synergist: 1-10 parts; Water: 10-100 parts.
2. A titanium alloy passivation solution according to claim 1, It is characterized in that The modified glycidyl methacrylate comprises the following raw materials: tannic acid, glycidyl methacrylate water, hydroquinone and ethyl acetate; The preparation steps of the modified glycidyl methacrylate are: a. Mix and stir tannic acid, glycidyl methacrylate, water and hydroquinone in a mass ratio of 1:8:1:0.1 at a stirring speed of 100-200 r / min for 5-7 min; b. The mixed solution obtained in step a is extracted with ethyl acetate and the upper organic phase is taken and subjected to reduced pressure rotary evaporation to obtain modified glycidyl methacrylate.
3. A titanium alloy passivation solution according to claim 1, It is characterized in that The modified phosphoric acid nanocellulose comprises the following raw materials: dried bamboo pulp paper, phosphoric acid, urea, water and sodium hydroxide; The preparation steps of the modified phosphoric acid nanocellulose are: a. The dried bamboo pulp paper is crushed and mixed with water, and the bamboo pulp mixture is treated using a homogenizer to obtain bamboo pulp; b. The bamboo pulp, phosphoric acid, urea and water were mixed to obtain a bamboo pulp mixture, the bamboo pulp mixture was crushed by an ultrasonic crusher, and then diluted with water to obtain a bamboo pulp mixed suspension; c. adding sodium hydroxide to the bamboo pulp mixed suspension to adjust the pH value of the bamboo pulp mixed suspension, then stirring and filtering to obtain a precipitate, and drying the precipitate to obtain modified phosphoric acid nanocellulose.
4. A titanium alloy passivation solution according to claim 1, It is characterized in that The nano filler is a mixture of nano silicon dioxide and nano zirconium oxide.
5. A titanium alloy passivation solution according to claim 1, It is characterized in that The preparation steps of the preservative are: a. Mix water and polyvinyl alcohol and heat to 60°C, then cool naturally to room temperature, add polytetrafluoroethylene emulsion, and stir evenly to prepare a spinning soaking solution, electrospin the spinning soaking solution to obtain primary fibers, and sinter the primary fibers to obtain spinning fibers; b. Dissolve chitosan, acetic acid solution, glycerol, glutaraldehyde and calcium chloride, mix them and stir them evenly to obtain a chitosan solution. Soak the spun fibers in a sodium alginate aqueous solution for 5-8 minutes to allow the spun fibers to be completely soaked in the sodium alginate aqueous solution. Take them out after soaking and dry them in the air. Spray the chitosan solution on the surface of the spun fibers. Then use hot air to dry the spun fibers. After drying, crush them to obtain a preservative.
6. A titanium alloy passivation solution according to claim 1, It is characterized in that The organic corrosion inhibitor is a mixture of hydroxyethylidene diphosphonic acid and diaminotriazole, and the mass ratio of hydroxyethylidene diphosphonic acid to diaminotriazole is 1.5:
1.
7. A titanium alloy passivation solution according to claim 1, It is characterized in that The inorganic corrosion inhibitor is a mixture of potassium ferrate, potassium periodate and cerium nitrate, and the mass ratio of potassium ferrate, potassium periodate and cerium nitrate is 1:2:
1.
8. A titanium alloy passivation solution according to claim 1, It is characterized in that The synergist is one of acetyl peroxide and didecyl peroxide.
9. A titanium alloy passivation solution according to claim 1, It is characterized in that The inorganic salt is a mixture of one or more of sodium silicate, potassium borate, potassium manganate, sodium bromate and sodium stannate.
10. A method for preparing a titanium alloy passivation solution, comprising the titanium alloy passivation solution according to any one of claims 1 to 9, It is characterized in that The method comprises the following preparation steps: S1. Add bisphenol A epoxy dipropionate, modified glycidyl methacrylate, modified phosphoric acid nanocellulose and water into a mixing tank, mix and heat at a temperature of 55-90° C., a stirring rate of 130-260 r / min, and a stirring time of 1-2 h to obtain a mixed solution A; S2, pour the inorganic salt into the mixed solution A obtained in S1, continue stirring for 25-45 minutes, and process with a homogenizer to obtain a mixed solution B; S3, adding organic corrosion inhibitor, inorganic corrosion inhibitor, nanofiller, preservative and synergist to the mixed solution B obtained in S2 and stirring evenly, then slowly adding film-forming aid dropwise at a rate of 30 times per minute, stirring while adding the film-forming aid dropwise, and finally filtering to obtain a mixed solution C; S4. Finally, sodium hydroxide is added to the mixed solution C to adjust the pH value of the mixed solution C to 6-7 to obtain a titanium alloy passivation solution.