Vanadium electrolyte and preparation method and preparation device thereof

By electrolyzing sulfite compounds with pentavalent or tetravalent vanadium compounds under ultraviolet light, the problem of low solubility in the preparation of vanadium electrolyte is solved, and high-efficiency preparation of high and low-priced vanadium electrolyte is achieved, and electrochemical performance is improved. and charge and discharge efficiency.

CN118957600APending Publication Date: 2024-11-15CHINA ENFI ENG CORP +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411023699.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the existing vanadium electrolyte preparation methods, the solubility of vanadium dipentoxide and ammonium metavanadate is low, resulting in low charge and discharge efficiency of the electrolyte and poor electrochemical performance.

Method used

The sulfite-containing compound or sulfur dioxide and pentavalent or tetravalent vanadium compounds are electrolyzed under ultraviolet light to form a high-valent vanadium electrolyte. A low-valent vanadium electrolyte is obtained through a one-step reaction to improve the electrochemical performance.

Benefits of technology

It has achieved efficient and convenient preparation of high and low-priced vanadium electrolytes, significantly improving electrochemical performance and charge and discharge efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957600A_ABST
    Figure CN118957600A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of electrolyte preparation, and discloses a vanadium electrolyte as well as a preparation method and a preparation device thereof, and the preparation method of the vanadium electrolyte comprises the following steps: mixing a sulfite-containing compound or sulfur dioxide, a vanadium-containing compound and water, and carrying out electrolysis under the action of ultraviolet light to form the vanadium electrolyte; the vanadium-containing compound comprises a pentavalent vanadium-containing compound and / or a tetravalent vanadium-containing compound; and the wavelength of the ultraviolet light is less than 400nm. The compound containing pentavalent vanadium or tetravalent vanadium and the compound containing sulfite or sulfur dioxide are used as raw materials, pentavalent vanadium or tetravalent vanadium is reduced into tetravalent vanadium or trivalent vanadium, the low-valent vanadium electrolyte is prepared from the high-valent vanadium compound only through one step, the preparation method is simple and easy to operate, and the prepared electrolyte is high in low-valent vanadium content and good in stability. The electrochemical performance is high; the preparation process is efficient and convenient.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of electrolyte preparation, and in particular to a vanadium electrolyte and a preparation method and a preparation device thereof. Background Art

[0002] There are two main methods for preparing vanadium electrolytes: chemical reduction and electrolysis. Among them, chemical reduction or a combination of chemical reduction and electrolysis can be used to prepare high-concentration electrolytes. However, the chemical method has the disadvantages of slow dissolution, low production volume, and the risk of dust pollution caused by the addition of reducing agents such as sulfur dioxide gas, as well as high energy consumption and low safety. The electrochemical performance of the electrolyte prepared by the chemical reduction method is not as good as that of the electrolyte prepared by the electrolysis method, and the chemical reduction method can usually only produce the dissolution of tetravalent vanadium. After the preparation is completed, the electrolyte still needs to be reduced to the appropriate valence state by electrolysis (usually a vanadium electrolyte containing 50% of tetravalent vanadium and 50% of trivalent vanadium).

[0003] In order to save costs, the electrolysis method generally uses relatively low-priced products such as vanadium pentoxide and ammonium metavanadate to prepare vanadium electrolyte. However, vanadium pentoxide and ammonium metavanadate have low solubility in sulfuric acid solution, the concentration of vanadium element near the electrode plate is low, the electrolysis reaction speed is slow, and it needs to be added in batches. The electrolysis time is long and the energy consumption is high, resulting in low electrochemical performance. Summary of the invention

[0004] In view of this, the present invention provides a vanadium electrolyte and a preparation method and preparation device thereof to solve the problem that the above-mentioned vanadium pentoxide, ammonium metavanadate, etc. have low solubility and the prepared electrolyte has low charge and discharge efficiency. A low-valent vanadium electrolyte is prepared in one step using a compound containing pentavalent vanadium or tetravalent vanadium as a raw material. The prepared electrolyte has a high content of low-valent vanadium and high electrochemical performance; the preparation process is efficient and convenient.

[0005] In a first aspect, the present invention provides a method for preparing a vanadium electrolyte, the preparation method comprising the following steps:

[0006] Mixing a sulfite-containing compound or sulfur dioxide, a vanadium-containing compound and water, and electrolyzing them under ultraviolet light to form a vanadium electrolyte;

[0007] The vanadium-containing compound includes a pentavalent vanadium-containing compound and / or a tetravalent vanadium-containing compound.

[0008] In an optional embodiment, the sulfite-containing compound comprises sulfite and / or sulfurous acid;

[0009] And / or, the pentavalent vanadium-containing compound includes any one or a combination of two or more of vanadium pentoxide, ammonium metavanadate or ammonium polyvanadate;

[0010] And / or, the tetravalent vanadium-containing compound comprises vanadyl sulfate.

[0011] In an optional embodiment, the molar ratio of the sulfite to the vanadium element in the vanadium-containing compound is (0.75-20.0):1;

[0012] And / or, the vanadium electrolyte further contains sulfuric acid, and the concentration of the sulfuric acid is 2-4 mol / L.

[0013] In an optional embodiment, during the electrolysis process, the current density is 100 mA / cm 2 -500mA / cm 2 ;

[0014] And / or, the wavelength of the ultraviolet light is 100-280nm; optionally, the ultraviolet light is UVC and / or VUV;

[0015] The light source used by the UVC is a low-pressure mercury lamp, and / or the light source used by the VUV is a vacuum ultraviolet lamp.

[0016] In an optional embodiment, the concentration of vanadium in the vanadium electrolyte is 1.5-2.5 mol / L;

[0017] And / or, after the electrolysis reaction is completed, the molar ratio of trivalent vanadium to tetravalent vanadium in the vanadium electrolyte is (0.9-1.1):1.

[0018] In an optional embodiment, during the electrolysis process, the cathode includes any one or a combination of two or more of a graphite electrode, a carbon felt electrode, a carbon paper electrode or a coated titanium electrode;

[0019] and / or, the anode comprises any one or a combination of two or more of a graphite electrode, a titanium electrode, an iridium-tantalum oxide-coated titanium electrode, a ruthenium-iridium oxide-coated titanium electrode, a gold-coated titanium electrode or a titanium nitride surface-modified titanium electrode;

[0020] and / or, the diaphragm of the electrolytic cell is a proton exchange membrane or an anion exchange membrane;

[0021] And / or, a sulfite-containing compound or sulfur dioxide, a vanadium-containing compound and water are mixed to obtain a mixed solution as the anolyte; an aqueous sulfuric acid solution or an aqueous sodium sulfate solution is used as the catholyte.

[0022] In a second aspect, the present invention provides a vanadium electrolyte preparation device, comprising a power supply and an electrolytic cell, wherein an anode region and a cathode region are formed inside the electrolytic cell through a diaphragm; the anode region is provided with an anode chamber and an anode plate, and the cathode region is provided with a cathode chamber and a cathode plate;

[0023] The anode plate and the cathode plate are connected to the negative electrode and the positive electrode of the power source respectively;

[0024] The cathode chamber is filled with an aqueous solution containing sulfite and vanadium, wherein the vanadium includes pentavalent vanadium and / or tetravalent vanadium;

[0025] An ultraviolet lamp is also arranged in the cathode chamber.

[0026] In an optional embodiment, the membrane is a proton exchange membrane or an anion exchange membrane;

[0027] and / or, the cathode plate comprises any one or a combination of two or more of a graphite electrode, a carbon felt electrode, a carbon paper electrode or a coated titanium electrode;

[0028] And / or, the anode plate comprises any one or a combination of two or more of a graphite electrode, a titanium electrode, an iridium-tantalum oxide-coated titanium electrode, a ruthenium-iridium oxide-coated titanium electrode, a gold-coated titanium electrode or a titanium nitride surface-modified titanium electrode;

[0029] And / or, the anode chamber is filled with a sulfuric acid aqueous solution or a sodium sulfate aqueous solution containing a concentration of .

[0030] In an optional embodiment, the ultraviolet lamp is immersed under the surface of an aqueous solution containing sulfite and vanadium;

[0031] Optionally, the ultraviolet lamp is provided with a protective cover;

[0032] Further optionally, the protective cover is a waterproof quartz shell.

[0033] In a third aspect, the present invention further provides an electrolyte prepared according to the preparation method and / or using the vanadium electrolyte preparation device.

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] The present invention provides a method for preparing a vanadium electrolyte, comprising: mixing a sulfite-containing compound or sulfur dioxide, a vanadium-containing compound and water, and performing electrolysis under ultraviolet light to form a vanadium electrolyte; the vanadium-containing compound comprises a pentavalent vanadium-containing compound and / or a tetravalent vanadium-containing compound. The present application uses a pentavalent vanadium-containing or tetravalent vanadium-containing compound and a sulfite-containing compound or sulfur dioxide as raw materials, the pentavalent vanadium or the tetravalent vanadium-containing compound is reduced to tetravalent vanadium or trivalent vanadium, and the high-valent vanadium compound is prepared in only one step to obtain a low-valent vanadium electrolyte. The preparation method is simple and easy to operate, and the prepared electrolyte has a high low-valent vanadium content and high electrochemical performance; the preparation process is efficient and convenient.

[0036] The present invention also provides a vanadium electrolyte preparation device, including a power source and an electrolytic cell, wherein an anode region and a cathode region are formed inside the electrolytic cell through a diaphragm; the anode region is provided with an anode chamber and an anode plate, and the cathode region is provided with a cathode chamber and a cathode plate; the anode plate and the cathode plate are respectively connected to the positive electrode and the negative electrode of the power source; the cathode chamber is filled with an aqueous solution containing sulfite and vanadium elements, wherein the vanadium elements include pentavalent vanadium elements and / or tetravalent vanadium elements; and an ultraviolet lamp is also provided in the cathode chamber. The aqueous solution containing sulfite and vanadium-containing compounds is used as the cathode liquid, and electrolysis is performed under the irradiation of ultraviolet light, which greatly improves the preparation efficiency of the electrolyte.

[0037] The electrolyte prepared by the present invention has higher electrochemical performance and can effectively improve the charge and discharge efficiency of the 10th cycle battery of the all-vanadium liquid flow. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0039] Figure 1 is a schematic diagram of a vanadium electrolyte preparation device in Example 1 of the present invention;

[0040] Figure 2 is a process flow chart of the vanadium electrolyte of Example 2 of the present invention;

[0041] Figure 3 The current and voltage during the charge and discharge process of the electrolyte of Example 2 of the present invention for an all-vanadium liquid flow cell;

[0042] Figure 4 This is the test result of the charge and discharge capacity of the electrolyte of Example 2 of the present invention used in an all-vanadium liquid flow cell.

[0043] Explanation of the reference numerals: 1. cathode chamber; 2. anode chamber; 3. diaphragm; 4. cathode plate; 5. anode plate; 6. quartz sleeve; 7. ultraviolet lamp; 8. cathode liquid inlet; 9. cathode liquid outlet; 10. anode liquid outlet. DETAILED DESCRIPTION

[0044] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0045] Unless otherwise specified or incompatible herewith, the terms and phrases used herein shall have the following meanings:

[0046] In the present application, the selection scope involving "and / or" includes any one of two or more related listed items, and also includes any and all combinations of the related listed items, wherein the any and all combinations include any combination of two related listed items, any more related listed items, or all related listed items.

[0047] In this application, in the "first aspect", "second aspect", "third aspect", "fourth aspect", etc., the terms "first", "second", "third", "fourth", etc. are used only for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first", "second", "third", "fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.

[0048] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0049] In this application, when it comes to percentage concentration, unless otherwise specified, it refers to the final concentration. The final concentration refers to the proportion of the added component in the system after the addition of the component.

[0050] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0051] A first aspect of the present invention provides a method for preparing a vanadium electrolyte, the method comprising the following steps:

[0052] Mixing a sulfite-containing compound or sulfur dioxide, a vanadium-containing compound and water, and electrolyzing them under ultraviolet light to form a vanadium electrolyte;

[0053] The vanadium-containing compound includes a pentavalent vanadium-containing compound and / or a tetravalent vanadium-containing compound.

[0054] The present application uses compounds containing pentavalent vanadium or tetravalent vanadium and compounds containing sulfite or sulfur dioxide as raw materials. Under the action of ultraviolet light, pentavalent vanadium or tetravalent vanadium is reduced to tetravalent vanadium or trivalent vanadium, and the high-valent vanadium compound is prepared into a low-valent vanadium electrolyte in only one step. The preparation method is simple and easy to operate. The prepared electrolyte has a high low-valent vanadium content and high electrochemical performance; the preparation process is efficient and convenient.

[0055] The present application utilizes sulfite to generate hydrated electrons (eaqˉ) with strong reducing ability under ultraviolet light excitation. The hydrated electrons then react with pentavalent vanadium to generate tetravalent vanadium, or the hydrated electrons reduce the tetravalent vanadium to trivalent vanadium.

[0056] In some embodiments, the sulfite-containing compound comprises sulfite and / or sulfurous acid;

[0057] Sulfites are soluble salts of sulfites.

[0058] And / or, the pentavalent vanadium-containing compound includes any one or a combination of two or more of vanadium pentoxide, ammonium metavanadate or ammonium polyvanadate;

[0059] And / or, the tetravalent vanadium-containing compound comprises vanadyl sulfate.

[0060] In some embodiments, the molar ratio of the sulfite to the vanadium element in the vanadium-containing compound is (0.75-20.0):1;

[0061] And / or, the vanadium electrolyte further contains sulfuric acid, and the concentration of the sulfuric acid is 2-4 mol / L.

[0062] In some embodiments, during the electrolysis process, the current density is 100 mA / cm 2 -500mA / cm 2 .

[0063] In some embodiments, the wavelength of the ultraviolet light is 100-280nm; optionally, the ultraviolet light is UVC (short-wave ultraviolet light, wavelength is 200-280nm) and / or VUV (vacuum ultraviolet light, wavelength is 100-200nm); the light source used may be a low-pressure mercury lamp (main emission wavelength is 254nm) and / or a vacuum ultraviolet lamp (main emission wavelength is 150-200nm);

[0064] In some embodiments, the concentration of vanadium in the vanadium electrolyte is 1.5-2.5 mol / L;

[0065] And / or, after the electrolysis reaction is completed, the molar ratio of trivalent vanadium to tetravalent vanadium in the vanadium electrolyte is (0.9-1.1): 1. Preferably, the valence of vanadium in the prepared vanadium electrolyte is 3.3-3.7.

[0066] In some embodiments, during the electrolysis process, the cathode of the electrolysis reaction includes any one or a combination of two or more of a graphite electrode, a carbon felt electrode, a carbon paper electrode, or a coated titanium electrode;

[0067] and / or, the anode of the electrolysis reaction comprises any one or a combination of two or more of a graphite electrode, a titanium electrode, an iridium-tantalum oxide-coated titanium electrode, a ruthenium-iridium oxide-coated titanium electrode, a gold-coated titanium electrode or a titanium nitride surface-modified titanium electrode;

[0068] and / or, the diaphragm of the electrolytic cell is a proton exchange membrane or an anion exchange membrane;

[0069] And / or, a sulfite-containing compound or sulfur dioxide, a vanadium-containing compound is mixed with water to obtain a mixed solution as the anolyte; an aqueous sulfuric acid solution or an aqueous sodium sulfate solution is used as the cathode solution; preferably, an aqueous sulfuric acid solution or an aqueous sodium sulfate solution with a concentration of 2-4 mol / L is used as the cathode solution.

[0070] The present invention also provides a vanadium electrolyte preparation device, comprising a power supply and an electrolytic cell, wherein an anode region and a cathode region are formed inside the electrolytic cell through a diaphragm; the anode region is provided with an anode chamber and an anode plate, and the cathode region is provided with a cathode chamber and a cathode plate;

[0071] The anode plate and the cathode plate are connected to the negative electrode and the positive electrode of the power source respectively;

[0072] The cathode chamber is filled with an aqueous solution containing sulfite and vanadium, wherein the vanadium includes pentavalent vanadium and / or tetravalent vanadium;

[0073] An ultraviolet lamp is also arranged in the cathode chamber.

[0074] In some embodiments, the membrane is a proton exchange membrane or an anion exchange membrane;

[0075] and / or, the cathode plate comprises any one or a combination of two or more of a graphite electrode, a carbon felt electrode, a carbon paper electrode or a coated titanium electrode;

[0076] And / or, the anode plate comprises any one or a combination of two or more of a graphite electrode, a titanium electrode, an iridium-tantalum oxide-coated titanium electrode, a ruthenium-iridium oxide-coated titanium electrode, a gold-coated titanium electrode or a titanium nitride surface-modified titanium electrode;

[0077] And / or, the anode chamber is filled with a sulfuric acid aqueous solution or a sodium sulfate aqueous solution containing a concentration of .

[0078] Optionally, the anode chamber is filled with a sulfuric acid aqueous solution or a sodium sulfate aqueous solution having a concentration of 2-4 mol / L.

[0079] In some embodiments, the ultraviolet lamp is immersed below the surface of an aqueous solution containing sulfite and a vanadium-containing compound;

[0080] Optionally, the ultraviolet lamp is provided with a protective cover;

[0081] Further optionally, the protective cover is a waterproof quartz shell.

[0082] The UV lamp is sealed and waterproofed with a protective cover to avoid direct contact between the UV lamp and water, thereby increasing the service life of the UV lamp.

[0083] The present invention also provides an electrolyte prepared according to the preparation method and / or using the vanadium electrolyte preparation device.

[0084] The present invention is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed by the present invention.

[0085] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0086] In the following experiments, the obtained vanadium electrolyte was made into a full vanadium liquid flow cell using the YTH-1 integrated liquid flow cell test system produced by Wuhan Zhisheng New Energy Co., Ltd. and tested. The charge and discharge efficiency of a battery is the ratio of the energy that the battery can provide during the discharge process to the energy it consumes during the charging process. The calculation formula is: charge and discharge efficiency = (discharge energy / charge energy) × 100%. Coulomb efficiency is the percentage of the discharge capacity of the battery to the charge capacity under charge and discharge conditions. The calculation formula is: Coulomb efficiency = (discharge capacity / charge capacity) × 100%.

[0087] Example 1

[0088] like Figure 1 As shown, this embodiment provides a vanadium electrolyte preparation device, including a power supply and an electrolytic cell, wherein an anode region and a cathode region are formed inside the electrolytic cell through a diaphragm 3; an anode chamber 2 and an anode plate 5 are provided in the anode region, and a cathode chamber 1 and a cathode plate 4 are provided in the cathode region; the anode plate 5 and the cathode plate 4 are connected to the positive and negative electrodes of the power supply respectively; an aqueous solution containing sulfite and vanadium elements is contained in the cathode chamber 1 as a cathode liquid, and the cathode liquid flows in from the cathode liquid inlet 8 and flows out from the cathode liquid outlet 9; the anode liquid flows in from the anode liquid inlet and flows out from the anode liquid outlet 10. The vanadium element includes pentavalent vanadium elements and / or tetravalent vanadium elements; an ultraviolet lamp 7 is also provided in the cathode chamber 1, and the ultraviolet lamp 7 is immersed under the liquid surface of the aqueous solution containing sulfite and vanadium compounds; the ultraviolet lamp 7 is provided with a sealed waterproof quartz sleeve 6. The diaphragm 3 is a proton exchange membrane; the cathode plate 4 is a graphite electrode; the anode plate 5 is a titanium electrode; the anode chamber 2 is filled with an aqueous solution containing 4 mol / L sulfuric acid.

[0089] Example 2

[0090] This embodiment provides a vanadium electrolyte and a preparation method thereof, comprising the following steps (process flow chart as shown in FIG. Figure 2 ):

[0091] At room temperature (20°C), weigh 273g of vanadium pentoxide (V2O5); add 333ml of 98% sulfuric acid aqueous solution to dissolve; weigh sodium sulfite according to the molar ratio of sodium sulfite to vanadium element in vanadium pentoxide of 0.75:1; mix the two, add water to 2000mL and stir to obtain a mixed solution as an electrolyte;

[0092] Place the mixed liquid in a storage tank and pump it into Figure 1 In the cathode chamber of the vanadium battery shown, the concentration of vanadium element in the cathode chamber is 1.5 mol / L, and the vanadium battery is circulated in the cathode chamber. The anode of the vanadium battery is electrolyzed under the ultraviolet light of a low-pressure mercury lamp (central wavelength = 254 nm), and the current density is 500 mA / cm 2 After 74 minutes of electrolysis, a vanadium electrolyte with a valence of 3.5 (the molar ratio of tetravalent vanadium to trivalent vanadium is 1:1) was obtained. 60 mL of the prepared vanadium electrolyte was used to make a full vanadium liquid flow cell for testing. The results are as follows: Figure 2 As shown, the discharge cut-off voltage is 1.0V, the charge cut-off voltage is 1.55V, the cycle is 10 times, and the current density is 160mA / cm 2 , the charge and discharge efficiency of the battery in the 10th cycle is 85.7%, and the coulombic efficiency is 95.37%. Figure 3 The electrolyte of this embodiment is used in an all-vanadium liquid flow cell, and the current and voltage during the charge and discharge process; Figure 4 The electrolyte of this embodiment is used in the test results of the charge and discharge capacity of the all-vanadium liquid flow battery.

[0093] Example 3

[0094] This embodiment provides a vanadium electrolyte, and the preparation method thereof comprises the following steps:

[0095] At room temperature (20°C), weigh 234 g of ammonium metavanadate (NH4VO3) and add appropriate amount of water to dissolve; weigh sulfurous acid according to the molar ratio of sulfurous acid to vanadium element in ammonium metavanadate being 10:1; mix the two and add water to 1000 mL and stir to obtain a mixed solution as an electrolyte;

[0096] The mixed solution is placed in the cathode chamber of a diaphragm electrolytic cell, and the concentration of vanadium in the cathode chamber is 2.0 mol / L.

[0097] Electrolysis was performed under the action of ultraviolet light with a central wavelength of 280 nm, and the current density was 100 mA / cm 2, electrolyzed for 175 minutes, and a vanadium electrolyte with a valence of 3.5 was obtained (the molar ratio of tetravalent vanadium to trivalent vanadium was 1:1). 60mL of the prepared vanadium electrolyte was used to make a full vanadium liquid flow cell for testing. The discharge cut-off voltage was 1.0V, the charge cut-off voltage was 1.55V, and the cycle was repeated 10 times with a current density of 160mA / cm 2 , the charge and discharge efficiency of the battery in the 10th cycle is 84.9%, and the coulombic efficiency is 96.18%.

[0098] Example 4

[0099] This embodiment provides a vanadium electrolyte, and the preparation method thereof comprises the following steps:

[0100] At room temperature (20°C), weigh ammonium polyvanadate ((NH4)2V6O 16 )750g, add 1000mL of water to dissolve; according to the molar ratio of sulfur dioxide to vanadium element in ammonium polyvanadate being 20:1, sulfur dioxide is introduced therein; and the mixed solution is used as an electrolyte;

[0101] The mixed solution was placed in the cathode chamber of a diaphragm electrolytic cell, wherein the concentration of vanadium was 2.5 mol / L, and electrolysis was performed under the action of ultraviolet light of a vacuum ultraviolet lamp (100-200 nm), and the current density was 200 mA / cm 2 , forming a vanadium electrolyte, electrolyzed for 105 minutes, and a vanadium electrolyte with a valence of 3.3 was obtained (the molar ratio of tetravalent vanadium to trivalent vanadium was 0.9:1). 60ml of the prepared vanadium electrolyte was used to make a full vanadium liquid flow single cell for testing. The discharge cut-off voltage was 1.0V, the charge cut-off voltage was 1.55V, and the cycle was repeated 10 times with a current density of 160mA / cm 2 , the charge and discharge efficiency of the battery in the 10th cycle is 85.9%, and the coulombic efficiency is 94.21%.

[0102] Example 5

[0103] At room temperature (20°C), weigh 182g of vanadyl sulfate, add sulfuric acid to dissolve and dilute to 1L. Add sodium sulfite in a molar ratio of 5:1 to the vanadium element in the vanadyl sulfate and stir to dissolve; obtain a mixed solution as an electrolyte;

[0104] Place the mixed liquid in a storage tank and pump it into Figure 1 The concentration of vanadium in the cathode chamber of the vanadium battery shown is 1.1 mol / L, and vanadium is circulated in the cathode chamber of the vanadium battery. The anode of the vanadium battery is electrolyzed under the ultraviolet light of a low-pressure mercury lamp (central wavelength = 254 nm), and the current density is 500 mA / cm 2, electrolyzed for 26 minutes, and a vanadium electrolyte with a valence of 3.7 (the molar ratio of tetravalent vanadium to trivalent vanadium is 1.1:1) was obtained. 60 mL of the prepared vanadium electrolyte was used to make a full vanadium liquid flow cell for testing. The discharge cut-off voltage was 1.0 V, the charge cut-off voltage was 1.55 V, and the cycle was repeated 10 times with a current density of 160 mA / cm 2 , the charge and discharge efficiency of the battery in the 10th cycle is 85.3%, and the coulombic efficiency is 95.15%.

[0105] Comparative Example 1

[0106] This comparative example provides a vanadium electrolyte, and the preparation method thereof comprises:

[0107] At room temperature (20°C), 273g of vanadium pentoxide was used as a raw material, and 333ml of a 98% sulfuric acid aqueous solution was added to dissolve it; oxalic acid was added according to a molar ratio of oxalic acid to vanadium pentoxide of 1.05:1, and after heating and reduction, the obtained tetravalent vanadium solution was Figure 1 The same electrolytic cell is shown, without UV lamp, and the current density is 100mA / cm 2 After 370 minutes of electrolysis, a vanadium electrolyte with a valence of 3.5 (the molar ratio of tetravalent vanadium to trivalent vanadium is 1:1) was obtained. 60 ml of the prepared vanadium electrolyte was used to make a full vanadium liquid flow cell for testing. The discharge cut-off voltage was 1.0 V, the charge cut-off voltage was 1.55 V, and the cycle was repeated 10 times with a current density of 160 mA / cm 2 , the charge and discharge efficiency of the battery in the 10th cycle is 79.9%, and the coulombic efficiency is 93.84%.

[0108] Comparative Example 2

[0109] This comparative example provides a vanadium electrolyte, and the preparation method thereof comprises:

[0110] Weigh 182 g of vanadyl sulfate, add sulfuric acid to dissolve and adjust the volume to 1 L. Weigh sodium sulfite according to the molar ratio of sodium sulfite to vanadium element in vanadyl sulfate of 5:1, heat in a water bath at 70°C with stirring for 1 hour, and reduce to obtain a tetravalent vanadium solution.

[0111] The obtained tetravalent vanadium solution is Figure 1 The same electrolytic cell is shown, without UV lamp, and the current density is 100mA / cm 2 After 180 minutes of electrolysis, a vanadium electrolyte with a valence of 3.5 was obtained. 60 ml of the prepared vanadium electrolyte was used to make a full vanadium liquid flow cell for testing. The discharge cut-off voltage was 1.0 V, the charge cut-off voltage was 1.55 V, and the cycle was repeated 10 times with a current density of 160 mA / cm 2, the charge and discharge efficiency of the battery in the 10th cycle is 80.3%, and the coulombic efficiency is 93.70%.

[0112] Comparative Example 3

[0113] The preparation method of this comparative example is basically the same as that of Example 2, except that the wavelength of the ultraviolet light is 400 nm.

[0114] The electrolysis took 235 minutes to obtain a vanadium electrolyte with a valence of 3.5. 60 ml of the prepared vanadium electrolyte was used to make a full vanadium liquid flow cell for testing. The discharge cut-off voltage was 1.0 V, the charge cut-off voltage was 1.55 V, and the current density was 160 mA / cm after 10 cycles. 2 , the charge and discharge efficiency of the battery in the 10th cycle is 80.5%, and the coulombic efficiency is 92.29%.

[0115] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A method for preparing a vanadium electrolyte, characterized in that: The preparation method comprises the following steps: Mixing a sulfite-containing compound or sulfur dioxide, a vanadium-containing compound and water, and electrolyzing them under ultraviolet light to form a vanadium electrolyte; The vanadium-containing compound includes a pentavalent vanadium-containing compound and / or a tetravalent vanadium-containing compound; The wavelength of the ultraviolet light is less than 400 nm.

2. The preparation method according to claim 1, characterized in that: In the mixed solution, the sulfite-containing compound includes sulfite and / or sulfurous acid; And / or, the pentavalent vanadium-containing compound includes any one or a combination of two or more of vanadium pentoxide, ammonium metavanadate or ammonium polyvanadate; And / or, the tetravalent vanadium-containing compound comprises vanadyl sulfate.

3. The preparation method according to claim 1 or 2, characterized in that: In the mixed solution, the molar ratio of sulfite to vanadium is (0.75-20.0):1; And / or, the vanadium electrolyte further contains sulfuric acid, and the concentration of the sulfuric acid is 2-4 mol / L.

4. The preparation method according to claim 1 or 2, characterized in that: During the electrolysis process, the current density is 100 mA / cm 2 -500mA / cm 2 ; And / or, the wavelength of the ultraviolet light is 100-280nm; optionally, the ultraviolet light is UVC and / or VUV; The light source used by the UVC is a low-pressure mercury lamp, and / or the light source used by the VUV is a vacuum ultraviolet lamp.

5. The preparation method according to any one of claims 1 to 4, characterized in that: The concentration of vanadium element in the vanadium electrolyte is 1.5-2.5 mol / L; And / or, after the electrolysis reaction is completed, the molar ratio of trivalent vanadium to tetravalent vanadium in the vanadium electrolyte is (0.9-1.1):

1.

6. The preparation method according to claim 1 or 2, characterized in that: During the electrolysis process, the cathode includes any one or a combination of two or more of a graphite electrode, a carbon felt electrode, a carbon paper electrode or a coated titanium electrode; and / or, the anode comprises any one or a combination of two or more of a graphite electrode, a titanium electrode, an iridium-tantalum oxide-coated titanium electrode, a ruthenium-iridium oxide-coated titanium electrode, a gold-coated titanium electrode or a titanium nitride surface-modified titanium electrode; and / or, the diaphragm of the electrolytic cell is a proton exchange membrane or an anion exchange membrane; And / or, a sulfite-containing compound or sulfur dioxide, a vanadium-containing compound and water are mixed to obtain a mixed solution as the anolyte; an aqueous sulfuric acid solution or an aqueous sodium sulfate solution is used as the catholyte.

7. A vanadium electrolyte preparation device, comprising a power supply and an electrolytic cell, characterized in that: The electrolytic cell is internally formed with an anode region and a cathode region through a diaphragm; the anode region is provided with an anode chamber and an anode plate, and the cathode region is provided with a cathode chamber and a cathode plate; The anode plate and the cathode plate are connected to the positive electrode and the negative electrode of the power source respectively; The cathode chamber is filled with an aqueous solution containing sulfite and vanadium, wherein the vanadium includes pentavalent vanadium and / or tetravalent vanadium; An ultraviolet lamp is also arranged in the cathode chamber.

8. The vanadium electrolyte preparation device according to claim 7, characterized in that: The diaphragm is a proton exchange membrane or an anion exchange membrane; and / or, the cathode plate comprises any one or a combination of two or more of a graphite electrode, a carbon felt electrode, a carbon paper electrode or a coated titanium electrode; And / or, the anode plate comprises any one or a combination of two or more of a graphite electrode, a titanium electrode, an iridium-tantalum oxide-coated titanium electrode, a ruthenium-iridium oxide-coated titanium electrode, a gold-coated titanium electrode or a titanium nitride surface-modified titanium electrode; And / or, the anode chamber is filled with a sulfuric acid aqueous solution or a sodium sulfate aqueous solution.

9. The vanadium electrolyte preparation device according to claim 7 or 8, characterized in that: The ultraviolet lamp is immersed under the liquid surface of the aqueous solution containing sulfite and vanadium element; Optionally, the ultraviolet lamp is provided with a protective cover; Further optionally, the protective cover is a waterproof quartz shell.

10. An electrolyte prepared by the preparation method according to any one of claims 1 to 6 and / or by the vanadium electrolyte preparation device according to any one of claims 7 to 9.

Citation Information

Cited By

  • Vanadium electrolyte and preparation method and application thereof