Charging method of silicon material
By controlling the feeding interval time and heating conditions of silicon materials, the hydrogen jump and sputtering of particulate silicon in the production process are reduced, the quality and equipment life of single crystal silicon are improved, and the hydrogen jump and sputtering in the existing technology are solved. The problem of silicon splashing.
Patent Information
- Application Number
- CN202411044435.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
AI Technical Summary
In the production process of single crystal silicon, particulate silicon contains hydrogen due to production process reasons, which leads to hydrogen jump and sputtering silicon problems at high temperatures, affecting the quality of single crystal silicon.
Through a feeding method of silicon material, poly-cylinder silicon material is added to the crucible in sequence using the feeding barrel. The first and last barrels are small materials, and the rest are granular silicon. During the feeding process, it is continuously heated through a heater to adjust The feeding interval time and heating power increase the distance between the feeding barrel and the water-cooled screen, and argon is introduced to control the solid proportion and heating conditions of the crucible liquid level, and reduce the risk of hydrogen jump and silicon splashing.
It effectively reduces the risk of hydrogen jumping and splashing of particulate silicon, improves the quality of single crystal silicon, saves energy and reduces the damage to the equipment by high temperature, extends the equipment life, and reduces the risk of dust scattering and crystal rod disconnection.
Smart Images

Figure CN118957734A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of photovoltaic technology, and in particular to a method for adding silicon material. Background Art
[0002] As a key supporting material for the modern information society, single crystal silicon is the main functional material for photovoltaic power generation using solar energy. Currently, single crystal silicon is mainly produced by the Czochralski method. However, due to its production process, the granular silicon used in the Czochralski method contains a certain amount of hydrogen. When melting at high temperatures, problems such as hydrogen jump and silicon splashing are prone to occur, affecting the quality of single crystal silicon. Summary of the invention
[0003] The present application aims to solve at least one of the technical problems existing in the prior art. To this end, the present application proposes a method for adding silicon material, which can reduce the risk of silicon hydrogen jumping and silicon splashing of particles and improve the quality of single crystal silicon.
[0004] In a first aspect, the present application provides a method for adding silicon material, comprising:
[0005] Multiple tubes of silicon material are added into the crucible in sequence through a feeding tube, the first tube and the last tube of silicon material are small materials, and the remaining tubes of silicon material are granular silicon;
[0006] During the feeding process of the multi-tube silicon material, the silicon material in the crucible is continuously heated by a heater;
[0007] The feeding interval time of two adjacent tubes of silicon material is the minimum value of the time required for the solid proportion of the liquid surface of the crucible to reach a preset proportion and the preset interval time.
[0008] According to the silicon material adding method of the present application, after each bucket of silicon material is added to the crucible, the next bucket of silicon material is added to the crucible at an interval, wherein the adding interval is the time required for the solid proportion of the crucible liquid surface to reach a preset proportion and the minimum value of the preset interval time, so as to avoid the adding interval time being too long and the liquid specific gravity in the crucible being too large, thereby reducing the risk of granular silicon hydrogen jumping and silicon splashing, and improving the quality of single crystal silicon.
[0009] According to an embodiment of the present application, the preset proportion is 80%-100%, and the preset interval time is 20min-35min.
[0010] According to an embodiment of the present application, the preset proportion is 95%, and the preset interval time is 25 minutes.
[0011] According to one embodiment of the present application, the remaining silicon material is 100% granular silicon.
[0012] According to one embodiment of the present application, the method further includes:
[0013] During the feeding process of the multi-tube silicon material, the heating power of the heater is adjusted so that the heating power during the feeding process of the granular silicon is reduced by 8%-10% compared with the heating power during the feeding process of the small material.
[0014] According to one embodiment of the present application, the method further includes:
[0015] During the feeding process of the multi-barrel silicon material, the first distance between the discharge port of the feeding barrel and the water cooling screen is adjusted so that the first distance during the feeding process of the granular silicon is 20%-30% larger than the first distance during the feeding process of the small material.
[0016] According to one embodiment of the present application, adjusting the first distance between the outlet of the charging barrel and the water cooling screen includes:
[0017] The position of the discharge port of the feeding barrel is adjusted to adjust the first distance between the discharge port of the feeding barrel and the water cooling screen.
[0018] According to one embodiment of the present application, adjusting the position of the feeding cylinder includes:
[0019] The length of the flange support tube is adjusted to adjust the position of the flange plate, so as to adjust the position of the discharge port of the feeding barrel. The flange plate is sleeved on the feeding barrel, and the flange support tube is connected to the flange plate.
[0020] According to one embodiment of the present application, the method further includes:
[0021] During the feeding process of the multi-tube silicon material, the second distance between the discharge port of the feeding tube and the crucible is adjusted so that the second distance during the feeding process of the granular silicon is 10%-15% larger than the second distance during the feeding process of the small material.
[0022] According to one embodiment of the present application, adjusting the second distance between the outlet of the feeding cylinder and the crucible includes:
[0023] The position of the crucible is adjusted to adjust a second distance between the discharge port of the feeding cylinder and the crucible.
[0024] According to one embodiment of the present application, the method further includes:
[0025] During the feeding process of the multi-tube silicon material, argon gas is introduced and the flow rate of the argon gas is adjusted so that the flow rate of the argon gas during the feeding process of the granular silicon is increased by 25%-50% compared with the flow rate of the argon gas during the feeding process of the small material.
[0026] The above one or more technical solutions in the embodiments of the present application have at least one of the following technical effects:
[0027] After each bucket of silicon material is added to the crucible, the next bucket of silicon material is added to the crucible at a certain interval, wherein the feeding interval is the minimum value of the time required for the solid ratio of the crucible liquid surface to reach the preset ratio and the preset interval time, so as to avoid the feeding interval time being too long and the liquid specific gravity in the crucible being too large, thereby reducing the risk of silicon hydrogen jump and silicon splashing of granular silicon and improving the quality of single crystal silicon;
[0028] The heating power of the corresponding heater when adding granular silicon is lower than that of the corresponding heater when adding small materials, so as to achieve the purpose of energy saving, and at the same time prevent the granular silicon from melting too quickly, reduce the damage to the crucible caused by high temperature, and extend the life of the crucible;
[0029] When feeding granular silicon, the distance between the discharge port of the feeding barrel and the water cooling screen is increased to reduce the risk of dust flying upward and adhering to the surface of the water cooling screen during the feeding process, thereby reducing the risk of crystal rod breakage during the crystal pulling process due to dust falling;
[0030] When adding granular silicon, the distance between the discharge port of the feeding barrel and the crucible is increased, thereby increasing the distance between the water-cooling screen and the crucible, reducing the risk of silicon liquid splashing onto the bottom of the water-cooling screen during the silicon melting process, and further reducing the risk of dust flying upward and adhering to the surface of the water-cooling screen during the feeding process.
[0031] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0033] Figure 1 It is a schematic flow chart of a method for adding silicon material provided in an embodiment of the present application;
[0034] Figure 2 It is a schematic diagram of the structure of the single crystal furnace provided in the embodiment of the present application. DETAILED DESCRIPTION
[0035] The embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and cannot be understood as limiting the present application.
[0036] The method for adding silicon material provided in the embodiments of the present application is described below with reference to the accompanying drawings.
[0037] Figure 1 A schematic flow chart of a method for adding silicon material provided in an embodiment of the present application.
[0038] like Figure 1 As shown, the method for adding silicon material provided in the embodiment of the present application includes step 110 and step 120.
[0039] Step 110, adding multiple tubes of silicon material into the crucible in sequence through a feeding tube, wherein the first tube of silicon material and the last tube of silicon material are small materials, and the remaining tubes of silicon material are granular silicon.
[0040] It should be noted that the method for adding silicon material provided in the embodiment of the present application can be applied to a single crystal furnace. Figure 2 This is a schematic diagram of the structure of the single crystal furnace provided in the embodiment of the present application. Figure 2 As shown, the single crystal furnace includes a charging barrel 1, a furnace body 2 and a crucible 4. The crucible 4 is located in the furnace body 2, and the opening of the crucible 4 faces upward. The crucible 4 can be arranged near the bottom of the furnace body 2. The crucible 4 is used to place silicon material. The charging barrel 1 is arranged vertically, and the bottom of the charging barrel 1 passes through the top of the furnace body 2 and extends into the furnace body 2. The charging barrel 1 is located above the crucible 4. The charging barrel 1 is used to add silicon material to the crucible 4.
[0041] During the feeding process, multiple tubes of silicon material are added to the crucible 4 in sequence through the feeding tube 1. Figure 2 As shown, a discharge port 13 is provided at the bottom of the feeding barrel 1, and the silicon material in the feeding barrel 1 enters the crucible 4 through the discharge port 13. Among the multiple barrels of silicon material added to the crucible 4, the first barrel of silicon material and the last barrel of silicon material are small materials, and the silicon materials in the remaining barrels except the first barrel and the last barrel are granular silicon. Among them, the small material is native polycrystalline silicon, which is a form of single silicon and a polycrystalline material composed of a large number of small crystals. The size of the small material is larger than that of the granular silicon, such as the size of the small material is 5-50mm, and the size of the granular silicon is 0.15-4mm.
[0042] The number of silicon material cylinders can be preset according to actual needs. For example, N cylinders of silicon material are added to the crucible 4 in sequence through the feeding cylinder 1, N>2, the first cylinder of silicon material and the Nth cylinder of silicon material are small materials, and the second cylinder to the N-1th cylinder of silicon material are granular silicon.
[0043] Step 120, during the feeding process of multiple tubes of silicon material, continuously heat the silicon material in the crucible by a heater; wherein the feeding interval time of two adjacent tubes of silicon material is the minimum value of the time required for the solid proportion of the crucible liquid surface to reach a preset proportion and the preset interval time.
[0044] Combination Figure 2As shown, the single crystal furnace further includes a heater 5. The heater 5 is located in the furnace body 2, and the heater 5 is arranged on the periphery of the crucible 4, such as the heater 5 can be arranged around the crucible 4. The heater 5 is used to heat and melt the silicon material in the crucible 4. The heater 5 can be a main heater, and the single crystal furnace can also include a bottom heater, which can be located at the bottom of the crucible 4.
[0045] During the feeding process, the silicon material in the crucible 4 is continuously heated by the heater 5 so that the silicon material in the crucible 4 is melted from solid to liquid. After each tube of silicon material is added to the crucible 4, the next tube of silicon material is added to the crucible 4 at a certain interval (i.e., the feeding interval time). The feeding interval time of each tube of silicon material can be the same as or different from that of the previous tube of silicon material. The feeding interval time of two adjacent tubes of silicon material is determined according to the time required for the solid ratio of the liquid surface of the crucible 4 to reach a preset ratio and the preset time interval.
[0046] The liquid surface of the crucible 4 refers to the surface of the substance (such as solid silicon) heated to a molten state in contact with the gas inside the crucible 4. The solid ratio of the liquid surface of the crucible 4 can be the ratio of the area of solid silicon at the liquid surface of the crucible 4 to the entire liquid surface area. For example, the liquid surface image of the crucible 4 is obtained in real time, the solid silicon area in the liquid surface image is identified, and the ratio of the solid silicon area to the entire liquid surface area is calculated, which is the solid ratio of the liquid surface of the crucible 4.
[0047] Each time a tube of silicon material is added to the crucible 4, the timing starts, and the solid percentage of the liquid surface of the crucible 4 is detected in real time. It should be noted that each time a tube of silicon material is added to the crucible 4, the solid silicon in the crucible 4 is the largest, and the solid percentage of the liquid surface of the crucible 4 is 100%. The silicon material in the crucible 4 is heated by the heater 5, and the solid silicon at the bottom of the crucible 4 first slowly melts into liquid, and then the solid silicon on the liquid surface of the crucible 4 slowly melts. When the solid silicon on the liquid surface of the crucible 4 slowly begins to melt, it indicates that the solid silicon at the bottom of the crucible 4 has melted, the solid percentage of the liquid surface of the crucible 4 begins to be less than 100%, and the solid percentage of the liquid surface of the crucible 4 slowly decreases.
[0048] In the process of real-time detection of the solid ratio of the liquid surface of the crucible 4, if the timing time has not exceeded the preset interval time, and it is detected that the solid ratio of the liquid surface of the crucible 4 has dropped to the preset ratio, the next tube of silicon material is added to the crucible 4, that is, the feeding interval time this time is the time required for the solid ratio of the liquid surface of the crucible 4 to reach the preset ratio. If the timing time reaches the preset interval time, and it is detected that the solid ratio of the liquid surface of the crucible 4 has not dropped to the preset ratio, the next tube of silicon material is added to the crucible 4, that is, the feeding interval time this time is the preset interval time.
[0049] If the feeding interval is too long, the liquid specific gravity in the crucible 4 is too large, the granular silicon directly enters the molten silicon, and the free hydrogen in the granular silicon is wrapped by the molten silicon, which is easy to cause hydrogen jumps and silicon splashing. Therefore, the preset proportion and the preset time interval can be determined according to the situation that the granular silicon reduces or even does not produce hydrogen jumps and silicon splashing. For example, the preset proportion can be the minimum solid proportion under the situation that the granular silicon reduces or even does not produce hydrogen jumps and silicon splashing, and the preset time interval can be the maximum time interval under the situation that the granular silicon reduces or even does not produce hydrogen jumps and silicon splashing.
[0050] Each time a tube of silicon material is added, the solid proportion of the liquid surface of the crucible 4 needs to be detected and timed to determine the time to add the next tube of silicon material, thereby ensuring that when each tube of silicon material is added to the crucible 4, the liquid surface of the crucible 4 can be mainly solid silicon, preventing granular silicon from directly entering the molten silicon, reducing or even avoiding the free hydrogen in the granular silicon from being wrapped by the molten silicon to produce hydrogen jumping and silicon splashing, thereby improving the quality of the produced single crystal silicon.
[0051] In some embodiments, the preset proportion is 80%-100%, and the preset interval time is 20min-35min. It is understandable that the preset proportion can be greater than or equal to 80% and less than 100%, such as the preset proportion can be 80%, 85%, 90%, 95% or 99%. The preset interval time can be greater than or equal to 20min and less than or equal to 35min, such as the preset interval time can be 20min, 25min, 30min or 35min.
[0052] In some embodiments, the preset percentage is 95%, and the preset interval time is 25 minutes, that is, the interval time between two adjacent tubes of silicon material is the minimum value of the time required for the solid percentage of the liquid surface of the crucible 4 to be reduced to 95% and 25 minutes. After adding a tube of silicon material to the crucible 4, if the interval time has not exceeded 25 minutes, and the solid percentage of the liquid surface of the crucible 4 has been reduced to 95%, then the next tube of silicon material is added to the crucible 4, and the interval time for this addition is the time required for the solid percentage of the liquid surface of the crucible 4 to be reduced to 95%; if the interval time reaches 25 minutes, and the solid percentage of the liquid surface of the crucible 4 has not been reduced to 95%, then the next tube of silicon material is added to the crucible 4, and the interval time for this addition is 25 minutes.
[0053] In the related art, the feeding interval between two adjacent tubes of silicon material is a fixed interval, and the fixed interval is greater than 35 minutes, resulting in a too long feeding interval between two adjacent tubes of silicon material, a large specific gravity of the liquid in the crucible, and hydrogen jumps and silicon splashing are prone to occur during the feeding process. In this embodiment, the feeding interval between two adjacent tubes of silicon material varies according to actual conditions, and the time required to reduce the solid proportion of the liquid surface of crucible 4 to 95% and the minimum value of 25 minutes are used as the feeding interval to avoid too long a feeding interval and too large a specific gravity of the liquid in crucible 4, thereby reducing the risk of hydrogen jumps and silicon splashing of granular silicon, and thus improving the quality of single crystal silicon.
[0054] In some embodiments, the remaining tubes of silicon material are 100% granular silicon. For example, in N tubes of silicon material, the second tube to the N-1th tube of silicon material are all 100% granular silicon.
[0055] In the related art, when loading granular silicon into the feeding barrel 1, it is necessary to first pad the feeding barrel 1 with small materials or blocks, and then fill the granular silicon. The loading process is too complicated, which increases the difficulty of loading for operators. However, when loading granular silicon into the feeding barrel 1 in this embodiment, 100% granular silicon is directly filled without padding with small materials or blocks, which reduces the difficulty of loading for operators.
[0056] In some embodiments, the method for adding silicon material further comprises:
[0057] During the feeding process of the multi-tube silicon material, the heating power of the heater is adjusted so that the heating power during the feeding process of the granular silicon is reduced by 8%-10% compared with the heating power during the feeding process of the small material.
[0058] It can be understood that the heating power during the granular silicon feeding process can be reduced by 8%, 8.5%, 9%, 9.5% or 10% etc. compared with the heating power during the small material feeding process.
[0059] During the feeding process, the heating power of the heater 5 can be adjusted according to the type of silicon material added to the crucible 4, that is, the heating power of the heater 5 corresponding to adding small materials to the crucible 4 can be different from the heating power of the heater 5 corresponding to adding granular silicon to the crucible 4.
[0060] Since the size of granular silicon is smaller than that of small materials, granular silicon has the advantage of faster melting than small materials. The heating power of the corresponding heater 5 when granular silicon is added is lower than the heating power of the corresponding heater 5 when small materials are added, so as to achieve the purpose of energy saving, and at the same time, it can prevent the granular silicon from melting too quickly, and also make the temperature of the crucible 4 relatively lower, reduce the damage to the crucible 4 caused by high temperature, and extend the life of the crucible 4.
[0061] For example, in the process of adding N tubes of silicon material into the crucible 4, when the first tube of silicon material (small material) is added into the crucible 4, the heating power of the heater 5 is adjusted to the first heating power. When the second tube of silicon material (granular silicon) is added into the crucible 4, the heating power of the heater 5 is adjusted from the first heating power to the second heating power. When the Nth tube of silicon material (small material) is added into the crucible 4, the heating power of the heater 5 is adjusted from the second heating power to the first heating power. The second heating power is less than the first heating power.
[0062] In some embodiments, the heating power during the granular silicon feeding process (second heating power) is 90kw, and the heating power during the small material feeding process (first heating power) is 100kw, that is, the heating power during the granular silicon feeding process is 10% less than the heating power during the small material feeding process, that is, the second heating power is 10% less than the first heating power.
[0063] In some embodiments, the method for adding silicon material further comprises:
[0064] During the feeding process of multi-barrel silicon materials, the first distance between the discharge port of the feeding barrel and the water cooling screen is adjusted so that the first distance during the feeding process of granular silicon is 20%-30% larger than the first distance during the feeding process of small materials.
[0065] It can be understood that the first distance during the granular silicon feeding process can be increased by 20%, 23%, 25%, 27% or 30% compared with the first distance during the small material feeding process.
[0066] Combination Figure 2 As shown, the single crystal furnace also includes a water cooling screen 3, which is located in the furnace body 1. After the silicon material in the crucible 4 is heated and melted, a single crystal silicon seed crystal is inserted into the melt surface. After the seed crystal and the melt are melted, the seed crystal is slowly pulled upward, and the crystal will grow at the lower end of the seed crystal. As the seed crystal is pulled, the crystal gradually grows to form a crystal rod. The water cooling screen 3 is used to cool the crystal rod during the crystal pulling process.
[0067] During the feeding process, the distance (i.e., the first distance) between the discharge port 13 of the feeding barrel 1 and the water cooling screen 3 can be adjusted according to the type of silicon material added to the crucible 4, that is, the first distance corresponding to adding small materials to the crucible 4 and the first distance corresponding to adding granular silicon to the crucible 4 may be different.
[0068] Since granular silicon also contains a certain amount of dust particles, the dust is easy to fly upward and adhere to the surface of the water cooling screen during the granular silicon feeding process. During the crystal pulling process, the dust is easy to fall and cause the crystal rod to break, affecting the quality of the single crystal silicon.
[0069] In this embodiment, the first distance corresponding to the addition of granular silicon is greater than the first distance corresponding to the addition of small materials, that is, the distance between the discharge port 13 of the feeding barrel 1 and the water-cooling screen 3 is increased when granular silicon is added, thereby reducing the risk of dust flying upward and adhering to the surface of the water-cooling screen 3 during the addition process, thereby reducing the risk of crystal rod breakage during the crystal pulling process due to dust falling.
[0070] For example, in the process of adding N cylinders of silicon material to the crucible 4, when adding the first cylinder of silicon material (small material) to the crucible 4, the first distance between the discharge port 13 of the feeding cylinder 1 and the water cooling screen 3 is adjusted to the first value. When adding the second cylinder of silicon material (granular silicon) to the crucible 4, the first distance between the discharge port 13 of the feeding cylinder 1 and the water cooling screen 3 is adjusted from the first value to the second value. When adding the Nth cylinder of silicon material (small material) to the crucible 4, the first distance between the discharge port 13 of the feeding cylinder 1 and the water cooling screen 3 is adjusted from the second value to the first value. Among them, the second value is greater than the first value.
[0071] In some embodiments, the first distance during the granular silicon feeding process is 40 mm, and the first distance during the small material feeding process is 32 mm. For example, the first distance during the granular silicon feeding process is 25% greater than the first distance during the small material feeding process, that is, the second value is 25% greater than the first value.
[0072] In some embodiments, adjusting the first distance between the outlet of the charging barrel and the water cooling shield includes:
[0073] The position of the discharge port of the feeding barrel is adjusted to adjust the first distance between the discharge port of the feeding barrel and the water cooling screen.
[0074] The position of the water cooling screen 3 remains unchanged, and the first distance between the discharge port 13 of the feeding barrel 1 and the water cooling screen 3 can be adjusted by adjusting the position of the discharge port 13 of the feeding barrel 1 .
[0075] Combination Figure 2 As shown, the water-cooling screen 3 is located above the discharge port 13 of the feeding barrel 1. By adjusting the position of the feeding barrel 1 in the vertical direction, the position of the discharge port 13 of the feeding barrel 1 in the vertical direction can be adjusted, thereby adjusting the first distance between the discharge port 13 of the feeding barrel 1 and the water-cooling screen 3.
[0076] For example, in the process of adding N cylinders of silicon material to the crucible 4, when adding the first cylinder of silicon material (small material) to the crucible 4, the discharge port 13 of the feeding cylinder 1 is adjusted in the vertical direction to be located at the first position, so that the first distance between the discharge port 13 of the feeding cylinder 1 and the water-cooling screen 3 is the first value. When adding the second cylinder of silicon material (granular silicon) to the crucible 4, the discharge port 13 of the feeding cylinder 1 is adjusted in the vertical direction to be located at the second position, so that the first distance between the discharge port 13 of the feeding cylinder 1 and the water-cooling screen 3 is adjusted from the first value to the second value. When adding the Nth cylinder of silicon material (small material) to the crucible 4, the discharge port 13 of the feeding cylinder 1 is adjusted in the vertical direction to be located at the first position, so that the first distance between the discharge port 13 of the feeding cylinder 1 and the water-cooling screen 3 is adjusted from the second value to the first value. Among them, the second position is lower than the first position. For example, the second position is 10 mm lower than the first position.
[0077] In some embodiments, adjusting the position of the charging cylinder includes:
[0078] The length of the flange support pipe is adjusted to adjust the position of the flange plate, so as to adjust the position of the discharge port of the feeding barrel. The flange plate is sleeved on the feeding barrel, and the flange support pipe is connected to the flange plate.
[0079] Combination Figure 2 As shown, the single crystal furnace also includes a flange support tube 11, a flange 12 and a furnace flange 21. The flange 12 is sleeved on the charging barrel 1, and the flange support tube 11 is located outside the furnace body 2 and is located above the flange 12 and connected to the flange 12. The flange support tube 11 is used to support the flange 12. The furnace flange 21 is located inside the furnace body 2 and below the flange 12. During the charging process, the furnace flange 21 can resist the descending flange 12 so that the silicon material in the charging barrel 1 is added to the crucible 4.
[0080] Shortening the length of the flange support tube 11 can raise the position of the flange 12, extend the length of the charging barrel 1 in the furnace body 2, thereby lowering the position of the discharge port 13 of the charging barrel 1 and increasing the first distance between the discharge port 13 of the charging barrel 1 and the water cooling screen 3. When feeding granular silicon, the length of the flange support tube 11 can be shortened by 10 mm, so that the first distance during the granular silicon feeding process is 10 mm larger than the first distance during the small material feeding process.
[0081] In some embodiments, the method for adding silicon material further comprises:
[0082] During the feeding process of multi-tube silicon material, the second distance between the discharge port of the feeding tube and the crucible is adjusted so that the second distance during the feeding process of granular silicon is 10%-15% larger than the second distance during the feeding process of small materials.
[0083] During the feeding process, the distance between the discharge port 13 of the feeding barrel 1 and the crucible 4 (i.e., the second distance) can be adjusted according to the type of silicon material added to the crucible 4, that is, the second distance corresponding to adding small materials to the crucible 4 and the second distance corresponding to adding granular silicon to the crucible 4 can be different.
[0084] During the silicon melting process, silicon liquid is easy to splash onto the surface of the water-cooled screen, affecting the problem of crystal pulling. In this embodiment, the second distance corresponding to the addition of granular silicon is greater than the second distance corresponding to the addition of small materials, that is, when adding granular silicon, the distance between the discharge port 13 of the feeding tube 1 and the crucible 4 is increased, thereby increasing the distance between the water-cooled screen 3 and the crucible 4, reducing the risk of silicon liquid splashing onto the bottom 31 of the water-cooled screen 3 during the silicon melting process, and further reducing the risk of dust flying upward and adhering to the surface of the water-cooled screen 3 during the addition process. Moreover, granular silicon has the advantage of being lighter than small materials. When adding granular silicon, increasing the distance between the discharge port 13 of the feeding tube 1 and the crucible 4 will not damage the crucible 4.
[0085] For example, in the process of adding N cylinders of silicon material to the crucible 4, when adding the first cylinder of silicon material (small material) to the crucible 4, the second distance between the discharge port 13 of the feeding cylinder 1 and the crucible 4 is adjusted to the third value. When adding the second cylinder of silicon material (granular silicon) to the crucible 4, the second distance between the discharge port 13 of the feeding cylinder 1 and the crucible 4 is adjusted to the fourth value. When adding the Nth cylinder of silicon material (small material) to the crucible 4, the second distance between the discharge port 13 of the feeding cylinder 1 and the crucible 4 is adjusted to the third value. Among them, the fourth value is greater than the third value.
[0086] In some embodiments, the second distance during the granular silicon feeding process is 40 mm, and the second distance during the small material feeding process is 35 mm, that is, the second distance during the granular silicon feeding process is 14% larger than the second distance during the small material feeding process, that is, the fourth value is 14% larger than the third value.
[0087] In some embodiments, adjusting the second distance between the outlet of the feeding cylinder and the crucible comprises:
[0088] The position of the crucible is adjusted to adjust the second distance between the discharge port of the feeding cylinder and the crucible.
[0089] Combination Figure 2 As shown, the feeding tube 1 is located above the crucible 4. By adjusting the position of the crucible 4 in the vertical direction, the second distance between the discharge port 13 of the feeding tube 1 and the crucible 4 can be adjusted.
[0090] For example, in the process of adding N tubes of silicon material to the crucible 4, when adding the first tube of silicon material (small material) to the crucible 4, the crucible 4 is adjusted to the third position in the vertical direction so that the second distance between the discharge port 13 of the feeding tube 1 and the crucible 4 is the third value. When adding the second tube of silicon material (granular silicon) to the crucible 4, the crucible 4 is adjusted to the second position in the vertical direction so that the second distance between the discharge port 13 of the feeding tube 1 and the crucible 4 is adjusted to the fourth value. When adding the Nth tube of silicon material (small material) to the crucible 4, the crucible 4 is adjusted to the third position in the vertical direction so that the first distance between the discharge port 13 of the feeding tube 1 and the crucible 4 is restored to the third value. Among them, the fourth position is lower than the third position. For example, the fourth position is 10 mm lower than the third position.
[0091] It should be noted that, in the process of adding granular silicon into the crucible 4, the position of the crucible 4 can be adjusted upward once each time a tube of granular silicon is added, but the position of the crucible 4 is still lower than the position of the crucible in the related art.
[0092] In some embodiments, the method for adding silicon material further comprises:
[0093] During the feeding process of the multi-tube silicon material, argon is introduced and the flow rate of argon is adjusted so that the flow rate of argon during the feeding process of the granular silicon is 25%-50% higher than that during the feeding process of the small material.
[0094] It is understandable that the flow rate of argon gas during the granular silicon feeding process may be increased by 25%, 30%, 35%, 40%, 45% or 50% etc. compared with the flow rate of argon gas during the small material feeding process.
[0095] During the feeding process, argon gas is introduced into the single crystal furnace, and the flow rate of argon gas can be adjusted according to the type of silicon material added to the crucible 4, that is, the flow rate of argon gas corresponding to the addition of small materials to the crucible 4 can be different from the flow rate of argon gas corresponding to the addition of granular silicon to the crucible 4.
[0096] Since the granular silicon also contains a certain amount of dust particles, the dust is easy to fly upward and adhere to the surface of the water cooling screen during the granular silicon feeding process. Therefore, in this embodiment, the flow rate of argon gas corresponding to the granular silicon feeding is greater than the flow rate of argon gas corresponding to the small material feeding, that is, the flow rate of argon gas is increased when the granular silicon is fed, so that the argon gas blowing is more sufficient, and more dust can be taken away, reducing the risk of dust flying upward and adhering to the surface of the water cooling screen 3 during the feeding process, thereby reducing the risk of crystal rod breaking during the crystal pulling process due to dust falling.
[0097] For example, in the process of adding N cylinders of silicon material to the crucible 4, when adding the first cylinder of silicon material (small material) to the crucible 4, the flow rate of argon gas is adjusted to the first flow rate. When adding the second cylinder of silicon material (granular silicon) to the crucible 4, the flow rate of argon gas is adjusted from the first flow rate to the second flow rate. When adding the Nth cylinder of silicon material (small material) to the crucible 4, the flow rate of argon gas is adjusted from the second flow rate to the first flow rate. The second flow rate is greater than the first flow rate.
[0098] In some embodiments, the argon flow rate during the granular silicon feeding process is 150 slpm, and the argon flow rate during the small material feeding process is 100 slpm. The argon flow rate during the granular silicon feeding process is 50% higher than the argon flow rate during the small material feeding process, that is, the second flow rate is 50% higher than the first flow rate.
[0099] According to the silicon material feeding method provided in the embodiment of the present application, after each bucket of silicon material is added to the crucible 4, the next bucket of silicon material is added to the crucible 4 at an interval, wherein the interval time is the time required for the solid-liquid ratio in the crucible to reach a preset ratio and the minimum value of the preset interval time, so as to avoid the feeding interval time being too long and the liquid specific gravity in the crucible 4 being too large, thereby reducing the risks of silicon hydrogen jump and silicon splashing of granular silicon and improving the quality of single crystal silicon; when the granular silicon is fed, the heating power of the corresponding heater 5 is lower than the heating power of the corresponding heater 5 when the small material is fed, so as to achieve the purpose of energy saving, and at the same time can prevent the granular silicon from melting too quickly. , and reduce the damage of high temperature to the crucible 4, and extend the life of the crucible 4; when adding granular silicon, increase the distance between the discharge port 13 of the feeding barrel 1 and the water-cooling screen 3, reduce the risk of dust flying upward and adhering to the surface of the water-cooling screen 3 during the feeding process, thereby reducing the risk of crystal rod breakage during the crystal pulling process due to dust falling; when adding granular silicon, increase the distance between the discharge port 13 of the feeding barrel 1 and the crucible 4, thereby increase the distance between the water-cooling screen 3 and the crucible 4, reduce the risk of silicon liquid splashing to the bottom 31 of the water-cooling screen 3 during the silicon melting process, and further reduce the risk of dust flying upward and adhering to the surface of the water-cooling screen 3 during the feeding process.
[0100] The terms "first", "second", etc. in the specification and claims of this application are used to distinguish similar objects, and are not used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable under appropriate circumstances, so that the embodiments of the present application can be implemented in an order other than those illustrated or described herein, and the objects distinguished by "first", "second", etc. are generally of the same type, and the number of objects is not limited. For example, the first object can be one or more.
[0101] In the description of the present application, “plurality” means two or more.
[0102] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0103] Although the embodiments of the present application have been shown and described, those skilled in the art will appreciate that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present application, and that the scope of the present application is defined by the claims and their equivalents.
Claims
1. A method for adding silicon material, It is characterized in that include: Multiple tubes of silicon material are added into the crucible in sequence through a feeding tube, the first tube of silicon material and the last tube of silicon material are small materials, and the remaining tubes of silicon material are granular silicon; During the feeding process of the multi-tube silicon material, the silicon material in the crucible is continuously heated by a heater; The feeding interval time of two adjacent tubes of silicon material is the minimum value of the time required for the solid proportion of the liquid surface of the crucible to reach a preset proportion and the preset interval time.
2. The method for adding silicon material according to claim 1, It is characterized in that The preset proportion is 80%-100%, and the preset interval time is 20min-35min.
3. The method for adding silicon material according to claim 2, It is characterized in that The preset proportion is 95%, and the preset interval time is 25 minutes.
4. The method for adding silicon material according to claim 1, It is characterized in that The remaining silicon material is 100% granular silicon.
5. The method for adding silicon material according to claim 1, It is characterized in that The method further comprises: During the feeding process of the multi-tube silicon material, the heating power of the heater is adjusted so that the heating power during the feeding process of the granular silicon is reduced by 8%-10% compared with the heating power during the feeding process of the small material.
6. The method for adding silicon material according to claim 1, It is characterized in that The method further comprises: During the feeding process of the multi-barrel silicon material, the first distance between the discharge port of the feeding barrel and the water cooling screen is adjusted so that the first distance during the feeding process of the granular silicon is increased by 20%-30% compared with the first distance during the feeding process of the small material.
7. The method for adding silicon material according to claim 6, It is characterized in that The step of adjusting the first distance between the outlet of the charging barrel and the water cooling screen comprises: The position of the discharge port of the feeding barrel is adjusted to adjust the first distance between the discharge port of the feeding barrel and the water cooling screen.
8. The method for adding silicon material according to claim 1, It is characterized in that The method further comprises: During the feeding process of the multi-tube silicon material, the second distance between the discharge port of the feeding tube and the crucible is adjusted so that the second distance during the feeding process of the granular silicon is 10%-15% larger than the second distance during the feeding process of the small material.
9. The method for adding silicon material according to claim 8, It is characterized in that The step of adjusting the second distance between the outlet of the feeding cylinder and the crucible comprises: The position of the crucible is adjusted to adjust a second distance between the discharge port of the feeding cylinder and the crucible.
10. The method for adding silicon material according to any one of claims 1 to 9, It is characterized in that The method further comprises: During the feeding process of the multi-tube silicon material, argon gas is introduced and the flow rate of the argon gas is adjusted so that the flow rate of the argon gas during the feeding process of the granular silicon is increased by 25%-50% compared with the flow rate of the argon gas during the feeding process of the small material.