Filling aid as well as preparation method and application thereof

The combination of filling additives prepared by grafting reaction of thiolated PAMAM and acidified dolomite powder and film-forming agents such as phosphate denaturated starch has solved the problems of insufficient strength and difficulty in desizing the electronic grade glass fiber cloth in the prior art, and achieved the High strength, environmentally friendly sizing effect and good desizing performance.

CN118957981APending Publication Date: 2024-11-15KINGBOARD (LIAN ZHOU) FIBRE GLASS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411011895.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The PVA sizing agent used in the secondary slurry of the existing electronic grade glass fiber cloth has difficulty desizing and environmental pollution. The smear film strength of the starch sizing agent is poor, which affects the strength of the fiber cloth and makes the desorption waste liquid difficult to degrade.

Method used

The filling additive prepared by grafting reaction of thiolated PAMAM and acidified dolomite powder is uniformly dispersed in the sizing agent to increase the strength of the fiber cloth, and the film forming agent and urea composed of phosphate denatured starch and hydroxyalkyl denatured starch are used. , Dioctamine is aided in nano zinc oxide catalyzing to improve the desizing effect.

Benefits of technology

It significantly improves the strength of the electronic grade glass fiber cloth, improves the desizing effect, reduces the biodegradability of the desizing waste liquid, reduces the hairy feathers of the fiber cloth, and improves the stability and coating effect of the serous film.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a filling aid and a preparation method and application thereof, the preparation method comprises the following steps: (1) adding 3.0 G PAMAM and deionized water into a reaction flask, stirring for 10 minutes, introducing nitrogen, dropwise adding ethyl 3-mercaptopropionate after 1 hour, stirring and reacting at 35 DEG C for 24 hours to obtain a reactant, and performing reduced pressure distillation and vacuum drying to obtain sulfhydrylated PAMAM; (2) performing ball milling on dolomite, sieving to obtain dolomite powder, adding into nitric acid, stirring for 1 hour at 80 DEG C, discharging, filtering to obtain filter residues, washing with distilled water to be neutral, and performing vacuum drying to obtain acidified dolomite powder; and (3) adding the sulfhydrylated PAMAM into deionized water, stirring for 10 minutes, adding the acidified dolomite powder, stirring and reacting for 4 hours at the temperature of 50 DEG C, discharging, filtering to obtain filter residues, drying in vacuum, and sieving to obtain the filling aid. The filling aid provided by the invention can be uniformly dispersed in a sizing agent system, so that the strength of the sized electronic-grade glass fiber cloth is effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a filling auxiliary agent and a preparation method and application thereof. Background Art

[0002] Electronic-grade glass fiber cloth is a reinforced composite material for the production of printed circuit boards. It has extremely high requirements for the production processes such as sizing and weaving. In order to ensure the good weaving performance of electronic-grade glass fiber yarn, it is usually necessary to use sizing agent to perform secondary sizing on its surface. At present, the sizing agent used in the secondary sizing of electronic-grade glass fiber cloth warp yarn mostly uses polyvinyl alcohol PVA or starch as the main film-forming agent. PVA has good film-forming properties, excellent mechanical and physical properties of the sizing film, and good miscibility with other sizing agents. However, due to the regular macromolecular chain structure of PVA and a large number of hydroxyl groups, it is difficult to desize and the desizing effect is not good. In addition, the waste liquid generated after desizing is difficult to degrade and has been listed as an environmental pollutant. Some developed countries restrict or even prohibit the use of PVA as a sizing agent. The desizing of starch-based sizing agents is relatively simple and environmentally friendly, but the strength of the sizing film formed by them is not good, which has an adverse effect on the strength of the electronic-grade glass fiber cloth after sizing. Therefore, it is necessary to add filling additives to starch-based sizing agents. Summary of the invention

[0003] The technical problem to be solved by the present invention is to provide a method for preparing a filling auxiliary agent, wherein the prepared filling auxiliary agent can be uniformly dispersed in a sizing agent system, and effectively improves the strength of electronic-grade glass fiber cloth after sizing.

[0004] In order to solve the above technical problems, the technical solution of the present invention is:

[0005] A method for preparing a filling auxiliary agent, characterized in that it comprises the following steps:

[0006] (1) 3.0 g PAMAM and deionized water were added to a reaction flask, and nitrogen was introduced after stirring for 10 minutes. After 1 hour, ethyl 3-mercaptopropionate was added dropwise, and the reaction was stirred at 35° C. for 24 hours to obtain a reactant. The reactant was distilled under reduced pressure and then vacuum dried at 60° C. to constant weight to obtain thiolated PAMAM;

[0007] (2) ball-milling dolomite and passing it through a 200-mesh sieve to obtain dolomite powder, adding the dolomite powder to nitric acid, stirring at 80° C. for 1 hour, filtering the product after discharge to obtain a filter residue, washing the filter residue with distilled water until neutral, and vacuum drying at 60° C. to constant weight to obtain acidified dolomite powder;

[0008] (3) Add the thiolated PAMAM obtained in step (1) into deionized water, stir for 10 minutes, then add the acidified dolomite powder obtained in step (2), stir and react at 50° C. for 4 hours, filter the product after discharge to obtain a filter residue, vacuum dry the filter residue at 60° C. to constant weight, and pass it through a 200-mesh sieve to obtain a filling aid.

[0009] Furthermore, in step (1) of the present invention, the mass ratio of 3.0 g PAMAM, deionized water, and ethyl 3-mercaptopropionate is 1:50:20;

[0010] Furthermore, in step (2) of the present invention, the mass concentration of nitric acid is 20%, and the mass ratio of dolomite powder to nitric acid is 1:10;

[0011] Furthermore, in step (3) of the present invention, the mass ratio of the thiolated PAMAM obtained in step (1), deionized water, and the acidified dolomite powder obtained in step (2) is 0.9:10:1.2.

[0012] Another technical problem to be solved by the present invention is to provide a filling auxiliary prepared by the above preparation method.

[0013] The present invention also provides the use of the filling auxiliary agent in preparing a sizing agent for electronic grade glass fiber cloth.

[0014] Furthermore, the sizing agent for electronic-grade glass fiber cloth of the present invention is made of the following raw materials in parts by weight: 3-5 parts of film-forming agent, 2-3 parts of lubricant, 1-2 parts of antistatic agent, 0.5-1 parts of softener, 5-5.5 parts of polyethylene glycol, 1-1.5 parts of filling aid, 0.5-0.9 parts of other additives, and 85-90 parts of deionized water.

[0015] Furthermore, the film-forming agent of the present invention is composed of phosphate modified starch and hydroxyalkyl modified starch in a mass ratio of 2:3, the lubricant is polyoxyethylene stearate, the antistatic agent is tetradecyl trimethyl ammonium bromide, and the softener is alkylphenol polyoxyethylene ether; the auxiliary agent is prepared by the following steps:

[0016] Urea, dioctylamine, dimethyl sulfoxide and nano zinc oxide were added to a reaction bottle under nitrogen protection, and the mixture was stirred and reacted at 140° C. for 8 hours to obtain a reaction solution. The reaction solution was filtered to obtain a solid. The solid was washed three times with deionized water and then vacuum dried at 60° C. to constant weight to obtain other additives.

[0017] Furthermore, in the preparation step of the auxiliary agent of the present invention, the ratio of urea, dioctylamine, dimethyl sulfoxide and nano zinc oxide is 1.2 mol: 1 mol: 160 mL: 0.06 mol.

[0018] Furthermore, the sizing agent for electronic grade glass fiber cloth of the present invention is prepared by the following steps:

[0019] S1. Weigh each raw material by mass, add the film-forming agent to 10 times its mass of deionized water, stir at a stirring speed of 100 rpm for 20 minutes, stop stirring and let stand for 10-15 hours to obtain a mixed slurry;

[0020] S2. The lubricant, antistatic agent, softener, polyethylene glycol, filling aid, and other additives were added to the remaining deionized water and stirred at a stirring speed of 150 rpm for 30 minutes to obtain a mixed solution;

[0021] S3. The mixed slurry obtained in step S1 and the mixed solution obtained in step S2 are mixed, and stirred at a stirring speed of 100 rpm for 50-70 minutes to obtain a sizing agent for electronic grade glass fiber cloth.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] (1) Dolomite powder is a filling agent with good mechanical properties. However, its dispersibility is poor when directly added to the sizing agent. Therefore, the present invention first treats 3.0G of PAMAM dendrimer with methyl thioglycolate to obtain thiolated PAMAM with a thiol terminal group, ball-mills the dolomite to obtain dolomite powder, and then treats it with nitric acid to obtain acidified dolomite powder. The nitric acid etches the surface of the dolomite powder to increase its surface roughness. At the same time, carboxyl groups are generated on the surface of the dolomite powder. Then, the thiol groups of the thiolated PAMAM are grafted onto the surface of the dolomite powder through a grafting reaction with the carboxyl groups and hydroxyl groups on the surface of the acidified dolomite powder to prepare a filling agent. PAMAM is a dendrimer, so that the filling agent can be evenly dispersed in the sizing agent system, effectively improving the strength of the electronic-grade glass fiber cloth after sizing.

[0024] (2) The film-forming agent used in the sizing agent for electronic-grade glass fiber cloth prepared by the present invention is composed of phosphate modified starch and hydroxyalkyl modified starch. The film-forming agent has good film-forming performance, and the formed film has good stability and coating effect. The desizing waste liquid has good biodegradability and is relatively environmentally friendly.

[0025] (3) The sizing agent for electronic-grade glass fiber cloth prepared by the present invention also uses an auxiliary agent prepared by reaction of urea and dioctylamine under the catalytic action of nano zinc oxide. The auxiliary agent enables the sizing agent to conform to the hairiness of the glass fiber during the weaving process, effectively reducing the hairiness of the electronic-grade glass fiber cloth. In addition, the auxiliary agent can also increase the size film removal rate of the sizing agent during desizing, thereby improving the desizing effect. DETAILED DESCRIPTION

[0026] The present invention will be described in detail below in conjunction with specific embodiments. The illustrative embodiments of the present invention and their descriptions are used to explain the present invention but are not intended to limit the present invention.

[0027] Example 1

[0028] Prepare the filling aid as follows:

[0029] (1) 3.0 g PAMAM and deionized water were added to a reaction flask, and nitrogen was introduced after stirring for 10 minutes. After 1 hour, ethyl 3-mercaptopropionate was added dropwise. The mass ratio of 3.0 g PAMAM, deionized water, and ethyl 3-mercaptopropionate was 1:50:20. The reaction was stirred at 35° C. for 24 hours to obtain a reactant. The reactant was distilled under reduced pressure and then vacuum dried at 60° C. to constant weight to obtain thiolated PAMAM;

[0030] (2) ball-milling dolomite and passing it through a 200-mesh sieve to obtain dolomite powder, adding the dolomite powder to 20% nitric acid at a mass ratio of 1:10, stirring at 80° C. for 1 hour, filtering the product after discharge to obtain a filter residue, washing the filter residue with distilled water until neutral, and vacuum drying at 60° C. to constant weight to obtain acidified dolomite powder;

[0031] (3) adding the thiolated PAMAM obtained in step (1) into deionized water, stirring for 10 minutes, and then adding the acidified dolomite powder obtained in step (2), wherein the mass ratio of the thiolated PAMAM obtained in step (1), deionized water, and the acidified dolomite powder obtained in step (2) is 0.9:10:1.2, and reacting at 50° C. with stirring for 4 hours. After discharging, filtering the product to obtain a filter residue, vacuum drying the filter residue at 60° C. to constant weight, and passing through a 200-mesh sieve to obtain a filling aid.

[0032] Example 2

[0033] The sizing agent for electronic grade glass fiber cloth is prepared from the following raw materials in parts by mass: 4 parts of a film-forming agent composed of phosphate modified starch and hydroxyalkyl modified starch in a mass ratio of 2:3, 2.8 parts of polyoxyethylene stearate, 1.6 parts of tetradecyltrimethylammonium bromide, 0.8 parts of alkylphenol polyoxyethylene ether, 5.2 parts of polyethylene glycol, 1.4 parts of a filling aid prepared in Example 1, 0.8 parts of other additives, and 87 parts of deionized water.

[0034] Other additives are prepared by the following steps:

[0035] Under nitrogen protection, urea, dioctylamine, dimethyl sulfoxide and nano zinc oxide were added to a reaction bottle in a ratio of 1.2 mol: 1 mol: 160 mL: 0.06 mol, and the reaction was stirred at 140 ° C for 8 hours to obtain a reaction solution. The reaction solution was filtered to obtain a solid. The solid was washed three times with deionized water and then vacuum dried at 60 ° C to constant weight to obtain other additives.

[0036] The preparation method of Example 2 comprises the following steps:

[0037] S1. Weigh the raw materials by mass, add a film-forming agent composed of phosphate modified starch and hydroxyalkyl modified starch in a mass ratio of 2:3 to 10 times its mass in deionized water, stir at a stirring speed of 100 rpm for 20 minutes, stop stirring and let stand for 12 hours to obtain a mixed slurry;

[0038] S2. Stearic acid polyoxyethylene ester, tetradecyl trimethyl ammonium bromide, alkylphenol polyoxyethylene ether, polyethylene glycol, filling aids, and other additives were added to the remaining deionized water and stirred at a stirring speed of 150 rpm for 30 minutes to obtain a mixed solution;

[0039] S3. The mixed slurry obtained in step S1 and the mixed solution obtained in step S2 are mixed, and stirred at a stirring speed of 100 rpm for 60 minutes to obtain a sizing agent for electronic grade glass fiber cloth.

[0040] Example 3

[0041] The sizing agent for electronic grade glass fiber cloth is prepared from the following raw materials in parts by mass: 3 parts of a film-forming agent composed of phosphate modified starch and hydroxyalkyl modified starch in a mass ratio of 2:3, 2 parts of polyoxyethylene stearate, 1.2 parts of tetradecyl trimethyl ammonium bromide, 1 part of alkylphenol polyoxyethylene ether, 5 parts of polyethylene glycol, 1.5 parts of the filling auxiliary agent prepared in Example 1, 0.7 parts of an auxiliary agent, and 90 parts of deionized water. The preparation steps of other auxiliary agents are the same as those in Example 2.

[0042] The preparation method of Example 3 comprises the following steps:

[0043] S1. Weigh the raw materials by mass, add a film-forming agent composed of phosphate modified starch and hydroxyalkyl modified starch in a mass ratio of 2:3 to 10 times its mass in deionized water, stir at a stirring speed of 100 rpm for 20 minutes, stop stirring and let stand for 10 hours to obtain a mixed slurry;

[0044] S2. Stearic acid polyoxyethylene ester, tetradecyl trimethyl ammonium bromide, alkylphenol polyoxyethylene ether, polyethylene glycol, filling aids, and other additives were added to the remaining deionized water and stirred at a stirring speed of 150 rpm for 30 minutes to obtain a mixed solution;

[0045] S3. The mixed slurry obtained in step S1 and the mixed solution obtained in step S2 are mixed, and stirred at a stirring speed of 100 rpm for 65 minutes to obtain a sizing agent for electronic grade glass fiber cloth.

[0046] Example 4

[0047] The sizing agent for electronic grade glass fiber cloth is prepared from the following raw materials in parts by mass: 4.5 parts of a film-forming agent composed of phosphate modified starch and hydroxyalkyl modified starch in a mass ratio of 2:3, 3 parts of polyoxyethylene stearate, 1 part of tetradecyl trimethyl ammonium bromide, 0.6 parts of alkylphenol polyoxyethylene ether, 5.5 parts of polyethylene glycol, 1.2 parts of the filling auxiliary agent prepared in Example 1, 0.5 parts of other auxiliary agents, and 88 parts of deionized water. The preparation steps of other auxiliary agents are the same as those in Example 2.

[0048] The preparation method of Example 4 comprises the following steps:

[0049] S1. Weigh the raw materials by mass, add a film-forming agent composed of phosphate modified starch and hydroxyalkyl modified starch in a mass ratio of 2:3 to 10 times its mass in deionized water, stir at a stirring speed of 100 rpm for 20 minutes, stop stirring and let stand for 15 hours to obtain a mixed slurry;

[0050] S2. Stearic acid polyoxyethylene ester, tetradecyl trimethyl ammonium bromide, alkylphenol polyoxyethylene ether, polyethylene glycol, filling aids, and other additives were added to the remaining deionized water and stirred at a stirring speed of 150 rpm for 30 minutes to obtain a mixed solution;

[0051] S3. The mixed slurry obtained in step S1 and the mixed solution obtained in step S2 are mixed, and stirred at a stirring speed of 100 rpm for 70 minutes to obtain a sizing agent for electronic grade glass fiber cloth.

[0052] Example 5

[0053] The sizing agent for electronic grade glass fiber cloth is prepared from the following raw materials in parts by weight: 5 parts of a film-forming agent composed of phosphate modified starch and hydroxyalkyl modified starch in a mass ratio of 2:3, 2.7 parts of polyoxyethylene stearate, 2 parts of tetradecyl trimethyl ammonium bromide, 0.5 parts of alkylphenol polyoxyethylene ether, 5.4 parts of polyethylene glycol, 1 part of the filling auxiliary agent prepared in Example 1, 0.9 parts of auxiliary agent, and 85 parts of deionized water. The preparation steps of the auxiliary agent are the same as those in Example 2.

[0054] The preparation method of Example 5 comprises the following steps:

[0055] S1. Weigh the raw materials by mass, add a film-forming agent composed of phosphate modified starch and hydroxyalkyl modified starch in a mass ratio of 2:3 to 10 times its mass in deionized water, stir at a stirring speed of 100 rpm for 20 minutes, stop stirring and let stand for 14 hours to obtain a mixed slurry;

[0056] S2. Stearic acid polyoxyethylene ester, tetradecyl trimethyl ammonium bromide, alkylphenol polyoxyethylene ether, polyethylene glycol, filling aids, additives were added to the remaining deionized water and stirred at a stirring speed of 150rpm for 30 minutes to obtain a mixed solution;

[0057] S3. The mixed slurry obtained in step S1 and the mixed solution obtained in step S2 are mixed, and stirred at a stirring speed of 100 rpm for 50 minutes to obtain a sizing agent for electronic grade glass fiber cloth.

[0058] Comparative Example 1

[0059] The difference from Example 2 is that the filling aid in the sizing agent raw material for electronic grade glass fiber cloth is replaced by dolomite powder with an average particle size of 200 meshes.

[0060] Comparative Example 2

[0061] The difference from Example 2 is that the raw material of the sizing agent for electronic grade glass fiber cloth does not include an auxiliary agent, thus omitting the step of preparing the auxiliary agent.

[0062] Experimental Example 1: Strong Test

[0063] The sizing agents prepared in Examples 2-5 and Comparative Example 1 were added to the sizing device to perform sizing treatment on the electronic-grade glass fiber yarn, and dried at 130°C to obtain electronic-grade glass fibers with a sizing film on the surface, and then the electronic-grade glass fibers were made into electronic-grade glass fiber cloth. The breaking strength of each electronic-grade glass fiber cloth was tested using an electronic tensile testing machine with reference to JC / T996-2006, and the test results are shown in Table 1:

[0064] Breaking strength(cN) Example 2 966.4 Example 3 966.9 Example 4 965.2 Example 5 964.1 Comparative Example 1 902.8

[0065] Table 1

[0066] As can be seen from Table 1, the breaking strengths of Examples 2-5 of the present invention are all relatively high, indicating that the present invention can effectively improve the strength of electronic-grade glass fiber cloth. Part of the raw materials used in Comparative Example 1 are different from those in Example 2. Compared with Example 2, the breaking strength of Comparative Example 1 is significantly reduced, indicating that compared with dolomite powder, the filling additive prepared by the present invention has a better effect on improving the strength of electronic-grade glass fiber cloth.

[0067] Experimental Example 2: Hairiness Test

[0068] The sizing agents prepared in Examples 2-5 and Comparative Example 2 were added to the sizing device to perform sizing treatment on the electronic-grade glass fiber yarn, and dried at 130°C to obtain electronic-grade glass fibers with a sizing film on the surface, and then the electronic-grade glass fibers were made into electronic-grade glass fiber cloth. The hairiness of each electronic-grade glass fiber cloth was tested with reference to FZ / T01086-2000, and the test results are shown in Table 2:

[0069] Feather content (mg / 500m) Example 2 3.1 Example 3 3.3 Example 4 3.7 Example 5 2.8 Comparative Example 2 6.2

[0070] Table 2

[0071] As can be seen from Table 2, the hairiness of Examples 2-5 of the present invention is relatively small, indicating that the present invention can effectively reduce the hairiness of electronic-grade glass fiber cloth. Part of the raw materials and preparation steps used in Comparative Example 2 are different from those in Example 2. Compared with Example 2, the hairiness of Comparative Example 2 is significantly increased, indicating that the additive prepared by the present invention can effectively reduce the hairiness of electronic-grade glass fiber cloth.

[0072] Experimental Example 3: Desizing Test

[0073] The sizing agents prepared in Examples 2-5 and Comparative Example 2 were added to the sizing device to perform sizing treatment on the electronic-grade glass fiber yarn, and dried at 130°C to obtain electronic-grade glass fibers with a sizing film on the surface. The electronic-grade glass fibers were made into electronic-grade glass fiber cloths, which were desized at 200°C for 15 minutes and then simmered at 380°C for 24 hours. The combustible content of each electronic-grade glass fiber cloth was tested with reference to GB / T9914.2-2013, and the test results are shown in Table 3:

[0074] Combustible content (%) Example 2 0.11 Example 3 0.13 Example 4 0.17 Example 5 0.09 Comparative Example 2 0.43

[0075] Table 3

[0076] As can be seen from Table 3, the combustible content of Examples 2-5 of the present invention is relatively low, indicating that the desizing effect of the sizing agent for electronic-grade glass fiber cloth prepared by the present invention is good. Part of the raw materials and preparation steps used in Comparative Example 2 are different from those in Example 2. Compared with Example 2, the combustible content of Comparative Example 2 is significantly increased, indicating that the auxiliary agent prepared by the present invention can effectively improve the desizing effect of the sizing agent for electronic-grade glass fiber cloth.

[0077] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A method for preparing a filling auxiliary agent, characterized in that: The following steps are involved: (1) 3.0 g PAMAM and deionized water were added to a reaction flask, and nitrogen was introduced after stirring for 10 minutes. After 1 hour, ethyl 3-mercaptopropionate was added dropwise, and the reaction was stirred at 35° C. for 24 hours to obtain a reactant. The reactant was distilled under reduced pressure and then vacuum dried at 60° C. to constant weight to obtain thiolated PAMAM; (2) ball-milling dolomite and passing it through a 200-mesh sieve to obtain dolomite powder, adding the dolomite powder to nitric acid, stirring at 80° C. for 1 hour, filtering the product after discharge to obtain a filter residue, washing the filter residue with distilled water until neutral, and vacuum drying at 60° C. to constant weight to obtain acidified dolomite powder; (3) Add the thiolated PAMAM obtained in step (1) into deionized water, stir for 10 minutes, then add the acidified dolomite powder obtained in step (2), stir and react at 50° C. for 4 hours, filter the product after discharge to obtain a filter residue, vacuum dry the filter residue at 60° C. to constant weight, and pass it through a 200-mesh sieve to obtain a filling aid.

2. The method for preparing a filling auxiliary agent according to claim 1, characterized in that: In the step (1), the mass ratio of 3.0G PAMA, deionized water and ethyl 3-mercaptopropionate is 1:50:

20.

3. The method for preparing a filling auxiliary agent according to claim 1, characterized in that: In the step (2), the mass concentration of nitric acid is 20%, and the mass ratio of dolomite powder to nitric acid is 1:

10.

4. The method for preparing a filling auxiliary agent according to claim 1, characterized in that: In the step (3), the mass ratio of the thiolated PAMAM obtained in the step (1), deionized water, and the acidified dolomite powder obtained in the step (2) is 0.9:10:1.

2.

5. The filling auxiliary agent obtained according to the preparation method of claims 1 to 4.

6. Use of the filling auxiliary according to claim 5 in preparing a sizing agent for electronic grade glass fiber cloth.

7. The use according to claim 6, characterized in that: The electronic grade glass fiber cloth sizing agent is prepared from the following raw materials in parts by weight: 3-5 parts of film former, 2-3 parts of lubricant, 1-2 parts of antistatic agent, 0.5-1 parts of softener, 5-5.5 parts of polyethylene glycol, 1-1.5 parts of filling auxiliary agent, 0.5-0.9 parts of other auxiliary agents and 85-90 parts of deionized water.

8. The use according to claim 6, characterized in that: The film-forming agent is composed of phosphate modified starch and hydroxyalkyl modified starch in a mass ratio of 2:3, the lubricant is polyoxyethylene stearate, the antistatic agent is tetradecyl trimethyl ammonium bromide, and the softener is alkylphenol polyoxyethylene ether; the other auxiliary agents are prepared by the following steps: Urea, dioctylamine, dimethyl sulfoxide and nano zinc oxide were added to a reaction bottle under nitrogen protection, and the mixture was stirred and reacted at 140° C. for 8 hours to obtain a reaction solution. The reaction solution was filtered to obtain a solid. The solid was washed three times with deionized water and then vacuum dried at 60° C. to constant weight to obtain other additives.

9. The use according to claim 8, characterized in that: In the preparation step of the other auxiliary agents, the ratio of urea, dioctylamine, dimethyl sulfoxide and nano zinc oxide is 1.2 mol: 1 mol: 160 mL: 0.06 mol.

10. The use according to any one of claims 7 to 9, characterized in that: The electronic grade glass fiber cloth sizing agent is prepared by the following steps: S1. Weigh each raw material by mass, add the film-forming agent to 10 times its mass of deionized water, stir at a stirring speed of 100 rpm for 20 minutes, stop stirring and let stand for 10-15 hours to obtain a mixed slurry; S2. The lubricant, antistatic agent, softener, polyethylene glycol, filling aid, and other additives were added to the remaining deionized water and stirred at a stirring speed of 150 rpm for 30 minutes to obtain a mixed solution; S3. The mixed slurry obtained in step S1 and the mixed solution obtained in step S2 are mixed, and stirred at a stirring speed of 100 rpm for 50-70 minutes to obtain a sizing agent for electronic grade glass fiber cloth.