Graphene antistatic cashmere fabric and preparation method thereof
By plasma treatment of graphene fibers and using anti-fouling finishing agents of lithium xiashi powder and cesium tungsten bronze powder to form a nanoprotective layer, the problem of poor anti-fouling performance of graphene anti-static cashmere fabrics is solved, and the long-term fabric is achieved Cleanliness and durability enhancements.
Patent Information
- Application Number
- CN202410993563.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing graphene anti-static cashmere fabric has poor anti-fouling performance and is prone to absorb dust and stains, and needs to be cleaned and repaired frequently.
Modified graphene fibers are treated with plasma, and cashmere fibers are placed in antifouling finishing agent made of lithium cylindrical powder and cesium tungsten bronze powder for soaking to form a stable nanoprotective layer, combined with ultrasonic oscillation technology to improve Anti-fouling performance.
The formed nanoprotective layer significantly improves the anti-fouling performance of the fabric, allowing it to remain clean for a long time, significantly improves the anti-fouling effect, and improves durability and anti-aging performance.
Smart Images

Figure BDA0004959516190000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fabric preparation, and in particular to a graphene antistatic cashmere fabric and a preparation method thereof. Background Art
[0002] Graphene is an emerging material that has been widely studied in recent years. It is ultra-thin, has excellent conductivity, super hardness, and is light and soft. It has great application prospects in aerospace, weapons and equipment, major infrastructure, as well as new energy, new energy vehicles, energy conservation and environmental protection, and electronic information.
[0003] Research shows that graphene materials can be applied to some functional fabrics, especially graphene materials have extremely excellent conductive properties and can be prepared into antistatic fabrics. Some graphene cashmere antistatic fabrics have appeared on the market. For example, the patent document with publication number CN113862853B discloses an antistatic and anti-pilling cashmere graphene blended yarn and its preparation process. The graphene composite fiber is mixed with cashmere fiber, and then a series of spinning processes are performed to obtain cashmere graphene blended yarn. The cashmere graphene blended yarn is prepared into fabrics, which can achieve good antistatic effect.
[0004] However, due to the strong adsorption capacity of cashmere and its soft and delicate texture, graphene anti-static cashmere fabric easily absorbs dust and stains, resulting in poor anti-fouling performance and requires frequent cleaning and care. Summary of the invention
[0005] The object of the present invention is to provide a graphene antistatic cashmere fabric and a preparation method thereof, which solves the problem that the existing graphene antistatic cashmere fabric has poor antifouling performance.
[0006] The present invention achieves the above-mentioned purpose through the following technical solutions:
[0007] A method for preparing graphene antistatic cashmere fabric, characterized in that the steps include:
[0008] S1, preparing graphene fiber, and subjecting it to plasma treatment to obtain modified graphene fiber;
[0009] S2, taking cashmere fiber, placing it in an antifouling finishing agent for immersion treatment, then taking out the woven fabric, washing and drying it, to obtain modified cashmere fiber;
[0010] Wherein, the raw materials of the antifouling finishing agent include 10-20 parts of eucryptite powder, 1-5 parts of cesium tungsten bronze powder and 40-60 parts of deionized water in parts by weight;
[0011] S3, weighing the modified graphene fiber and the modified cashmere fiber in a mass ratio of 1:10-20 and mixing them evenly, adding a wool-forming agent and then layering them for 1-3 times, and then performing a wool-suffocating treatment for 12-16 hours to obtain a mixed fiber;
[0012] S4, taking the mixed fiber, and sequentially performing the steps of opening and cleaning, carding, drawing, roving, spinning and winding to obtain a blended yarn;
[0013] S5. Taking the blended yarn for weaving, the graphene antistatic cashmere fabric is obtained.
[0014] A further improvement is that the specific operation of preparing graphene fibers is:
[0015] Preparing a spinning solution: taking a graphene oxide solution, adjusting the pH to 6-10, and obtaining a spinning solution;
[0016] Preparing raw fibers: taking the spinning solution through a 0.5-1 mm spinneret and injecting it into a coagulation bath at a speed of 0.2-1 mL / min, and then drying to obtain raw fibers;
[0017] Stretching and shaping: placing the original fiber in a protective atmosphere furnace, controlling the temperature to 200-400° C., and applying tension to the original fiber to make the fiber length stretching rate 28-32%;
[0018] Reduction: Take the original fibers after stretching and shaping, place them in a reducing agent for reduction for 1-5 hours, wash and dry to obtain graphene oxide fibers.
[0019] A further improvement is that the reducing agent is selected from one of hydrazine hydrate, hydrobromic acid, sodium borohydride or hydroiodic acid.
[0020] A further improvement is that the plasma treatment refers to: using a glow discharge low-temperature plasma instrument to perform argon plasma treatment, with a treatment pressure of 20 Pa, a treatment power of 100 W, and a treatment time of 50-60 s.
[0021] A further improvement is that the soaking treatment refers to: controlling the temperature of the antifouling finishing agent to 55-65° C. and soaking the fabric in the antifouling finishing agent for 6-10 hours.
[0022] A further improvement is that during the soaking process, ultrasonic oscillation treatment with a frequency of 20-25 kHz and a power of 300-450 W is applied to the antifouling finishing agent.
[0023] The present invention also provides a graphene antistatic cashmere fabric, which is prepared by the above preparation method.
[0024] The beneficial effects of the present invention are:
[0025] (1) The present invention adopts an antifouling finishing agent made of eucryptite powder and cesium tungsten bronze powder, which are fused to form a stable nano protective layer, which is attached to the surface of cashmere fiber to play an antifouling property, and the ultraviolet shielding performance of cesium tungsten bronze powder is utilized to improve the anti-aging performance of the protective layer, while improving the surface activity of eucryptite and enhancing the adhesion of eucryptite, so that the antifouling effect is maintained for a long time;
[0026] (2) The present invention enhances the biocompatibility of graphene fibers by subjecting them to plasma treatment, thereby increasing the bonding strength between the graphene fibers and the modified cashmere fibers and improving durability. DETAILED DESCRIPTION
[0027] The present application is further described in detail below in conjunction with specific embodiments. It is necessary to point out that the following specific implementation methods are only used to further illustrate the present application and cannot be understood as limiting the scope of protection of the present application. Technical personnel in this field can make some non-essential improvements and adjustments to the present application based on the above application content.
[0028] 1. Main instruments and materials
[0029] (1) Plasma instrument: HD-1B glow discharge low-temperature plasma instrument is selected;
[0030] (2) Ultrasonic generator: purchased from Foshan Lintai Ultrasonic Cleaning Equipment Technology Co., Ltd.
[0031] (3) Cashmere fiber: purchased from Qinghe, Hebei, variety Qinghe white cashmere;
[0032] (4) Graphene oxide solution: 100 g of graphite powder and 50 g of sodium nitrate were placed in a glass container, and 2.3 L of concentrated sulfuric acid was slowly added to the container. The mixture was stirred for 2.5 h in an ice bath. 600 g of potassium permanganate was weighed and slowly added to the container. The temperature was maintained at 20 °C and the stirring was continued for 1 h. The ice bath was then removed and the container was placed in a 35 °C water bath. The mixture was stirred for 2.5 h to obtain a dark brown paste. 4.8 L of hot water was added to the mixture and stirred. After the temperature reached 98 °C, the mixture was quickly transferred to a 98 °C hot water bath and stirred at a constant temperature for 5 min. The hot water bath was then removed and the mixture was transferred to an ordinary water bath and stirred for 30 min. 1.4 L of 50 °C deionized water and 1 L of 1.5 L of 2.5 L of 4.8 L of 5.5 L of 2.5 L of 1.5 L of 2.5 L of 2.5 L of 4.8 ... 30% hydrogen peroxide, the reactant changes from brown to yellow, and after stirring for another 12 minutes, the reactant is taken out and filtered, and the filter cake is washed and centrifuged 3 times with 3% hydrochloric acid, and then redispersed in deionized water to obtain a brown suspension. After dialysis for 3 days, the graphene oxide solution is obtained.
[0033] (5) Eucryptite powder: β-eucryptite is used in this paper. The specific preparation method is as follows: Si(OC2H5)4 is pre-hydrolyzed in 75% ethanol water to obtain Si(OH)4 solution, LiNO3 and Al(NO3)3·9H2O are dissolved in anhydrous ethanol, and evenly mixed with the prepared Si(OH)4 solution. Then, it is added dropwise to a citric acid ethanol solution (the ratio of citric acid to metal ions is 2:1), and a small amount of polyethylene glycol is added as a dispersant. The pH value of the solution is 3. The solution is then placed in a constant temperature water bath at 75°C and heated to form a transparent gel after 100 minutes. Finally, the obtained gel is dried to obtain a loose brown-yellow dry gel powder, which is then calcined at 900°C for 3 hours to obtain β-eucryptite powder with a particle size of 20-25nm.
[0034] (6) Cesium tungsten bronze powder: Weigh tungstic acid and cesium hydroxide in a mass ratio of 3:1 and grind until the mixture is uniform; put the ground material into a sealed container and then put it into a muffle furnace for reaction at 800°C for 2 hours; thus, cesium tungsten bronze powder is obtained.
[0035] 2. Implementation of the experiment
[0036] Example 1
[0037] A method for preparing graphene antistatic cashmere fabric, comprising the steps of:
[0038] S1, preparing graphene fiber, and subjecting it to plasma treatment to obtain modified graphene fiber;
[0039] Among them, the specific operation of preparing graphene fiber is:
[0040] Preparing a spinning solution: taking a graphene oxide solution, adjusting the pH to 6, and obtaining a spinning solution;
[0041] Preparation of raw fibers: taking the spinning solution through a 0.5 mm spinneret and injecting it into a coagulation bath at a speed of 0.2 mL / min, and then drying to obtain raw fibers;
[0042] Stretching and shaping: placing the original fiber in a nitrogen protective atmosphere furnace, controlling the temperature to 200° C., and applying tension to the original fiber to make the fiber length stretching rate reach 28%;
[0043] Reduction: Take the original fiber after stretching and shaping, place it in a hydrazine hydrate reducing agent for reduction for 1 hour, wash and dry to obtain graphene oxide fiber.
[0044] Plasma treatment refers to: using a glow discharge low-temperature plasma instrument to perform argon plasma treatment, with a treatment pressure of 20 Pa, a treatment power of 100 W, and a treatment time of 50 s.
[0045] S2, taking cashmere fiber, placing it in an antifouling finishing agent for immersion treatment, then taking out the woven fabric, washing and drying it, to obtain modified cashmere fiber;
[0046] Among them, the raw materials of the anti-fouling finishing agent include 10 parts of eucryptite powder, 1 part of cesium tungsten bronze powder and 40 parts of deionized water, calculated by weight; the immersion treatment refers to: controlling the temperature of the anti-fouling finishing agent to 55°C, placing the fabric in the anti-fouling finishing agent and immersing it for 6 hours, and applying ultrasonic oscillation treatment with a frequency of 20kHz and a power of 300W to the anti-fouling finishing agent during the immersion process.
[0047] S3, weighing the modified graphene fiber and the modified cashmere fiber in a mass ratio of 1:10 and mixing them evenly, adding a wool-mixing agent (based on the total weight of the fiber, including 4% wool-mixing oil FX-905 and 1% antistatic agent FX-AS301, the same below), and then layering them once, and then performing a wool-smothering treatment (temperature 25° C., humidity 80%, the same below) for 12 hours to obtain a mixed fiber;
[0048] S4, take the mixed fiber, and carry out the opening and cleaning, carding, drawing, roving, spinning and winding steps in sequence (in the opening and cleaning step, the combing needle beater speed is 480r / min, and the comprehensive beater speed is 820r / min; in the carding step, the basis weight is 17g / 5m, the cylinder speed is 320r / min, the doffer speed is 18r / min, and the flat plate speed is 85mm / min; in the drawing step, the first 6 roots are combined, the drafting multiple is 9 times, the drawing dry weight is 18g / 5m, and the sliver delivery speed is 220m / min; the second 6 roots are combined, the drafting multiple is 8 times, and the drawing dry weight is 18 g / 5m, sliver delivery speed 200m / min; in the roving process, dry weight 3g / 5m, spindle speed 620r / min, front roller speed 200r / min, back zone stretching multiple 1.5 times, twist coefficient 85; in the spun yarn process, dry weight 2g / 100m, spindle speed 14000r / min, front roller speed 200r / min, back zone stretching multiple 1.5 times, total drafting multiple 25 times, twist coefficient 350, jaw spacing 2.6mm; in the winding process, production tension 200, speed 1200m / min. The same below), to obtain blended yarn;
[0049] S5. Take the blended yarn and weave it according to a conventional process to obtain the graphene antistatic cashmere fabric.
[0050] Example 2
[0051] A method for preparing graphene antistatic cashmere fabric, comprising the steps of:
[0052] S1, preparing graphene fiber, and subjecting it to plasma treatment to obtain modified graphene fiber;
[0053] Among them, the specific operation of preparing graphene fiber is:
[0054] Preparing a spinning solution: taking a graphene oxide solution, adjusting the pH to 8, and obtaining a spinning solution;
[0055] Preparation of original fibers: taking the spinning solution through a 0.6 mm spinneret and injecting it into a coagulation bath at a speed of 0.4 mL / min, and then drying to obtain original fibers;
[0056] Stretching and shaping: placing the original fiber in a nitrogen protective atmosphere furnace, controlling the temperature to 300° C., and applying tension to the original fiber to make the fiber length stretching rate 30%;
[0057] Reduction: Take the original fibers after stretching and shaping, place them in a hydrobromic acid reducing agent for reduction for 3 hours, wash and dry to obtain graphene oxide fibers.
[0058] Plasma treatment refers to: using a glow discharge low-temperature plasma instrument to perform argon plasma treatment, with a treatment pressure of 20 Pa, a treatment power of 100 W, and a treatment time of 55 s.
[0059] S2, taking cashmere fiber, placing it in an antifouling finishing agent for immersion treatment, then taking out the woven fabric, washing and drying it, to obtain modified cashmere fiber;
[0060] Among them, the raw materials of the anti-fouling finishing agent include 15 parts of eucryptite powder, 3 parts of cesium tungsten bronze powder and 50 parts of deionized water, calculated by weight; the immersion treatment refers to: controlling the temperature of the anti-fouling finishing agent to 60°C, placing the fabric in the anti-fouling finishing agent and immersing it for 8 hours, and applying ultrasonic oscillation treatment with a frequency of 22kHz and a power of 380W to the anti-fouling finishing agent during the immersion process.
[0061] S3, weighing the modified graphene fiber and the modified cashmere fiber in a mass ratio of 1:15 and mixing them evenly, adding a wool-making agent and then layering them twice, and then performing a wool-smothering treatment for 14 hours to obtain a mixed fiber;
[0062] S4, taking the mixed fiber, and sequentially performing the steps of opening and cleaning, carding, drawing, roving, spinning and winding to obtain a blended yarn;
[0063] S5. Take the blended yarn and weave it according to a conventional process to obtain the graphene antistatic cashmere fabric.
[0064] Example 3
[0065] A method for preparing graphene antistatic cashmere fabric, comprising the steps of:
[0066] S1, preparing graphene fiber, and subjecting it to plasma treatment to obtain modified graphene fiber;
[0067] Among them, the specific operation of preparing graphene fiber is:
[0068] Preparing a spinning solution: taking a graphene oxide solution, adjusting the pH to 10, and obtaining a spinning solution;
[0069] Preparation of raw fibers: taking the spinning solution through a 1 mm spinneret and injecting it into a coagulation bath at a speed of 1 mL / min, and then drying to obtain raw fibers;
[0070] Stretching and shaping: placing the original fiber in a nitrogen protective atmosphere furnace, controlling the temperature to 400° C., and applying tension to the original fiber to make the fiber length stretching rate 32%;
[0071] Reduction: Take the original fibers after stretching and shaping, place them in a hydroiodic acid reducing agent for reduction for 5 hours, wash and dry, and then obtain graphene oxide fibers.
[0072] Plasma treatment refers to: using a glow discharge low-temperature plasma instrument to perform argon plasma treatment, with a treatment pressure of 20 Pa, a treatment power of 100 W, and a treatment time of 60 s.
[0073] S2, taking cashmere fiber, placing it in an antifouling finishing agent for immersion treatment, then taking out the woven fabric, washing and drying it, to obtain modified cashmere fiber;
[0074] Among them, the raw materials of the anti-fouling finishing agent include 20 parts of eucryptite powder, 5 parts of cesium tungsten bronze powder and 60 parts of deionized water, calculated by weight; the immersion treatment refers to: controlling the temperature of the anti-fouling finishing agent to 65°C, placing the fabric in the anti-fouling finishing agent and immersing it for 10 hours, and applying ultrasonic oscillation treatment with a frequency of 25kHz and a power of 450W to the anti-fouling finishing agent during the immersion process.
[0075] S3, weighing the modified graphene fiber and the modified cashmere fiber in a mass ratio of 1:20 and mixing them evenly, adding a wool-forming agent and then layering them for 3 times, and then performing a wool-suffocating treatment for 16 hours to obtain a mixed fiber;
[0076] S4, taking the mixed fiber, and sequentially performing the steps of opening and cleaning, carding, drawing, roving, spinning and winding to obtain a blended yarn;
[0077] S5. Take the blended yarn and weave it according to a conventional process to obtain the graphene antistatic cashmere fabric.
[0078] Comparative Example 1
[0079] A method for preparing graphene antistatic cashmere fabric, comprising the steps of:
[0080] S1. Prepare graphene fiber, the specific operation is as follows:
[0081] Preparing a spinning solution: taking a graphene oxide solution, adjusting the pH to 8, and obtaining a spinning solution;
[0082] Preparation of original fibers: taking the spinning solution through a 0.6 mm spinneret and injecting it into a coagulation bath at a speed of 0.4 mL / min, and then drying to obtain original fibers;
[0083] Stretching and shaping: placing the original fiber in a nitrogen protective atmosphere furnace, controlling the temperature to 300° C., and applying tension to the original fiber to make the fiber length stretching rate 30%;
[0084] Reduction: Take the original fibers after stretching and shaping, place them in a hydrobromic acid reducing agent for reduction for 3 hours, wash and dry to obtain graphene oxide fibers.
[0085] Plasma treatment refers to: using a glow discharge low-temperature plasma instrument to perform argon plasma treatment, with a treatment pressure of 20 Pa, a treatment power of 100 W, and a treatment time of 55 s.
[0086] S2, taking cashmere fiber, placing it in an antifouling finishing agent for immersion treatment, then taking out the woven fabric, washing and drying it, to obtain modified cashmere fiber;
[0087] Among them, the raw materials of the anti-fouling finishing agent include 15 parts of eucryptite powder, 3 parts of cesium tungsten bronze powder and 50 parts of deionized water, calculated by weight; the immersion treatment refers to: controlling the temperature of the anti-fouling finishing agent to 60°C, placing the fabric in the anti-fouling finishing agent and immersing it for 8 hours, and applying ultrasonic oscillation treatment with a frequency of 22kHz and a power of 380W to the anti-fouling finishing agent during the immersion process.
[0088] S3, weighing graphene fiber and modified cashmere fiber in a mass ratio of 1:15 and mixing them evenly, adding a wool-making agent and then layering them twice, and then performing a wool-smothering treatment for 14 hours to obtain a mixed fiber;
[0089] S4, taking the mixed fiber, and sequentially performing the steps of opening and cleaning, carding, drawing, roving, spinning and winding to obtain a blended yarn;
[0090] S5. Take the blended yarn and weave it according to a conventional process to obtain the graphene antistatic cashmere fabric.
[0091] Comparative Example 2
[0092] A method for preparing graphene antistatic cashmere fabric, comprising the steps of:
[0093] S1, preparing graphene fiber, and subjecting it to plasma treatment to obtain modified graphene fiber;
[0094] Among them, the specific operation of preparing graphene fiber is:
[0095] Preparing a spinning solution: taking a graphene oxide solution, adjusting the pH to 8, and obtaining a spinning solution;
[0096] Preparation of original fibers: taking the spinning solution through a 0.6 mm spinneret and injecting it into a coagulation bath at a speed of 0.4 mL / min, and then drying to obtain original fibers;
[0097] Stretching and shaping: placing the original fiber in a nitrogen protective atmosphere furnace, controlling the temperature to 300° C., and applying tension to the original fiber to make the fiber length stretching rate 30%;
[0098] Reduction: Take the original fibers after stretching and shaping, place them in a hydrobromic acid reducing agent for reduction for 3 hours, wash and dry to obtain graphene oxide fibers.
[0099] Plasma treatment refers to: using a glow discharge low-temperature plasma instrument to perform argon plasma treatment, with a treatment pressure of 20 Pa, a treatment power of 100 W, and a treatment time of 55 s.
[0100] S2, taking cashmere fiber, placing it in an antifouling finishing agent for immersion treatment, then taking out the woven fabric, washing and drying it, to obtain modified cashmere fiber;
[0101] Among them, according to the weight percentage, the raw materials of the anti-fouling finishing agent include 18 parts of eucryptite powder and 50 parts of deionized water; the soaking treatment refers to: controlling the temperature of the anti-fouling finishing agent to 60°C, placing the fabric in the anti-fouling finishing agent and soaking it for 8 hours, and applying ultrasonic oscillation treatment with a frequency of 22kHz and a power of 380W to the anti-fouling finishing agent during the soaking process.
[0102] S3, weighing the modified graphene fiber and the modified cashmere fiber in a mass ratio of 1:15 and mixing them evenly, adding a wool-making agent and then layering them twice, and then performing a wool-smothering treatment for 14 hours to obtain a mixed fiber;
[0103] S4, taking the mixed fiber, and sequentially performing the steps of opening and cleaning, carding, drawing, roving, spinning and winding to obtain a blended yarn;
[0104] S5. Take the blended yarn and weave it according to a conventional process to obtain the graphene antistatic cashmere fabric.
[0105] Comparative Example 3
[0106] A method for preparing graphene antistatic cashmere fabric, comprising the steps of:
[0107] S1, preparing graphene fiber, and subjecting it to plasma treatment to obtain modified graphene fiber;
[0108] Among them, the specific operation of preparing graphene fiber is:
[0109] Preparing a spinning solution: taking a graphene oxide solution, adjusting the pH to 8, and obtaining a spinning solution;
[0110] Preparation of original fibers: taking the spinning solution through a 0.6 mm spinneret and injecting it into a coagulation bath at a speed of 0.4 mL / min, and then drying to obtain original fibers;
[0111] Stretching and shaping: placing the original fiber in a nitrogen protective atmosphere furnace, controlling the temperature to 300° C., and applying tension to the original fiber to make the fiber length stretching rate 30%;
[0112] Reduction: Take the original fibers after stretching and shaping, place them in a hydrobromic acid reducing agent for reduction for 3 hours, wash and dry to obtain graphene oxide fibers.
[0113] Plasma treatment refers to: using a glow discharge low-temperature plasma instrument to perform argon plasma treatment, with a treatment pressure of 20 Pa, a treatment power of 100 W, and a treatment time of 55 s.
[0114] S2, taking cashmere fiber, placing it in an antifouling finishing agent for immersion treatment, then taking out the woven fabric, washing and drying it, to obtain modified cashmere fiber;
[0115] Among them, the raw materials of the anti-fouling finishing agent include 18 parts of cesium tungsten bronze powder and 50 parts of deionized water in parts by weight; the immersion treatment refers to: controlling the temperature of the anti-fouling finishing agent to 60°C, placing the fabric in the anti-fouling finishing agent and immersing it for 8 hours, and applying ultrasonic oscillation treatment with a frequency of 22kHz and a power of 380W to the anti-fouling finishing agent during the immersion process.
[0116] S3, weighing the modified graphene fiber and the modified cashmere fiber in a mass ratio of 1:15 and mixing them evenly, adding a wool-making agent and then layering them twice, and then performing a wool-smothering treatment for 14 hours to obtain a mixed fiber;
[0117] S4, taking the mixed fiber, and sequentially performing the steps of opening and cleaning, carding, drawing, roving, spinning and winding to obtain a blended yarn;
[0118] S5. Take the blended yarn and weave it according to a conventional process to obtain the graphene antistatic cashmere fabric.
[0119] Blank group
[0120] A method for preparing graphene antistatic cashmere fabric, comprising the steps of:
[0121] S1. Weigh graphene fiber (prepared in the same manner as in Example 2) and cashmere fiber in a mass ratio of 1:15 and mix them evenly. After adding a wool-forming agent, lay the fibers twice and perform a wool-smothering treatment for 14 hours to obtain mixed fibers.
[0122] S2, taking the mixed fiber, and sequentially performing the steps of opening and cleaning, carding, drawing, roving, spinning and winding to obtain a blended yarn;
[0123] S3, taking the blended yarn and weaving it according to a conventional process to obtain the graphene antistatic cashmere fabric.
[0124] 3. Performance Test
[0125] The graphene antistatic cashmere fabric samples prepared in Examples 1-3, Comparative Examples 1-3 and the blank group were taken and the following performance tests were performed respectively:
[0126] Antifouling performance: Refer to GB / T 30159.1-2013 "Testing and evaluating the antifouling performance of textiles Part 1: Antifouling", and use the liquid staining method to test the sample. The specific process is: take 2 layers of filter paper and place them on a smooth horizontal surface, place the sample with the front side facing up and flat on the filter paper, and use a dropper to drop about 0.05mL of soy sauce liquid on each of the three parts of the sample, with a dropper. The distance between each drop is at least 50mm, and the dropper mouth is about 6mm away from the sample surface; after the sample is left to stand for 30s, observe each drop at a viewing angle of about 45° for rating. The rating standards refer to Table 1 below. Then wash the sample 20 times and repeat the above rating process.
[0127] Table 1: Contamination levels
[0128] Contamination level Contamination status description Level 5 The droplet is clear and has a good arc shape with a large contact angle. The droplet does not wet the contact surface of the sample. Level 4 The surface where the droplet contacts the sample is partially or completely dark, and about three-quarters of the liquid remains on the sample surface. Level 3 The surface of the droplet in contact with the sample is partially or completely dark, and about half of the liquid remains on the surface of the sample. Level 2 The surface of the droplet in contact with the sample is partially or completely dark, and about a quarter of the liquid volume remains on the surface of the sample Level 1 The droplet disappears on the sample surface and wets it completely
[0129] 4. Results Analysis
[0130] The test results of the above antifouling performance are summarized in Table 2 below:
[0131] Table 2: Antifouling performance test results
[0132]
[0133] As can be seen from Table 2 above, the antifouling properties of the graphene antistatic cashmere fabrics prepared in Examples 1-3 of the present invention before and after washing are very outstanding, reaching level 5, which is significantly better than the blank group, which shows that the present invention effectively solves the problem of poor antifouling properties of existing graphene antistatic cashmere fabrics. In Comparative Example 1, due to the plasma treatment process of the graphene fiber, the antifouling level before washing is reduced to level 4, and further reduced to level 3 after washing; Comparative Examples 2 and Comparative Examples 3 use only one component of eucryptite powder or cesium tungsten bronze powder in the antifouling finishing agent, so that the antifouling properties before and after washing are significantly reduced, which shows that both are indispensable, and only the fusion of the two can form a stable nano protective layer and maintain high efficiency for a long time.
[0134] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. A method for preparing graphene antistatic cashmere fabric, characterized in that the steps include: S1, preparing graphene fiber, and subjecting it to plasma treatment to obtain modified graphene fiber; S2, taking cashmere fiber, placing it in an antifouling finishing agent for immersion treatment, then taking out the woven fabric, washing and drying it, to obtain modified cashmere fiber; Wherein, the raw materials of the antifouling finishing agent include 10-20 parts of eucryptite powder, 1-5 parts of cesium tungsten bronze powder and 40-60 parts of deionized water in parts by weight; S3, weighing the modified graphene fiber and the modified cashmere fiber in a mass ratio of 1:10-20 and mixing them evenly, adding a wool-forming agent and then layering them for 1-3 times, and then performing a wool-suffocating treatment for 12-16 hours to obtain a mixed fiber; S4, taking the mixed fiber, and sequentially performing the steps of opening and cleaning, carding, drawing, roving, spinning and winding to obtain a blended yarn; S5. Taking the blended yarn for weaving, the graphene antistatic cashmere fabric is obtained.
2. The method for preparing a graphene antistatic cashmere fabric according to claim 1, characterized in that: The specific operation of preparing graphene fiber is as follows: Preparing a spinning solution: taking a graphene oxide solution, adjusting the pH to 6-10, and obtaining a spinning solution; Preparing raw fibers: taking the spinning solution through a 0.5-1 mm spinneret and injecting it into a coagulation bath at a speed of 0.2-1 mL / min, and then drying to obtain raw fibers; Stretching and shaping: placing the original fiber in a protective atmosphere furnace, controlling the temperature to 200-400° C., and applying tension to the original fiber to make the fiber length stretching rate 28-32%; Reduction: Take the original fibers after stretching and shaping, place them in a reducing agent for reduction for 1-5 hours, wash and dry, and then obtain graphene oxide fibers.
3. The method for preparing a graphene antistatic cashmere fabric according to claim 2, characterized in that: The reducing agent is selected from one of hydrazine hydrate, hydrobromic acid, sodium borohydride or hydroiodic acid.
4. The method for preparing a graphene antistatic cashmere fabric according to claim 1, characterized in that: The plasma treatment refers to: using a glow discharge low-temperature plasma instrument to perform argon plasma treatment, with a treatment pressure of 20 Pa, a treatment power of 100 W, and a treatment time of 50-60 s.
5. The method for preparing a graphene antistatic cashmere fabric according to claim 1, characterized in that: The soaking treatment refers to: controlling the temperature of the antifouling finishing agent to 55-65° C. and soaking the fabric in the antifouling finishing agent for 6-10 hours.
6. The method for preparing a graphene antistatic cashmere fabric according to claim 5, characterized in that: During the soaking process, the antifouling finishing agent is subjected to ultrasonic oscillation treatment with a frequency of 20-25 kHz and a power of 300-450 W.
7. A graphene antistatic cashmere fabric, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 6.
Citation Information
Cited By
Anti-pilling knitted fabric and preparation method thereof
CN119162832A
Wear-resistant nanofiber reinforced protective graphene fiber as well as preparation method and application thereof
CN119900120A
Wear-resistant nanofiber-reinforced protective graphene fibers and their preparation methods and applications
CN119900120B
Cashmere and graphene fiber blending process
CN120291348A