Anti-wrinkle antibacterial fabric and preparation method thereof

CN118957991APending Publication Date: 2024-11-15SHISHI YUSHENG DINGFENG WEAVING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410881486.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-03
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Traditional anti-wrinkle technologies such as high-temperature ironing and formaldehyde derivative finishing have short-term effects and potential health risks, making it difficult to maintain the wrinkle resistance and safety of the fabric under external forces such as washing.

Method used

The crosslinking agent obtained by copolymerizing unsaturated dicarboxylic acid monomer, isocyanate ethyl acrylate, styrene and other monomers is used to form a stable crosslinking agent. , used for fabric finishing and added antibacterial agents to improve antibacterial performance.

Benefits of technology

It achieves good wrinkle recovery and long-term antibacterial properties of the fabric under water washing conditions, while ensuring the mechanical strength and whiteness of the fabric.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004924666850000101
    Figure BDA0004924666850000101
Patent Text Reader

Abstract

The invention discloses an anti-wrinkle antibacterial fabric and a preparation method thereof.The fabric is treated with a finishing agent, and every 1000 mL of the finishing agent comprises 40-70 g of a cross-linking agent, 2-5 g of a cross-linking activator, 5-15 g of a surfactant and 10-20 g of an antibacterial agent; the cross-linking agent is obtained by free radical copolymerization of the following reaction monomers in parts by mass: 10-20 parts of unsaturated dicarboxylic acid monomer, 5-10 parts of styrene and 2-5 parts of isocyanate ethyl acrylate, and the mass ratio of the unsaturated dicarboxylic acid monomer to the isocyanate ethyl acrylate is 1: (0.12-0.2). The fabric provided by the invention has good crease resistance, strength performance and apparent performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of functional fabrics, and in particular to an anti-wrinkle and antibacterial fabric and a preparation method thereof. Background Art

[0002] Cotton, silk, linen and other hydrophilic fiber fabrics are widely welcomed in the clothing industry due to their excellent moisture absorption, breathability and comfort. The cellulose structure of these fabrics contains abundant hydroxyl groups, which form a dense hydrogen bond network on the cellulose molecular chain, giving the cellulose and the cotton fibers it constitutes a certain rigidity and structural stability. However, during washing, polar water molecules penetrate into the fiber and interfere with the hydrogen bond network, causing some hydrogen bonds to break, resulting in fiber dislocation and wrinkles that are difficult to recover, which seriously affects the aesthetics and service life of the fabric.

[0003] In order to eliminate or reduce fabric wrinkles, traditional methods often use high-temperature ironing, but it requires additional manpower and the effect is short-lived. With the advancement of science and technology, chemical finishing technology has gradually become the mainstream, aiming to fundamentally improve the wrinkle resistance of fabrics. Among them, formaldehyde derivatives such as dihydroxymethyl dihydroxyethylene urea are widely used. Its mechanism of action is to use the active groups such as hydroxyl groups contained in the reagent to cross-link and bond with the active groups in the fiber structure to form a network structure, thereby limiting the movement of the fiber when under stress, effectively improving the morphological stability and wrinkle resistance of the fabric.

[0004] Although the finishing technology of formaldehyde derivatives is effective in improving anti-wrinkle performance, there is a potential risk of formaldehyde residues. Long-term exposure may cause irritation to human skin and respiratory system or even more serious health effects. Summary of the invention

[0005] The present application provides an anti-wrinkle and antibacterial fabric and a preparation method thereof. The fabric has good anti-wrinkle performance and can maintain good recovery ability under the action of external forces such as washing.

[0006] In the first aspect, the present application provides an anti-wrinkle and antibacterial fabric, which is treated with a finishing agent, and each 1000 mL of the finishing agent includes: 40 to 70 g of a cross-linking agent, 2 to 5 g of a cross-linking activator, 5 to 15 g of a surfactant, and 10 to 20 g of an antibacterial agent; the cross-linking agent is obtained by free radical copolymerization of reaction monomers containing the following parts by mass: 10 to 20 parts of an unsaturated dicarboxylic acid monomer, 5 to 10 parts of styrene, and 2 to 5 parts of isocyanate ethyl acrylate, and the mass ratio of the unsaturated dicarboxylic acid monomer to the isocyanate ethyl acrylate is 1:0.12 to 0.2.

[0007] The cross-linking agent used in the present application is an acrylic copolymer obtained by copolymerization of monomers. Unsaturated dicarboxylic acid monomers provide abundant carboxylic acid groups for the cross-linking agent, which can react with hydroxyl groups in fibers such as cotton, silk, and hemp to form a network structure, which is conducive to limiting the degree of freedom of fiber molecular segments and improving its anti-wrinkle effect. Further, a large amount of carboxylic acid groups contained in the copolymer will cause the loss of fiber strength and whiteness, and there will be a decline in fabric use performance and apparent performance. For this reason, the present application also introduces an appropriate amount of monomers containing isocyanates to replace unsaturated dicarboxylic acid monomers, and utilizes the coordination of isocyanate groups and carboxylic acid groups to achieve good cross-linking, which is conducive to achieving the balance of fabric anti-wrinkle performance and strength and whiteness. In addition, it should be noted that the isocyanate group has poor stability and needs to be used in conjunction with the carboxylic acid group. Styrene monomer is a hard monomer, and coordination with the remaining two monomers is conducive to improving the stability and film-forming property of the copolymer.

[0008] Preferably, the free radical copolymerization is carried out by emulsion polymerization or suspension polymerization.

[0009] Preferably, the amount of initiator used in the free copolymerization is 1-3% of the mass of the reaction monomers.

[0010] Preferably, the initiator is selected from one or more of benzoyl peroxide, potassium persulfate, ammonium persulfate, sodium persulfate, azobisisobutyronitrile and azobisisoheptanenitrile.

[0011] Preferably, the reactive monomers further include 1 to 4 parts of vinyl siloxane monomers and 1 to 5 parts of hydroxyl-containing monomers, calculated in parts by mass.

[0012] The high concentration of carboxylic acid groups (-COOH) in the crosslinker copolymer can cause its charge stability to decrease, easily causing aggregation and gelation between copolymer particles. The application adds hydrophobic vinyl siloxane monomers to improve the hydrophobicity of polymer chains, which helps to form a tighter micellar structure in free radical copolymerization and enhance the stability of the crosslinker copolymer. The hydroxyl group of the hydroxyl-containing monomer can improve the dispersibility of the emulsion in water, and when it coexists with the carboxylic acid group, it can enhance the interaction between latex particles by forming a hydrogen bond structure and improve the stability of the crosslinker copolymer.

[0013] Preferably, the unsaturated dicarboxylic acid monomer is selected from one or more of maleic acid, fumaric acid, and methylene succinic acid.

[0014] Preferably, the vinyl siloxane monomer is selected from one or more of vinyl trimethoxy silane, vinyl triethoxy silane, vinyl dimethyl methoxy silane, vinyl dimethyl ethoxy silane and vinyl triphenyl silane.

[0015] Preferably, the hydroxyl-containing monomer is selected from one or more of hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxybutyl acrylate, hydroxyethyl methacrylate, and hydroxypropyl methacrylate.

[0016] Preferably, the cross-linking active agent is selected from one or a combination of N,N'-dicyclohexylcarbodiimide, 4-dimethylaminopyridine, 1-ethyl-(3-dimethylhexylpropyl)carbodiimide hydrochloride, and N-hydroxysuccinimide.

[0017] The cross-linking activator can increase the activity of the carboxylic acid in the cross-linking agent, thereby promoting the esterification cross-linking reaction between the cross-linking agent and the fiber, which is beneficial to improving the anti-wrinkle effect of the fabric after finishing.

[0018] Preferably, the antibacterial agent is a silver ion antibacterial agent.

[0019] Preferably, the reaction monomer further comprises 2 to 5 parts of 1-vinylimidazole.

[0020] 1-vinyl imidazole can provide imidazole groups for the cross-linking agent, which can chelate with silver ions, which is beneficial to reduce the loss of the antibacterial agent during water washing and use, improve the sustained-release performance of the antibacterial agent, and play a long-lasting antibacterial effect.

[0021] Preferably, the fabric comprises one or more fibers selected from cotton, wool, linen, hemp, ramie, viscose, silk and rayon.

[0022] In a second aspect, the present application provides a method for preparing an anti-wrinkle and antibacterial fabric, comprising the following steps:

[0023] Preparation of finishing agent: adding the cross-linking agent, the cross-linking activator, the surfactant and the antibacterial agent into water and mixing them evenly to obtain the finishing agent;

[0024] Fabric finishing: adding the fabric to a finishing agent with a bath ratio of 1:20-50, dipping and padding the fabric twice, and the fabric liquid carrying rate after dipping and padding is 80-90%; then drying at 100-170°C, and then washing and drying to obtain wrinkle-resistant and antibacterial fabric;

[0025] Preferably, the fabric impregnation finishing temperature is 80-90°C.

[0026] Preferably, the fabric is immersed for 1 to 3 minutes each time.

[0027] In summary, this application has the following beneficial effects:

[0028] 1. The cross-linking agent of the fabric finishing agent of the present application introduces carboxylic acid groups and isocyanate groups, which can effectively ensure the mechanical strength and whiteness of the fabric while improving the anti-wrinkle performance of the fabric.

[0029] 2. The present application introduces hydrophobic silicone monomers and hydroxyl-containing monomers into the cross-linking agent, thereby significantly improving the stability of the cross-linking agent copolymer and reducing the probability of agglomeration or gelation thereof.

[0030] 3. The present application achieves improvement in the long-term antibacterial properties of fabrics by introducing vinyl imidazole into the cross-linking agent and combining it with an anionic antibacterial agent. DETAILED DESCRIPTION

[0031] Preparation examples of raw materials and / or intermediates

[0032] Preparation Example 1

[0033] The crosslinking agent is prepared by emulsion polymerization process as follows:

[0034] Dissolve lauryl alcohol polyoxyethylene ether in water to prepare a 2wt% emulsion for use; weigh 160g of maleic acid, 25g of ethyl isocyanate acrylate, 80g of styrene, 35g of vinyltrimethoxysilane, 25g of hydroxyethyl acrylate, and 30g of 1-vinylimidazole, add into 1000ml of the emulsion, and heat to 50°C; then add 5.2g of diisopropylbenzene peroxide, heat to 80°C, and keep warm for copolymerization for 3h to obtain a crosslinking agent.

[0035] Preparation Example 2

[0036] The crosslinking agent is prepared by emulsion polymerization process as follows:

[0037] Dissolve lauryl alcohol polyoxyethylene ether in water to prepare a 2wt% emulsion for use; weigh 190g of fumaric acid, 35g of ethyl isocyanate acrylate, 100g of styrene, 20g of vinyltrimethoxysilane, 45g of hydroxyethyl acrylate, and 20g of 1-vinylimidazole, add into 1000ml of the emulsion, and heat to 50°C; then add 5.5g of diisopropylbenzene peroxide, heat to 80°C, and keep warm for 4h to carry out copolymerization reaction to obtain a cross-linking agent.

[0038] Preparation Example 3

[0039] The crosslinking agent is prepared by emulsion polymerization process as follows:

[0040] Dissolve lauryl alcohol polyoxyethylene ether in water to prepare a 2wt% emulsion for use; weigh 120g of maleic acid, 20g of ethyl isocyanate acrylate, 60g of styrene, 15g of vinyltrimethoxysilane, 20g of hydroxyethyl methacrylate, and 40g of 1-vinylimidazole, add them into 1000ml of the emulsion, and heat it to 50°C; then add 4.3g of sodium persulfate, heat it to 78°C, and keep it warm for 3h to carry out copolymerization reaction to obtain a cross-linking agent.

[0041] Preparation Example 4

[0042] The crosslinking agent is different from that in Preparation Example 1 in that hydroxyethyl acrylate is replaced by an equal amount of vinyltrimethoxysilane.

[0043] Preparation Example 5

[0044] The crosslinking agent is different from that in Preparation Example 1 in that vinyltrimethoxysilane is replaced by an equal amount of hydroxyethyl acrylate.

[0045] Preparation Example 6

[0046] The crosslinking agent is different from that in Preparation Example 1 in that hydroxyethyl acrylate and vinyltrimethoxysilane are replaced by equal amounts of maleic acid.

[0047] Preparation Example 7

[0048] The cross-linking agent is different from that in Preparation Example 1 in that 1-vinylimidazole is replaced by an equal amount of styrene.

[0049] Preparation Example 8

[0050] The crosslinking agent is different from that in Preparation Example 1 in that isocyanate ethyl acrylate is replaced by an equal amount of maleic acid.

[0051] Preparation Example 9

[0052] The crosslinking agent is different from that in Preparation Example 1 in that maleic acid is replaced by an equal amount of ethyl isocyanate acrylate.

[0053] Preparation Example 10

[0054] The crosslinking agent is different from that in Preparation Example 1 in that maleic acid is replaced by an equal amount of acrylic acid.

[0055] Example

[0056] Embodiment 1, a wrinkle-resistant and antibacterial fabric is prepared according to the following steps:

[0057] Preparation of finishing agent: 600g of the crosslinking agent obtained in Preparation Example 1, 35g of the crosslinking activator, 100g of the surfactant and 150g of the silver ion antibacterial agent were added to 10L of water, and mixed and stirred to obtain the finishing agent. Among them, the crosslinking activator was 1-ethyl-(3-dimethylhexylpropyl) carbodiimide hydrochloride and N-hydroxysuccinimide in a mass ratio of 3:1; the surfactant was the penetrant JFC.

[0058] Fabric finishing: The fabric was added to the finishing agent at a bath ratio of 1:40 for two dips and two pads. After the second dip and pad, the fabric had a liquid carrying rate of 90%. The finishing agent was then dried at 160°C, and then washed and dried to obtain wrinkle-resistant and antibacterial fabric. The warp density of the fabric was 28 strands / cm, the weft density was 24 shuttles / cm, the warp yarn was cotton and linen blended yarn (cotton 50%, linen 50%), and the weft yarn was cotton yarn.

[0059] Embodiment 2, a wrinkle-resistant and antibacterial fabric is prepared according to the following steps:

[0060] Preparation of finishing agent: 400g of the crosslinking agent obtained in Preparation Example 2, 22g of the crosslinking activator, 60g of the surfactant and 100g of the silver ion antibacterial agent were added to 10L of water, and the mixture was stirred evenly to obtain the finishing agent. Among them, the crosslinking activator was 1-ethyl-(3-dimethylhexylpropyl)carbodiimide hydrochloride and N-hydroxysuccinimide in a mass ratio of 3:1; the surfactant was the penetrant JFC.

[0061] Fabric finishing: The fabric was added to the finishing agent at a bath ratio of 1:50 for two dips and two pads. After the second dip and pad, the fabric had a liquid carrying rate of 90%. The finishing agent was then dried at 160°C, and then washed and dried to obtain wrinkle-resistant and antibacterial fabrics. The warp density of the fabric was 30 strands / cm, the weft density was 26 shuttles / cm, the warp yarn was cotton and linen blended yarn (cotton 50%, linen 50%), and the weft yarn was cotton yarn.

[0062] Embodiment 3, a wrinkle-resistant and antibacterial fabric is prepared according to the following steps:

[0063] Preparation of finishing agent: 700g of the crosslinking agent obtained in Preparation Example 3, 45g of the crosslinking activator, 150g of the surfactant and 180g of the silver ion antibacterial agent were added to 10L of water, and mixed and stirred to obtain the finishing agent. Among them, the crosslinking activator was N,N'-dicyclohexylcarbodiimide; the surfactant was the penetrant JFC.

[0064] Fabric finishing: The fabric was added to the finishing agent at a bath ratio of 1:40 for two dips and two pads. After the second dip and pad, the fabric had a liquid carrying rate of 90%. The finishing agent was then dried at 160°C, and then washed and dried to obtain wrinkle-resistant and antibacterial fabric. The warp density of the fabric was 28 strands / cm, the weft density was 24 shuttles / cm, the warp yarn was cotton and linen blended yarn (cotton 50%, linen 50%), and the weft yarn was cotton yarn.

[0065] Example 4 is an anti-wrinkle and antibacterial fabric. The difference from Example 1 is that in the finishing agent preparation step, the cross-linking agent obtained in Preparation Example 1 is replaced by an equal amount of the cross-linking agent obtained in Preparation Example 4.

[0066] Example 5 is an anti-wrinkle and antibacterial fabric. The difference from Example 1 is that in the finishing agent preparation step, the cross-linking agent obtained in Preparation Example 1 is replaced by an equal amount of the cross-linking agent obtained in Preparation Example 5.

[0067] Example 6, an anti-wrinkle and antibacterial fabric, is different from Example 1 in that, in the finishing agent preparation step, an equal amount of the cross-linking agent obtained in Preparation Example 6 replaces the cross-linking agent obtained in Preparation Example 1.

[0068] Example 7, an anti-wrinkle and antibacterial fabric, is different from Example 1 in that, in the finishing agent preparation step, an equal amount of the cross-linking agent obtained in Preparation Example 7 replaces the cross-linking agent obtained in Preparation Example 1.

[0069] Comparative Example

[0070] Comparative Example 1 is an anti-wrinkle and antibacterial fabric, which is different from Example 1 in that, in the finishing agent preparation step, the cross-linking agent obtained in Preparation Example 1 is replaced by an equal amount of the cross-linking agent obtained in Preparation Example 8.

[0071] Comparative Example 2 is an anti-wrinkle and antibacterial fabric, which is different from Example 1 in that, in the finishing agent preparation step, the cross-linking agent obtained in Preparation Example 1 is replaced by an equal amount of the cross-linking agent obtained in Preparation Example 9.

[0072] Comparative Example 3 is an anti-wrinkle and antibacterial fabric, which is different from Example 1 in that, in the finishing agent preparation step, the cross-linking agent obtained in Preparation Example 1 is replaced by an equal amount of the cross-linking agent obtained in Preparation Example 10.

[0073] Comparative Example 4 is an anti-wrinkle and antibacterial fabric, which is different from Example 1 in that in the finishing agent preparation step, the cross-linking agent and the cross-linking activator obtained in Preparation Example 1 are replaced by an equal amount of dihydroxymethyl dihydroxyethylene urea.

[0074] Performance testing

[0075] Test 1: Anti-wrinkle performance test

[0076] According to the provisions of GB / T 3819-1997 "Recovery angle method for determination of crease recovery of textile fabrics", the warp and weft crease recovery angles of the finished fabric sample are tested, and the sum of the two is taken as the wrinkle recovery angle.

[0077] Test 2: Strength performance test

[0078] According to GB / T 3923.1-2013 "Tensile properties of textile fabrics - Part 1: Determination of breaking strength and elongation at break (strip method)", the breaking strength of the fabric before and after treatment with the finishing agent was tested. Then the breaking strength retention of the fabric was calculated according to the formula "breaking strength of the sample after treatment / breaking strength of the sample before treatment × 100%".

[0079] Test 3: Whiteness test

[0080] The whiteness of the finished fabric samples was tested in accordance with the provisions of GB / T 8424.2-2001 “Textile Colour Fastness Tests - Instrumental Assessment Method for Relative Whiteness”.

[0081] Test 4: Crosslinker stability test

[0082] Take 100 ml of the cross-linking agent and add it to a test tube and place it in a constant temperature oven at 50°C for 8 hours. After taking it out, observe whether the cross-linking agent solution in the test tube has precipitation or gelation.

[0083] Test 5: Long-term antibacterial performance test

[0084] According to GB / T 20944.3-2008 "Evaluation of antibacterial properties of textiles Part 3: Oscillation method", the antibacterial activity of the fabric against Escherichia coli was tested before and after washing 20 times. The antibacterial rate was calculated by the petri dish counting method, and then the antibacterial rate reduction value was calculated according to the formula "antibacterial rate before washing - antibacterial rate after washing". The fabric washing operation was carried out in accordance with the provisions of GB / T 8629-2017 "Household washing and drying procedures for textile experiments".

[0085] Table 1. Test results

[0086]

[0087] Analysis of test results:

[0088] (1) It can be seen from the combination of Examples 1 to 7 and Comparative Examples 1 to 4 and Table 1 that the present application uses a cross-linking agent containing polycarboxylic acid groups and isocyanate groups as the main component of the fabric finishing agent to perform anti-wrinkle finishing on the fabric, which can effectively improve its anti-wrinkle effect while ensuring the strength performance and whiteness of the fabric. The reason may be that the rich carboxylic acid groups in the cross-linking agent can react and cross-link with the hydroxyl groups in fibers such as cotton, silk, and linen to form a network structure, which is conducive to limiting the degree of freedom of the fiber molecular chain segments and improving their anti-wrinkle effect. A proper amount of isocyanate groups can replace the cross-linking effect of carboxylic acid groups to achieve good cross-linking effect, while reducing the damage caused by carboxylic acids to the strength and whiteness of the fabric.

[0089] (2) It can be seen from Example 1 and Examples 4 to 6 and Table 1 that the present application introduces silicone monomers and hydroxyl-containing monomers into the crosslinking agent, which is beneficial to improving the stability of the crosslinking agent and inhibiting its tendency to settle or gel. The reason may be that the addition of hydrophobic vinyl siloxane monomers can increase the hydrophobicity of the polymer chain, which helps to form a tighter micelle structure in the free radical copolymerization and enhance the stability of the crosslinking agent copolymer. The hydroxyl group of the hydroxyl-containing monomer can improve the dispersibility of the emulsion in water. At the same time, when it coexists with the carboxylic acid group, it can enhance the interaction between the latex particles by forming a hydrogen bond structure. The two work together to improve the stability of the crosslinking agent copolymer.

[0090] (3) Combining Example 1 and Example 7 with Table 1, it can be seen that the introduction of 1-vinylimidazole in the cross-linking agent is beneficial to improving the long-term antibacterial property of the fabric. The reason may be that the nitrogen-containing heterocyclic ring in 1-vinylimidazole can chelate with silver ions, effectively controlling the release rate of silver ions and reducing the loss of silver ion antibacterial agents in scenarios such as water washing.

[0091] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A wrinkle-resistant and antibacterial fabric, It is characterized in that The fabric is treated with a finishing agent, wherein each 1000 mL of the finishing agent comprises: 40-70 g of a cross-linking agent, 2-5 g of a cross-linking activator, 5-15 g of a surfactant, and 10-20 g of an antibacterial agent; the cross-linking agent is obtained by free radical copolymerization of reaction monomers containing the following parts by mass: 10-20 parts of an unsaturated dicarboxylic acid monomer, 5-10 parts of styrene, and 2-5 parts of ethyl isocyanate acrylate, and the mass ratio of the unsaturated dicarboxylic acid monomer to the ethyl isocyanate acrylate is 1:0.12-0.

2.

2. The anti-wrinkle and antibacterial fabric according to claim 1, It is characterized in that The reactive monomers further include 1 to 4 parts of vinyl siloxane monomers and 1 to 5 parts of hydroxyl-containing monomers in parts by mass.

3. The anti-wrinkle and antibacterial fabric according to claim 1, It is characterized in that The unsaturated dicarboxylic acid monomer is selected from one or more of maleic acid, fumaric acid and methylene succinic acid.

4. The anti-wrinkle and antibacterial fabric according to claim 2, It is characterized in that The vinyl siloxane monomer is selected from one or more of vinyl trimethoxy silane, vinyl triethoxy silane, vinyl dimethyl methoxy silane, vinyl dimethyl ethoxy silane and vinyl triphenyl silane.

5. The anti-wrinkle and antibacterial fabric according to claim 2, It is characterized in that The hydroxyl-containing monomer is selected from one or more of hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxybutyl acrylate, hydroxyethyl methacrylate, and hydroxypropyl methacrylate.

6. The anti-wrinkle and antibacterial fabric according to claim 1, It is characterized in that The cross-linking active agent is selected from one or a combination of N,N'-dicyclohexylcarbodiimide, 4-dimethylaminopyridine, 1-ethyl-(3-dimethylhexylpropyl)carbodiimide hydrochloride, and N-hydroxysuccinimide.

7. The anti-wrinkle and antibacterial fabric according to claim 1, It is characterized in that The antibacterial agent is a silver ion antibacterial agent.

8. The anti-wrinkle and antibacterial fabric according to claim 7, It is characterized in that The reaction monomer also includes 2 to 5 parts of 1-vinylimidazole.

9. The anti-wrinkle and antibacterial fabric according to claim 1, It is characterized in that The fabric comprises one or more fibers selected from cotton, wool, flax, hemp, ramie, viscose, silk, and rayon.

10. The method for preparing the anti-wrinkle and antibacterial fabric according to any one of claims 1 to 9, It is characterized in that The steps include: Preparation of finishing agent: adding the cross-linking agent, the cross-linking activator, the surfactant and the antibacterial agent into water and mixing them evenly to obtain the finishing agent; Fabric finishing: adding the fabric to a finishing agent with a bath ratio of 1:20-50, dipping and padding the fabric twice, and the fabric liquid carrying rate after dipping and padding is 80-90%; then drying at 100-170°C, and then washing and drying to obtain wrinkle-resistant and antibacterial fabric; Preferably, the fabric impregnation finishing temperature is 80-90°C.