Nanometer device and preparation method thereof
Through the cyclic etching method of surface self-limiting modification and selective removal of modified layers, the Ge impurity diffusion transition layer in GAA devices is removed, and combined with the selective epitaxial and annealing treatment of single crystal materials, the SiGe/Si superlattice is solved. The subthreshold swing problem caused by Ge diffusion in the stack achieves the retention and improvement of electrical characteristics of high-quality conductive channel layers.
Patent Information
- Application Number
- CN202411023911.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
AI Technical Summary
In the existing GAA device process, SiGe/Si superlattice stack has defects such as Ge diffusion and dislocation during the epitaxial process, which makes it difficult for the subthreshold swing (SS) of silicon channel devices to reach the ideal value of 60mV/dec, which affects Conductive characteristics.
Using the cyclic etching method of surface self-limiting modification and selective removal of modified layers, the Ge impurity diffusion transition layer and damage layer in nanosheets are removed, the high-quality single-crystal nanochannel layer is retained, and the channel surface is selectively epitaxy Single crystal material is grown, annealed, and the sacrificial layer/channel layer interface transition defect layer is gradually removed.
Effectively reduce Ge residue and roughness of the channel surface, improve the conductivity characteristics, sub-threshold pendulum (SS) reaches the ideal value of silicon 60mV/dec, and enhances the gate to channel electrostatic control capability and carrier output. fortune characteristics.
Smart Images

Figure CN118969619A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of semiconductor devices, and in particular to a nano device and a preparation method thereof. Background Art
[0002] As CMOS devices continue to shrink along Moore's Law, mass production has entered the 5-3nm technology node. The use of all-around gate (GAA) devices can effectively suppress the short channel effect.
[0003] The current mainstream GAA device process flow is as follows: Figure 1 As shown, the epitaxial method of SiGe / Si superlattice stacking is adopted, and SiGe is generally removed as a sacrificial layer, leaving Si material as a conductive channel. Because when SiGe and Si are alternately epitaxially grown, it is a quasi-heterogeneous epitaxy (there is a difference in the atomic radius of Si and Ge), there is a transition layer, and there may be low-concentration Ge diffusion and dislocation stacking faults and point defects in the transition layer, so there is a certain gap in the characteristics of the silicon channel device of superlattice epitaxy. For example, the subthreshold swing (SS) period currently reported is 70mV / dec and above, which is difficult to reach the ideal value of 60mV / dec for silicon.
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] The object of the present invention is to provide a nano device and a preparation method thereof, which can effectively remove the Ge impurity diffusion transition layer and the damage layer in the nano sheet, thereby retaining the high-quality single crystal nano channel layer as the final conductive channel layer. The nano device prepared by the channel processing method of the present invention can achieve a subthreshold swing (SS) of 60mV / dec, which is the ideal value of silicon.
[0006] In a first aspect, the present invention provides a method for preparing a nanodevice, comprising the following steps:
[0007] S1, preparing a GAA device structure without removing the dummy gate and releasing the channel;
[0008] S2, removing the natural oxide layer on the dummy gate;
[0009] S3, selectively removing the dummy gate layer;
[0010] S4, selectively removing SiO2 material at the bottom of the dummy gate and the top of the stacked fin;
[0011] S5, selectively etching the sacrificial layer;
[0012] S6, thinning the channel layer by using a surface modification and modified layer etching method;
[0013] S7, selectively epitaxially growing a single crystal material on the surface of the released channel layer, and performing annealing treatment;
[0014] S8, step S6 and step S7 are performed cyclically to remove the transition defect layer at the interface of the sacrificial layer / channel layer;
[0015] S9, growing HK, metal gate material and dielectric material in sequence, and performing grinding and planarization.
[0016] The subthreshold swing (SS) of silicon channel devices in the prior art is 70mV / dec and above, which is difficult to reach the ideal silicon value of 60mV / dec. The reason for this problem may be that the roughness of the channel surface affects the ballistic transport and the Ge residue on the channel surface. Based on this, the present invention, based on the existing process flow scheme of GAA, removes the defective transition layer through a channel treatment process to leave a high-quality channel layer, improves the electrostatic control ability of the gate over the channel, and at the same time improves the carrier transport characteristics of the channel, improves the mobility, and reduces the subthreshold swing. Among them, the etching method of the present invention for accurately removing the defective layer with low damage is mainly based on the scheme of surface self-limiting modification and selective removal of the modified layer cycle.
[0017] Studies have shown that the subthreshold swing (SS) of the nano device prepared by the preparation method of the present invention can reach the ideal value of silicon, 60 mV / dec.
[0018] As a preferred embodiment of the present technical solution, in step S1, the concentration of Ge in the sacrificial layer / channel layer in the GAA device structure is 20-40%. The present invention does not strictly limit the materials of the sacrificial layer and the channel layer, and the sacrificial layer can be SiGe or a combination of other materials, and the material of the channel layer is not limited to silicon, and can also be other semiconductor epitaxial materials, such as GaAs, InP, Si, Ge, etc.
[0019] As a preferred embodiment of the present technical solution, step S2 includes: removing the natural oxide layer on the dummy gate by using diluted HF, the treatment time is 5-60s, and the HF diluent is preferably a mixed solution of water and HF with a volume ratio of 100:1.
[0020] As a preferred embodiment of the present technical solution, in step S3, a tetramethylhydroxylamine (TMAH) solution is used to selectively remove the dummy gate polysilicon material.
[0021] As a preferred embodiment of the present technical solution, in step S4, DHF or BOE is used to selectively remove the SiO2 material at the bottom of the dummy gate and the top of the stacked fin, wherein the ratio of hydrofluoric acid and water in DHF is 100:1, and BOE is a buffered etchant composed of NH4F, HF and a surfactant, both of which can effectively etch the SiO2 oxide film at the bottom of the dummy gate and the top of the stacked fin.
[0022] As a preferred embodiment of the present technical solution, in step S5, the sacrificial layer can be selectively etched away by conventional methods, for example, a remote plasma selective etching method can be used. At this time, the plasma source includes any one of a mixed gas of NF3, NH3, O2 and He and a mixed gas of CF4, O2 and He, wherein the volume ratio of NF3, NH3, O2 and He in the mixed gas of NF3, NH3, O2 and He is preferably 1:2:5:20; the volume ratio of CF4, O2 and He in the mixed gas of CF4, O2 and He is preferably 1:5:1.
[0023] Further, step S6 includes: alternatingly using surface modification and modified layer etching methods to thin the channel layer to a thickness of 2-12nm, and preferably 7nm, wherein during the surface modification, one or more mixed gases of N2, O2, H2, Ar and He ionized by a remote plasma source are selected; and during the modified layer etching, one or more mixed gases of NF3, NH3, CF4, F2, ClF3 and He ionized by a remote plasma source are selected.
[0024] The present invention is an etching method for cyclically removing defective layers based on surface self-limiting modification and selective removal of modified layers. The principle is that at a fixed temperature within the temperature range of this scheme, the surface oxidation reaction of the gas is self-limiting (the reaction of O2 or N2 with a single substance is essentially a redox reaction). Because the product is in a solid state, it will hinder the further progress of the reaction to reach an equilibrium thickness, thereby achieving a self-limiting effect. Selective removal is based on selecting appropriate reaction gases and conditions to selectively etch the aforementioned oxide layer, nitride layer or oxynitride layer and stop at the surface of the non-oxidized nitride layer.
[0025] In addition to the above-mentioned method of alternating between surface modification and modified layer etching to thin the channel layer, surface modification and modified layer etching can also be performed simultaneously. Specifically, step S6 includes: simultaneously performing surface modification and modified layer etching to thin the channel layer to a thickness of 2-12nm, and preferably 7nm; wherein, when performing surface modification and modified layer etching simultaneously, a mixed gas of any two or more of N2, O2, H2, Ar, NF3, NH3, CF4, F2, ClF3 and He ionized by a remote plasma source is used, specifically a partial mixed gas of the gases used for surface modification and modified layer etching, so as to achieve the purpose of surface modification and modified layer etching at the same time.
[0026] More preferably, the surface modification treatment and the modified layer etching treatment are performed alternately: ① RPS plasma is used for surface modification: the pressure is 0.1-3T, preferably 0.8T, the power is 100-2000W, preferably 900W, the gas is: N2 flow rate is 10-10000sccm, preferably 1000sccm, O2 flow rate is 10-10000sccm, preferably 1000sccm, the treatment time is 3-60s, preferably 10s; ② modification RPS plasma is used for layer etching: gas pressure is 0.1-3T, preferably 0.8T, power is 100-2000W, preferably 900W, gas is: NH3 flow rate is 3-10000sccm, preferably 500sccm, NF3 flow rate is 10-10000sccm, preferably 100sccm, He flow rate is 3-10000sccm, preferably 2000sccm, treatment time is 3-60s, preferably 10s. The number of cycles of ① and ② is determined according to the removal thickness, preferably 3 times.
[0027] As a preferred embodiment of the present technical solution, in step S7, a LPCVD system is used to selectively epitaxially grow a single crystal material on the surface of the released channel layer under a low pressure condition of 1mT-1T, so as to epitaxially grow a single crystal material on the surface of the silicon nanosheet / wire that is the same as the channel for further repair, and the thickness of the single crystal material is 0.5-4nm, preferably 1nm, and then annealing is performed;
[0028] Among them, during the epitaxial growth, SiH4, H2 and HCl are preferably used as gas sources; and during the annealing treatment, it is preferably treated in a mixed atmosphere of H2 and N2 at 500-1000°C for 10-1000s, wherein the temperature is preferably 800°C and the time is preferably 60s.
[0029] After the epitaxial growth of silicon single crystal material, the interface thinning treatment of step S6 is performed, that is, the etching scheme and the epitaxial growth cycle are performed to remove the SiGe / Si interface transition defect layer and leave high-quality Si as the channel material.
[0030] In a second aspect, the present invention also provides a nanodevice prepared using the above method, which should also fall within the protection scope of the present invention.
[0031] The method for preparing the nanodevice of the present invention has at least the following beneficial effects:
[0032] After the existing nanosheet channel is released, the present invention adopts a process of self-limiting modification of SiGe and Si surfaces, selective removal of the modified layer, and multiple cycles of selective epitaxial growth, which can effectively remove the Ge impurity diffusion transition layer and the damaged layer in the nanosheet, thereby retaining the high-quality single-crystal nanochannel layer as the final conductive channel layer; at the same time, after the growth of the dielectric material, an interface treatment step is added to reduce the interface state and improve the electrical characteristics of the device. Therefore, the subthreshold swing (SS) of the nanodevice prepared by the channel treatment method of the present invention can reach the ideal value of silicon 60mV / dec. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0034] Figure 1 A process flow chart for preparing a GAA device in the prior art;
[0035] Figure 2 It is a partial flow chart of the method for preparing the nano device of the present invention;
[0036] Figure 3 It is a schematic diagram of the structure of the GAA nano device of the present invention;
[0037] Figure 4 The step S2 of the present invention is to remove the natural oxide layer on the dummy gate;
[0038] Figure 5 The dummy gate layer is selectively removed in step S3 of the present invention;
[0039] Figure 6 In step S4 of the present invention, the SiO2 material on the top of the stacked fin at the bottom of the dummy gate is selectively removed;
[0040] Figure 7 The sacrificial layer is selectively etched in step S5 of the present invention;
[0041] Figure 8 The step S6 of the present invention is to thin the channel layer;
[0042] Fig. 9 The step S7 of the present invention is to selectively epitaxially grow a single crystal material;
[0043] Fig.10 Step S9 of the present invention is to grow HK and metal gate materials;
[0044] Fig.11It is the growth medium material of step S9 of the present invention.
[0045] Reference numerals:
[0046] 1: Source lead; 2: Gate lead; 3: Drain lead; 4: Sidewall; 5: Inner sidewall; 6: Channel layer; 7: Source; 8: Drain; 9: Dummy gate; 10: Dielectric; 11: Dummy gate dielectric; 12: Sacrificial layer. DETAILED DESCRIPTION
[0047] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.
[0048] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form also includes the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this description, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0049] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0050] Example 1
[0051] As shown in 2-11, this embodiment provides a method for preparing a nanodevice, comprising the following steps:
[0052] S1. A GAA device structure without removing the dummy gate and releasing the channel is prepared according to a conventional method, wherein the Ge concentration in the sacrificial layer / channel layer is 30%, and the thickness of the channel layer is 12 nm;
[0053] S2, using 100:1 diluted HF to remove the natural oxide layer on the dummy gate, the treatment time is 30s;
[0054] S3, using TMAH to selectively remove the dummy gate polysilicon material;
[0055] S4, using 100:1 diluted DHF to selectively remove SiO2 material at the bottom of the dummy gate and the top of the stacked fin;
[0056] S5. Selectively etching the sacrificial layer by remote plasma selective etching, wherein the plasma source is a mixed gas of NF3, NH3, O2 and He with a volume ratio of 1:2:5:20;
[0057] S6. Alternately use the surface modification and modified layer etching methods to thin the channel layer to a thickness of 7 nm, wherein, during the surface modification, a remote plasma source ionized gas treatment is used, the gas pressure is controlled to be 2T, the power is 900W, the N2 gas flow rate is 1000sccm, and the O2 gas flow rate is 1000sccm for 10s; during the modified layer etching, a remote plasma source ionized gas treatment is used, the gas pressure is controlled to be 2T, the power is 900W, the NH3 gas flow rate is 500sccm, the NF3 gas flow rate is 100sccm, and the He gas flow rate is 2000sccm for 10s;
[0058] S7, using an LPCVD system, under a low pressure of 1 mT, selectively epitaxially growing a Si single crystal material with a thickness of 1 nm on the surface of the released channel layer, and then performing an annealing treatment at 800° C. for 60 seconds in an atmosphere of H2 and N2;
[0059] S8, step S6 and step S7 are cycled for 3 times to remove the transition defect layer at the interface of the sacrificial layer / channel layer;
[0060] S9. When the residual concentration of Ge element, interface state density and roughness reach the device interface requirements, HK and metal gate materials are grown and planarized through CMP equipment; finally, the medium is grown and planarized through grinding with CMP equipment to obtain a GAA nanodevice.
[0061] Example 2
[0062] S1. A GAA device structure without removing the dummy gate and releasing the channel is prepared according to a conventional method, wherein the Ge concentration in the sacrificial layer / channel layer is 30%, and the thickness of the channel layer is 12 nm;
[0063] S2, using 100:1 diluted HF to remove the natural oxide layer on the dummy gate, the treatment time is 30s;
[0064] S3, using TMAH to selectively remove the dummy gate polysilicon material;
[0065] S4, using 100:1 diluted DHF to selectively remove SiO2 material at the bottom of the dummy gate and the top of the stacked fin;
[0066] S5, selectively etching the sacrificial layer by remote plasma selective etching, wherein the plasma source is a mixed gas of CF4, O2 and He in a volume ratio of 1:5:1;
[0067] S6. Surface modification and modified layer etching are performed simultaneously to reduce the channel layer to a thickness of 7 nm. Specifically, gas treatment under remote plasma source ionization is adopted, and the gas pressure is controlled to be 2T, the power is 900W, the N2 gas flow rate is 1000sccm, the O2 gas flow rate is 1000sccm, the NH3 gas flow rate is 500sccm, the NF3 gas flow rate is 100sccm, and the He gas flow rate is 2000sccm for 30s.
[0068] S7, using an LPCVD system, under a low pressure of 1 mT, selectively epitaxially growing a single crystal material with a thickness of 1 nm on the surface of the released channel layer, and then performing an annealing treatment at 800° C. for 60 seconds in an atmosphere of H2 and N2;
[0069] S8, step S6 and step S7 are cycled for 3 times to remove the transition defect layer at the interface of the sacrificial layer / channel layer;
[0070] S9. When the residual concentration of Ge element, interface state density and roughness reach the device interface requirements, HK and metal gate materials are grown and planarized through CMP equipment; finally, the medium is grown and planarized through grinding with CMP equipment to obtain a GAA nanodevice.
[0071] Example 3
[0072] S1. A GAA device structure without removing the dummy gate and releasing the channel is prepared according to a conventional method, wherein the Ge concentration in the sacrificial layer / channel layer is 20%, and the thickness of the channel layer is 10 nm;
[0073] S2, using 100:1 diluted HF to remove the natural oxide layer on the dummy gate, the treatment time is 5s;
[0074] S3, using TMAH to selectively remove the dummy gate polysilicon material;
[0075] S4, using 100:1 diluted DHF to selectively remove SiO2 material at the bottom of the dummy gate and the top of the stacked fin;
[0076] S5. Selectively etching the sacrificial layer by remote plasma selective etching, wherein the plasma source is a mixed gas of NF3, NH3, O2 and He with a volume ratio of 1:2:5:20;
[0077] S6. Alternately use the surface modification and modified layer etching methods to thin the channel layer to a thickness of 2 nm, wherein, during the surface modification, a remote plasma source ionized gas treatment is used, the gas pressure is controlled to be 0.1 T, the power is 2000 W, the N2 gas flow rate is 10 sccm, and the O2 gas flow rate is 10 sccm for 60 s; during the modified layer etching, a remote plasma source ionized gas treatment is used, the gas pressure is controlled to be 0.1 T, the power is 2000 W, the NH3 gas flow rate is 10 sccm, the NF3 gas flow rate is 10 sccm, and the He gas flow rate is 3 sccm for 60 s;
[0078] S7, using an LPCVD system, under a low pressure of 1 mT, selectively epitaxially growing a single crystal material with a thickness of 0.5 nm on the surface of the released channel layer, and then performing an annealing treatment at 500° C. for a treatment time of 1000 s in an atmosphere of H2 and N2;
[0079] S8, step S6 and step S7 are cycled 4 times to remove the transition defect layer at the interface of the sacrificial layer / channel layer;
[0080] S9. When the residual concentration of Ge element, interface state density and roughness reach the device interface requirements, HK and metal gate materials are grown and planarized through CMP equipment; finally, the medium is grown and planarized through grinding with CMP equipment to obtain a GAA nanodevice.
[0081] Example 4
[0082] S1. A GAA device structure without removing the dummy gate and releasing the channel is prepared according to a conventional method, wherein the Ge concentration in the sacrificial layer / channel layer is 40%, and the thickness of the channel layer is 20 nm;
[0083] S2, using 100:1 diluted HF to remove the natural oxide layer on the dummy gate, the treatment time is 60s;
[0084] S3, using TMAH to selectively remove the dummy gate polysilicon material;
[0085] S4, using 100:1 diluted DHF to selectively remove SiO2 material at the bottom of the dummy gate and the top of the stacked fin;
[0086] S5, selectively etching the sacrificial layer by remote plasma selective etching, wherein the plasma source is a mixed gas of CF4, O2 and He in a volume ratio of 1:5:1;
[0087] S6, synchronously performing surface modification and modified layer etching to reduce the channel layer to a thickness of 12 nm, wherein, during surface modification, a remote plasma source ionized gas treatment is used, the gas pressure is controlled to be 3 T, the power is 100 W, the N2 gas flow rate is 10000 sccm, and the O2 gas flow rate is 10000 sccm for 3 s; during modified layer etching, a remote plasma source ionized gas treatment is used, the gas pressure is controlled to be 3 T, the power is 100 W, the NH3 gas flow rate is 10000 sccm, the NF3 gas flow rate is 10000 sccm, and the He gas flow rate is 10000 sccm for 3 s;
[0088] S7, using an LPCVD system, under 1T low pressure conditions, selectively epitaxially growing a single crystal material with a thickness of 4nm on the surface of the released channel layer, and then performing annealing treatment at 1000°C for 10s in an H2 and N2 atmosphere;
[0089] S8, step S6 and step S7 are cycled 4 times to remove the transition defect layer at the interface of the sacrificial layer / channel layer;
[0090] S9. When the residual concentration of Ge element, interface state density and roughness reach the device interface requirements, HK and metal gate materials are grown and planarized through CMP equipment; finally, the medium is grown and planarized through grinding with CMP equipment to obtain a GAA nanodevice.
[0091] The present invention tests the subthreshold floating (SS) of the GAA nanodevices prepared in the above-mentioned embodiments 1-4. The test results are shown in Table 1.
[0092] Table 1 Test results
[0093] Serial number SS(mV / dec) Example 1 63 Example 2 62 Example 3 61 Example 4 60
[0094] Research shows that the SS values of the GAA nanodevices prepared in the above embodiments can reach the theoretical limit of silicon, which is 60 mV / dec.
[0095] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a nanodevice, characterized in that: The following steps are involved: S1, preparing a GAA device structure without removing the dummy gate and releasing the channel; S2, removing the natural oxide layer on the dummy gate; S3, selectively removing the dummy gate layer; S4, selectively removing SiO2 material at the bottom of the dummy gate and the top of the stacked fin; S5, selectively etching the sacrificial layer; S6, thinning the channel layer by using a surface modification and modified layer etching method; S7, selectively epitaxially growing a single crystal material on the surface of the released channel layer, and performing annealing treatment; S8, step S6 and step S7 are performed cyclically to remove the transition defect layer at the interface of the sacrificial layer / channel layer; S9, growing HK, metal gate material and dielectric material in sequence, and performing grinding and planarization.
2. The preparation method according to claim 1, characterized in that: In step S1 , the concentration of Ge in the sacrificial layer / channel layer in the GAA device structure is 20-40%.
3. The preparation method according to claim 1, characterized in that: Step S2 includes: using diluted HF to remove the natural oxide layer on the dummy gate, and the processing time is 5-60 seconds.
4. The preparation method according to claim 1, characterized in that: In step S3, TMAH is used to selectively remove the dummy gate layer.
5. The preparation method according to claim 1, characterized in that: In step S4, the SiO2 material at the bottom of the dummy gate and the top of the stacked fin is selectively removed by using a DHF or BOE method.
6. The preparation method according to claim 1, characterized in that: In step S5, the sacrificial layer is selectively etched by remote plasma selective etching, wherein the plasma source includes any one of a mixed gas of NF3, NH3, O2 and He and a mixed gas of CF4, O2 and He; Preferably, the volume ratio of NF3, NH3, O2 and He in the mixed gas of NF3, NH3, O2 and He is 1:2:5:20; The volume ratio of CF4, O2 and He in the mixed gas of CF4, O2 and He is 1:5:
1.
7. The preparation method according to claim 1, characterized in that: Step S6 includes: alternately using the surface modification and modified layer etching methods to thin the channel layer to a thickness of 2-12 nm, Wherein, during the surface modification, a mixed gas of one or more of N2, O2, H2, Ar and He ionized by a remote plasma source is used; When etching the modified layer, a mixed gas of one or more of NF3, NH3, CF4, F2, ClF3 and He ionized by a remote plasma source is used.
8. The preparation method according to claim 1, characterized in that: Step S6 includes: performing surface modification and modified layer etching simultaneously to thin the channel layer to a thickness of 2-12 nm; When surface modification and modified layer etching are performed simultaneously, a mixed gas of any two or more of N2, O2, H2, Ar, NF3, NH3, CF4, F2, ClF3 and He ionized by a remote plasma source is used.
9. The preparation method according to claim 1, characterized in that: In step S7, a single crystal material with a thickness of 0.5-4 nm is selectively epitaxially grown on the surface of the released channel layer under a low pressure condition of 1 mT-1 T using an LPCVD system, and then annealing is performed; Wherein, during the epitaxial growth, SiH4, H2 and HCl are used as gas sources; During the annealing treatment, the process is carried out at 500-1000° C. for 10-1000 seconds in a mixed atmosphere of H 2 and N 2 .
10. A nano device, characterized in that: Prepared according to the preparation method according to any one of claims 1 to 9.