Solid electrolyte membrane, preparation method thereof and secondary battery
By using a solid electrolyte membrane with a porous base film structure in secondary batteries, combining polyimide, inorganic flame retardant and nanoceramic materials, the safety and electrochemical performance problems of liquid electrolytes are solved, and the flame retardant of batteries is improved. Mechanical and electrochemical properties.
Patent Information
- Application Number
- CN202411034558.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
AI Technical Summary
The existing liquid electrolytes used in secondary batteries have low energy density, polluted the environment and safety hazards. Polymer solid electrolytes are prone to fire after mechanical impact, and the increase of liquid flame retardants affects electrochemical performance.
A porous base film is used as the base material of the solid electrolyte membrane, including polyimide and an inorganic flame retardant, and its pores are filled with polymer solid electrolyte and nanoceramic materials to form a multilayer structure to improve flame retardant and mechanical properties.
It improves the safety and electrochemical performance of the battery, enhances flame retardant performance and mechanical strength, shortens the ion migration path, improves ion conductivity, reduces lithium dendrites, broadens the ionic free range, and enhances the comprehensive performance of the battery.
Smart Images

Figure CN118970149A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of batteries, and in particular to a solid electrolyte membrane and a preparation method thereof, and a secondary battery. Background Art
[0002] Energy crisis and environmental pollution have driven the booming development of the electric vehicle market. As the core component of electric vehicles, high-energy-density secondary batteries have received widespread attention and have broad market prospects.
[0003] At present, secondary batteries use liquid electrolytes, which have safety issues such as low energy density, environmental pollution, leakage, and flammability. In order to effectively solve the above problems, solid electrolytes can be used instead of liquid electrolytes. Among them, polymer solid electrolytes are mainly composed of high molecular polymers, and high molecular polymer electrolytes can cause fires after short circuits and mechanical shocks. In order to improve the flame retardant properties of polymer solid electrolytes, liquid flame retardants are added to the polymer components in traditional technologies to meet the requirements of flame retardant levels.
[0004] However, as the amount of liquid flame retardant added increases, the mechanical properties of the polymer electrolyte are affected, resulting in a decrease in the electrochemical performance of the battery. Summary of the invention
[0005] Based on this, it is necessary to provide a solid electrolyte membrane and a preparation method thereof and a secondary battery, taking into account the flame retardant properties and mechanical properties of the polymer solid electrolyte and improving the safety and electrochemical performance of the battery.
[0006] The first aspect of the present application provides a solid electrolyte membrane, comprising: a porous base membrane, the material of the porous base membrane includes polyimide and an inorganic flame retardant; a solid electrolyte layer, formed in the pores of the porous base membrane, the solid electrolyte layer includes a polymer solid electrolyte, an electrolyte salt and a nano-ceramic material.
[0007] In some embodiments, the solid electrolyte layer includes: a first solid electrolyte layer, the first solid electrolyte layer includes a first polymer solid electrolyte, a first electrolyte salt and a first nano-ceramic material; a second solid electrolyte layer, the second solid electrolyte layer includes a second polymer solid electrolyte, a second electrolyte salt and a second nano-ceramic material; wherein the first solid electrolyte layer faces the positive electrode of the electrochemical device, the second solid electrolyte layer faces the negative electrode of the electrochemical device, and the first polymer solid electrolyte has better oxidation resistance than the second polymer solid electrolyte.
[0008] In some embodiments, a thickness ratio of the first solid electrolyte layer to the second solid electrolyte layer is (3:7) to (7:3).
[0009] In some embodiments, the first nano-ceramic material accounts for 1% to 10% by mass in the first solid electrolyte layer; and / or the second nano-ceramic material accounts for 1% to 10% by mass in the second solid electrolyte layer.
[0010] In some embodiments, the first polymer solid electrolyte accounts for 80% to 94% by mass in the first solid electrolyte layer; and / or the second polymer solid electrolyte accounts for 70% to 89% by mass in the second solid electrolyte layer.
[0011] In some embodiments, the first polymer solid electrolyte includes at least one of poly(vinylidene fluoride-hexafluoropropylene) (PVDF-HFP), polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), polymethyl methacrylate (PMMA), and polypropylene carbonate (PPC); the second polymer solid electrolyte includes at least one of polyethylene oxide (PEO), polyethylene glycol monomethyl ether acrylate (PEGMA), polydioxolane, polyethylene carbonate, and polyethylene terephthalate (PET).
[0012] In some embodiments, the inorganic flame retardant accounts for 10% to 30% by weight in the porous base membrane.
[0013] In some embodiments, the thickness of the solid electrolyte membrane is 20 μm to 60 μm;
[0014] In some embodiments, the ionic conductivity (40° C.) of the solid electrolyte membrane is 2.6*10 -5 S / cm~8.7*10 -4 S / cm.
[0015] The second aspect of the present application provides a method for preparing a solid electrolyte membrane, comprising the following steps: mixing a dianhydride compound, a diamine compound and an inorganic flame retardant, performing a thermal imidization treatment, and preparing a porous base membrane; filling fillers in the pores of the porous base membrane to prepare a solid electrolyte membrane; wherein the fillers include polymer solid electrolytes, electrolyte salts and nano-ceramic materials.
[0016] The third aspect of the present application provides a secondary battery, comprising the solid electrolyte membrane provided in the first aspect of the present application or the solid electrolyte membrane prepared by the preparation method provided in the second aspect of the present application.
[0017] Compared with the traditional technology, this application has at least the following beneficial effects:
[0018] The solid electrolyte membrane provided by the present application, the polyimide and the inorganic flame retardant in the porous base membrane improve the flame retardant performance of the solid electrolyte, thereby improving the safety of the battery. The framework structure of the porous base membrane improves the mechanical properties and flexibility of the solid electrolyte membrane on the one hand; on the other hand, the vertically arranged channels in the porous base membrane can shorten the ion migration path, realize the rapid migration of lithium ions, and the porous base membrane can limit the migration of anions in the lithium salt, increase the number of lithium ion migrations of the electrolyte, thereby improving the ionic conductivity of the solid electrolyte membrane, thereby improving the electrochemical performance of the solid electrolyte. In addition, the inorganic flame retardant in the porous base membrane improves the mechanical strength of the solid electrolyte and inhibits the growth of lithium dendrites; the nano-ceramic material in the solid electrolyte layer further improves the flame retardant performance of the solid electrolyte membrane, further improves the safety of the battery, and at the interface with the polymer electrolyte, destroys the regular arrangement of the polymer electrolyte, expands its amorphous region, reduces the crystallinity, broadens the free range of ions in the polymer electrolyte, improves the ionic conductivity of the solid electrolyte membrane, and improves the electrochemical performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 A flow chart of a method for preparing a solid electrolyte membrane in one embodiment of the present application is provided. DETAILED DESCRIPTION
[0020] References to embodiments of the present application will now be provided in detail, one or more examples of which are described below. Each example is provided as an explanation rather than a limitation of the present application. In fact, it will be apparent to those skilled in the art that various modifications and variations may be made to the present application without departing from the scope or spirit of the present application. For example, a feature described or described as part of one embodiment may be used in another embodiment to produce a further embodiment.
[0021] Therefore, it is intended that the present application covers such modifications and variations that fall within the scope of the appended claims and their equivalents. Other objects, features and aspects of the present application are disclosed in or are apparent from the following detailed description. It will be appreciated by those of ordinary skill in the art that this discussion is merely a description of exemplary embodiments and is not intended to limit the broader aspects of the present application.
[0022] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0023] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.
[0024] If not otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0025] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0026] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, it is mentioned that the method may also include step (c), which means that step (c) can be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0027] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0028] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0029] The first aspect of the present application provides a solid electrolyte membrane, which includes a porous base membrane and a solid electrolyte layer. The porous base membrane includes polyimide and an inorganic flame retardant. The solid electrolyte layer is formed in the pores of the porous base membrane, and the solid electrolyte layer includes a polymer solid electrolyte, an electrolyte salt and a nano-ceramic material.
[0030] The solid electrolyte membrane provided by the present application, the polyimide and inorganic flame retardant in the porous base membrane improve the flame retardant performance of the solid electrolyte, thereby improving the safety of the battery. The framework structure of the porous base membrane improves the mechanical properties and flexibility of the solid electrolyte membrane on the one hand; on the other hand, the vertically arranged channels in the porous base membrane can shorten the ion migration path, realize the rapid migration of lithium ions, and the porous base membrane can limit the migration of anions in the lithium salt, increase the number of lithium ion migrations of the electrolyte, thereby improving the ionic conductivity of the solid electrolyte membrane, thereby improving the electrochemical performance of the solid electrolyte. In addition, the inorganic flame retardant in the porous base membrane improves the mechanical strength of the solid electrolyte and inhibits the growth of lithium dendrites; the nano-ceramic material in the solid electrolyte layer further improves the flame retardant performance of the solid electrolyte membrane, further improves the safety of the battery, and at the interface with the polymer electrolyte, destroys the regular arrangement of the polymer electrolyte, expands its amorphous region, reduces the crystallinity, broadens the free range of ions in the polymer electrolyte, improves the ionic conductivity of the solid electrolyte membrane, and improves the electrochemical performance of the battery.
[0031] In some embodiments, the inorganic flame retardant includes one or more of aluminum oxide, silicon dioxide, titanium dioxide, zinc oxide, zirconium oxide, lithium aluminum titanium phosphate, lithium lanthanum phosphate, and lithium lanthanum zirconium titanate.
[0032] In some embodiments, the polymer solid electrolyte includes one or more of polyethylene oxide (PEO), poly(vinylidene fluoride-hexafluoropropylene) (PVDF-HFP), polyacrylonitrile (PAN), polyvinylidene fluoride (PVDF), polypropylene carbonate (PPC), polymethyl methacrylate (PMMA), polyethylene glycol monomethyl ether acrylate (PEGMA), polydioxolane, polyethylene carbonate, and polyethylene terephthalate (PET).
[0033] In some embodiments, the electrolyte salt is a lithium salt, which includes one or more of lithium hexafluorophosphate, lithium perchlorate, lithium tetrafluoroborate, lithium bistrifluoromethanesulfonyl imide, lithium bisfluorosulfonyl imide, lithium difluorooxalatoborate, and lithium dioxalatoborate.
[0034] In some embodiments, the nano ceramic material includes one or more of aluminum oxide, silicon dioxide, titanium dioxide, zinc oxide, zirconium oxide, lithium aluminum titanium phosphate, lithium lanthanum phosphate, and lithium lanthanum zirconium titanate. Further, the nano ceramic material includes one or more of lithium aluminum titanium phosphate, lithium lanthanum phosphate, and lithium lanthanum zirconium titanate.
[0035] In some embodiments, the solid electrolyte layer includes a first solid electrolyte layer and a second solid electrolyte layer. The first solid electrolyte layer includes a first polymer solid electrolyte, a first electrolyte salt and a first nano-ceramic material. The second solid electrolyte layer includes a second polymer solid electrolyte, a second electrolyte salt and a second nano-ceramic material. Wherein, the first solid electrolyte layer faces the positive electrode of the electrochemical device, the second solid electrolyte layer faces the negative electrode of the electrochemical device, and the first polymer solid electrolyte has better oxidation resistance than the second polymer solid electrolyte.
[0036] The first solid electrolyte layer faces the positive electrode of the electrochemical device, and the second solid electrolyte layer faces the negative electrode of the electrochemical device. The first polymer solid electrolyte has better oxidation resistance than the second polymer solid electrolyte, so that a good interface effect is formed between the solid electrolyte membrane and the positive electrode and the negative electrode, thereby improving the interface compatibility between the solid electrolyte membrane and the electrode.
[0037] In some embodiments, the first electrolyte salt and the second electrolyte salt are both lithium salts, the first electrolyte salt and the second electrolyte salt are the same or different, and are independently selected from one or more of lithium hexafluorophosphate, lithium perchlorate, lithium tetrafluoroborate, lithium bistrifluoromethanesulfonyl imide, lithium bisfluorosulfonyl imide, lithium difluorooxalatoborate, and lithium dioxalatoborate.
[0038] In some embodiments, the first nanoceramic material and the second nanoceramic material are the same or different and are independently selected from one or more of aluminum oxide, silicon dioxide, titanium dioxide, zinc oxide, zirconium oxide, lithium aluminum titanium phosphate, lithium lanthanum phosphate, and lithium lanthanum zirconium titanate.
[0039] In some embodiments, the second nano-ceramic material has better stability to lithium than the first nano-ceramic material.
[0040] In some embodiments, the thickness ratio of the first solid electrolyte layer to the second solid electrolyte layer is (3:7) to (7:3), including but not limited to 3:7, 4:6, 5:5, 6:4, and 7:3. Within the above thickness ratio range, the interface compatibility between the solid electrolyte and the electrode is further improved. Further, the thickness ratio of the first solid electrolyte layer to the second solid electrolyte layer is (3:7) to (4:6).
[0041] It is understandable that although the first solid electrolyte layer has higher oxidation resistance, its ionic conductivity performance is lower than that of the second solid electrolyte layer. Therefore, the thickness of the first solid electrolyte layer is slightly lower than that of the second solid electrolyte layer, which is beneficial to taking into account the interface compatibility and ionic conductivity of the solid electrolyte membrane, thereby improving the comprehensive electrochemical performance of the solid electrolyte membrane.
[0042] It should be noted that in the present application, the "thickness of the first solid electrolyte layer" refers to the dimension of the first solid electrolyte layer in the thickness direction of the porous substrate membrane; naturally, the "thickness of the second solid electrolyte layer" refers to the dimension of the second solid electrolyte layer in the thickness direction of the porous substrate membrane.
[0043] In some embodiments, the mass percentage of the first nano-ceramic material in the first solid electrolyte layer is 1% to 10%, including but not limited to 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, and 10%.
[0044] In some embodiments, the mass percentage of the second nano-ceramic material in the second solid electrolyte layer is 1% to 10%, including but not limited to 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, and 10%.
[0045] In some embodiments, the mass percentage of the first polymer solid electrolyte in the first solid electrolyte layer is 80% to 94%, including but not limited to 80%, 82%, 84%, 86%, 88%, 90%, 92%, and 94%.
[0046] In some embodiments, the mass proportion of the second polymer solid electrolyte in the second solid electrolyte layer is 70% to 89%, including but not limited to 70%, 74%, 78%, 82%, 86%, 89%. In some embodiments, the first polymer solid electrolyte includes at least one of poly(vinylidene fluoride-hexafluoropropylene) (PVDF-HFP), polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), polymethyl methacrylate (PMMA), and polypropylene carbonate (PPC); the second polymer solid electrolyte includes at least one of polyethylene oxide (PEO), polyethylene glycol monomethyl ether acrylate (PEGMA), polydioxolane, polyethylene carbonate, and polyethylene terephthalate (PET).
[0047] The first polymer solid electrolyte and the second polymer solid electrolyte are arranged in this way so that the electrolyte selected near the positive electrode side has strong oxidation resistance, and when a high-voltage positive electrode is selected, the electrolyte can be prevented from being oxidized under high-voltage conditions, resulting in damage to battery performance. In addition, electrolytes such as PEO and PEGMA are selected on the negative electrode side, which have strong plasticity and improve the solid-solid contact interface between the electrode and the solid electrolyte.
[0048] In some embodiments, the inorganic flame retardant accounts for 10% to 30% by weight of the porous base membrane.
[0049] In some embodiments, the mass proportion of nano-ceramic material in the solid electrolyte layer is 1% to 10%, including but not limited to 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, and 10%.
[0050] In some embodiments, the thickness of the solid electrolyte membrane is 20 μm to 60 μm, including but not limited to 20 μm, 30 μm, 40 μm, 50 μm, and 60 μm. Within the above thickness range, the solid electrolyte membrane maintains certain mechanical properties and flame retardant properties while ensuring a certain ionic conductivity. Further, the thickness of the solid electrolyte membrane is 20 μm to 40 μm.
[0051] In some embodiments, the ionic conductivity (40° C.) of the solid electrolyte membrane is 2.6*10 -5 S / cm~8.7*10 -4 S / cm.
[0052] The second aspect of the present application provides a method for preparing a solid electrolyte membrane, such as Figure 1 As shown, the following steps are included:
[0053] S1. Mix a dianhydride compound, a diamine compound and an inorganic flame retardant, and perform a thermal imidization treatment to prepare a porous base film.
[0054] S2. Forming a solid electrolyte layer in the pores of the porous base membrane to prepare a solid electrolyte membrane.
[0055] The solid electrolyte layer includes a polymer solid electrolyte, an electrolyte salt and a nano-ceramic material.
[0056] The preparation method of the solid electrolyte membrane provided by the present application has a simple production process. By preparing a porous base membrane, the polyimide and inorganic flame retardant in the porous base membrane improve the flame retardant performance of the solid electrolyte, thereby improving the safety of the battery. The framework structure of the porous base membrane improves the mechanical properties and flexibility of the solid electrolyte membrane on the one hand; on the other hand, the vertically arranged channels in the porous base membrane can shorten the ion migration path, realize the rapid migration of lithium ions, and the porous base membrane can limit the migration of anions in the lithium salt, increase the number of lithium ion migrations of the electrolyte, thereby improving the ionic conductivity of the solid electrolyte membrane, thereby improving the electrochemical performance of the solid electrolyte. In addition, the inorganic flame retardant in the porous base membrane improves the mechanical strength of the solid electrolyte and inhibits the growth of lithium dendrites. The nano-ceramic material in the solid electrolyte layer further improves the flame retardant performance of the solid electrolyte membrane, further improves the safety of the battery, and at the interface with the polymer electrolyte, destroys the regular arrangement of the polymer electrolyte, expands its amorphous region, reduces the crystallinity, broadens the free range of ions in the polymer electrolyte, improves the ionic conductivity of the solid electrolyte membrane, and improves the electrochemical performance of the battery.
[0057] In some embodiments, the molar ratio of the dianhydride compound to the diamine compound is 1:(0.95-1.05).
[0058] In some embodiments, the dianhydride compound includes one or more of 1S,2S,4R,5R-cyclohexanetetracarboxylic dianhydride (H'PMDA), pyromellitic dianhydride (PMDA), cyclobutanetetracarboxylic dianhydride (CBDA), hexafluoroisopropylphthalic anhydride (6FDA), 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride (ODPA), 3,3',4,4'-benzophenone tetracarboxylic dianhydride (BTDA), 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA) and bisphenol A diether dianhydride (BPADA).
[0059] In some embodiments, the diamine compound includes one or more of 2,2′-bis(trifluoromethyl)diaminobiphenyl (TFMB) and diaminodiphenyl ether (ODA).
[0060] In some embodiments, the inorganic flame retardant includes one or more of aluminum oxide, silicon dioxide, titanium dioxide, zinc oxide, zirconium oxide, lithium aluminum titanium phosphate, and lithium lanthanum phosphate.
[0061] In some embodiments, the polymer solid electrolyte includes one or more of polyethylene oxide (PEO), poly(vinylidene fluoride-hexafluoropropylene), polyacrylonitrile (PAN), polyvinylidene fluoride (PVDF), polypropylene carbonate, polymethyl methacrylate (PMMA), polyethylene glycol monomethyl ether acrylate (PEGMA), polydioxolane, polyethylene carbonate, and polyethylene terephthalate.
[0062] In some embodiments, the electrolyte salt is a lithium salt, which includes one or more of lithium hexafluorophosphate, lithium perchlorate, lithium tetrafluoroborate, lithium bistrifluoromethanesulfonyl imide, lithium bisfluorosulfonyl imide, lithium difluorooxalatoborate, and lithium dioxalatoborate.
[0063] In some embodiments, a dianhydride compound, a diamine compound and an inorganic flame retardant are mixed and subjected to thermal imidization treatment to prepare a porous base film, comprising the following steps:
[0064] S11, mixing the dianhydride compound, the diamine compound, the first solvent and the inorganic flame retardant to obtain a porous base film precursor solution.
[0065] S12, performing a first coating treatment on the porous base film precursor liquid to obtain a first liquid film.
[0066] S13, adding a phase separation solvent to the first liquid membrane for immersion treatment, taking it out, and sequentially performing a first drying treatment and a thermal imidization treatment to obtain a porous base membrane.
[0067] The polyamic acid is formed by using dianhydride compounds and diamine compounds, and the solution viscosity is low, which improves the dispersion of the inorganic flame retardant in the porous base film precursor solution and reduces agglomeration, thereby improving the uniformity of pore formation when a solid electrolyte membrane is subsequently formed.
[0068] In some embodiments, the phase separation solvent is a mixed solvent of ethanol and the first solvent.
[0069] In some embodiments, the first coating-treated support is a glass plate.
[0070] In some of these embodiments, the first coating process is a manual coating process.
[0071] In some embodiments, the blade height of the first coating process is 20 μm to 60 μm.
[0072] In some embodiments, the soaking time is 60 min to 180 min.
[0073] In some embodiments, the temperature of the first drying process is 40° C. to 80° C., and the time of the first drying process is 2 h to 4 h.
[0074] In some embodiments, the temperature of the thermal imidization treatment is 200°C to 400°C.
[0075] In some specific embodiments, the thermal imidization treatment is performed by a segmented heating method, and the temperature rise procedure of the thermal imidization treatment is as follows:
[0076] Stage 1: Heat to 100°C at 5°C / min-10°C / min, keep warm for 30min-60min;
[0077] Stage 2: Heat up to 200°C at 5°C / min-10°C / min, and keep warm for 30-60 minutes;
[0078] Stage three: heat to 300°C at 5°C / min to 10°C / min, and keep warm for 30min to 60min.
[0079] In some embodiments, mixing a dianhydride compound, a diamine compound, a first solvent, and an inorganic flame retardant to obtain a porous base film precursor solution comprises the following steps:
[0080] S111, mixing an inorganic flame retardant and a first solvent, and performing a first stirring process to obtain a first mixed liquid.
[0081] S112, adding the dianhydride compound and the diamine compound to the first mixed solution, performing a second stirring treatment, and obtaining a porous base film precursor solution.
[0082] In some embodiments, the first solvent includes one or more of N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), and N-methylpyrrolidone (NMP).
[0083] In some embodiments, the temperature of the first stirring treatment is -10°C to 5°C, the time of the first stirring treatment is 0.5h to 2h, and the atmosphere of the first stirring treatment is an inert gas.
[0084] In some embodiments, the temperature of the second stirring treatment is -10°C to 5°C, the stirring speed of the second stirring treatment is 300 r / min to 800 r / min, and the time of the second stirring treatment is 6 h to 18 h.
[0085] In some embodiments, a solid electrolyte layer is formed in the pores of a porous base membrane to prepare a solid electrolyte membrane, comprising the following steps:
[0086] S21, mixing a polymer solid electrolyte, an electrolyte salt, a second solvent and a nano-ceramic material to obtain a filler liquid.
[0087] S22, the filler liquid is filled into the pores of the porous base membrane, and a second drying process is performed to form a solid electrolyte membrane to obtain a solid electrolyte membrane.
[0088] In some embodiments, a scraper is used to remove excess filler liquid from the surface of the porous substrate.
[0089] In some embodiments, the temperature of the second drying process is 60° C. to 80° C., and the time of the second drying process is 12 h to 36 h.
[0090] In some embodiments, the second solvent includes one or more of acetonitrile (ACN), N-methylpyrrolidone (NMP), dimethylformamide (DMF), dimethyl sulfoxide (DMSO), acetone, dichloromethane, chloroform, xylene, and tetrahydrofuran (THF).
[0091] In some embodiments, mixing a polymer solid electrolyte, an electrolyte salt, a second solvent, and a nano-ceramic material to obtain a filler solution comprises the following steps:
[0092] S2111, mixing a polymer solid electrolyte, an electrolyte salt and a second solvent, and performing a third stirring treatment to obtain a second mixed solution.
[0093] S2112, adding the nano-ceramic material to the second mixed solution, performing a fourth stirring process, and obtaining a filler solution.
[0094] In some embodiments, mixing a polymer solid electrolyte, an electrolyte salt, a second solvent, and a nano-ceramic material to obtain a filler solution comprises the following steps:
[0095] S2121, mixing the first polymer solid electrolyte, the first electrolyte salt, and the second solvent, and performing a third stirring treatment to obtain a third mixed solution.
[0096] S2122, adding the first nano-ceramic filler to the third mixed solution, performing a fourth stirring process, and obtaining a first filler solution.
[0097] S2123, mixing a second polymer solid electrolyte, a second electrolyte salt, and a second solvent, and performing a third stirring treatment to obtain a fourth mixed solution.
[0098] S2124, adding the second nano-ceramic filler to the fourth mixed solution, and performing the fourth stirring process again to obtain a second filler solution.
[0099] In some embodiments, the temperature of the third stirring treatment is 30° C. to 50° C., and the time of the third stirring treatment is 12 h to 36 h.
[0100] In some embodiments, the temperature of the fourth stirring treatment is 30° C. to 50° C., the stirring speed of the fourth stirring treatment is 300 r / min to 600 r / min, and the time of the fourth stirring treatment is 12 h to 36 h.
[0101] In some embodiments, the filler liquid is filled into the pores of the porous base film, and a second drying process is performed to form a solid electrolyte membrane, thereby obtaining a solid electrolyte membrane, comprising the following steps:
[0102] S2211, performing a second coating process on the first filler liquid to obtain a second liquid film.
[0103] S2212, placing the porous base membrane into the second liquid membrane for immersion treatment, taking it out, and performing a second drying treatment to form a first solid electrolyte layer to obtain a first intermediate.
[0104] S2213, performing a third coating process on the second filler liquid to obtain a third liquid film.
[0105] S2214, placing the first intermediate into the third liquid membrane for immersion treatment, taking it out, and performing a second drying treatment again to form a second solid electrolyte layer to obtain a solid electrolyte membrane.
[0106] In some embodiments, the filler liquid is filled into the pores of the porous base film, and a second drying process is performed to form a solid electrolyte membrane, thereby obtaining a solid electrolyte membrane, comprising the following steps:
[0107] S2221, performing a third coating process on the second filler liquid to obtain a third liquid film.
[0108] S2222, placing the porous base membrane into the third liquid membrane for immersion treatment, taking it out, and performing a second drying treatment to form a second solid electrolyte layer to obtain a second intermediate.
[0109] S2223, performing a second coating process on the first filler liquid to obtain a second liquid film.
[0110] S2224, placing the second intermediate into the second liquid film for immersion treatment, taking it out, and performing a second drying treatment again to form a first solid electrolyte layer to obtain a solid electrolyte membrane.
[0111] In some embodiments, the sum of the thickness of the second coating process and the thickness of the third coating process is 20 μm to 60 μm.
[0112] The third aspect of the present application provides a secondary battery, which is the solid electrolyte membrane provided in the first aspect of the present application or the solid electrolyte membrane prepared by the preparation method provided in the second aspect of the present application.
[0113] In some embodiments, the secondary battery further includes a positive electrode and a negative electrode, and the first solid electrolyte layer and the second solid electrolyte layer in the solid electrolyte membrane are adjacent to the positive electrode and the negative electrode in the secondary battery, respectively.
[0114] The present application will be further described below with reference to specific embodiments and comparative examples.
[0115] Example 1
[0116] Solid electrolyte membrane:
[0117] (1) 1.27 g of lithium lanthanum zirconium titanate (LLZTO) was dissolved in 32.92 mL of N,N-dimethylacetamide (DMAc), and the mixture was stirred for 1 h at 0°C in a nitrogen atmosphere to obtain a first mixed solution; then 2.24 g of 1S,2S,4R,5R-cyclohexanetetracarboxylic dianhydride (H'PMDA) and 3.20 g of 2,2'-bis(trifluoromethyl)diaminobiphenyl (TFMB) were added to the first mixed solution, and the mixture was stirred for 12 h at 0°C at a speed of 600 r / min to obtain a porous base film precursor solution.
[0118] Wherein, the molar ratio of H'PMDA to TFMB is 1:1.
[0119] (2) Pour the porous base film precursor liquid onto a glass plate and perform a first coating process. Manually adjust the scraper height to 20 μm and the coating speed to 5 cm / min to obtain a first liquid film.
[0120] (3) Spray ethanol and N,N-dimethylacetamide (DMAc) in a volume ratio of 1:1 on the first liquid film, soak it at 25°C for 100 minutes, take it out, and place it in an oven at 40°C for a first drying treatment for 3 hours, and then perform a thermal imidization treatment to obtain a porous base membrane.
[0121] Among them, the mass proportion of LLZTO in the porous base membrane is 20%; the heating program of thermal imidization treatment is as follows: stage one: heating to 100°C at 5°C / min, keeping warm for 30 minutes; stage two: heating to 200°C at 5°C / min, keeping warm for 30 minutes; stage three: heating to 300°C at 5°C / min, keeping warm for 30 minutes.
[0122] (4) Mix 0.8 g of polyethylene oxide (PEO), 0.14 g of lithium bis(fluorosulfonyl)imide (LiFSI) and 10 mL of N,N-dimethylformamide (DMF), and perform a third stirring treatment at 40° C. for 24 hours to obtain a second mixed solution; add 0.06 g of lithium lanthanum zirconate titanate (LLZTO) to the second mixed solution, and perform a fourth stirring treatment at 40° C. for 12 hours. The stirring speed of the fourth stirring treatment is 400 rpm / min to obtain a filler liquid.
[0123] (5) placing the porous base membrane on a flat plate; filling the pores of the porous base membrane with a filler liquid, removing excess filler on the surface of the porous substrate with a scraper, and performing a second drying treatment at 80° C. for 12 hours to form a solid electrolyte layer and obtain a solid electrolyte membrane.
[0124] Among them, LLZTO accounts for 6% of the mass in the solid electrolyte layer; the thickness of the solid electrolyte membrane is 20μm.
[0125] Secondary battery:
[0126] The secondary battery includes a positive electrode, a negative electrode and the above-mentioned solid electrolyte membrane. The secondary battery is assembled in a glove box filled with argon gas, with metallic lithium as the negative electrode and lithium iron phosphate material as the positive electrode (LFP:SP:PVDF=8:1:1).
[0127] Example 2
[0128] Solid electrolyte membrane:
[0129] (1) 1.27 g of lithium lanthanum zirconium titanate (LLZTO) was dissolved in 32.92 mL of N,N-dimethylacetamide (DMAc), and the mixture was stirred for 1 h at 0°C in a nitrogen atmosphere to obtain a first mixed solution; 2.24 g of 1S,2S,4R,5R-cyclohexanetetracarboxylic dianhydride (H'PMDA) and 3.20 g of 2,2'-bis(trifluoromethyl)diaminobiphenyl (TFMB) were added to the first mixed solution, and the mixture was stirred for 12 h at 0°C at a stirring speed of 600 r / min to obtain a porous base film precursor solution.
[0130] Wherein, the molar ratio of H'PMDA to TFMB is 1:1.
[0131] (2) Pour the porous base film precursor liquid onto a glass plate and perform a first coating process. Manually adjust the scraper height to 20 μm and the coating speed to 5 cm / min to obtain a first liquid film.
[0132] (3) Ethanol and N,N-dimethylacetamide (DMAc) in a volume ratio of 1:1 are sprayed on the first liquid film, and a first immersion treatment is performed at 25°C for 100 minutes. The film is taken out and placed in an oven at 40°C for a first drying treatment for 3 hours, followed by a thermal imidization treatment to obtain a porous base film.
[0133] Among them, the mass proportion of LLZTO in the porous base membrane is 20%; the heating program of thermal imidization treatment is as follows: stage one: heating to 100°C at 5°C / min, keeping warm for 30 minutes; stage two: heating to 200°C at 5°C / min, keeping warm for 30 minutes; stage three: heating to 300°C at 5°C / min, keeping warm for 30 minutes.
[0134] (4) Mix 0.87 g of poly (vinylidene fluoride-hexafluoropropylene) (PVDF-HFP), 0.07 g of the first electrolyte salt lithium bis(fluorosulfonyl)imide (LiFSI), and 20 mL of the second solvent N,N-dimethylformamide (DMF), and perform a third stirring treatment to obtain a third mixed solution; add 0.06 g of the first nano-ceramic material lithium aluminum titanium phosphate (LATP) to the third mixed solution, and perform a fourth stirring treatment to obtain a first filler liquid.
[0135] (5) Mix 0.8 g of polyethylene oxide (PEO), 0.14 g of lithium bis(fluorosulfonyl)imide (LiFSI), and 20 mL of N,N-dimethylformamide (DMF), and perform a third stirring treatment to obtain a fourth mixed solution; add 0.06 g of a second nano-ceramic material, lithium lanthanum zirconate titanate (LLZTO), to the fourth mixed solution, and perform a fourth stirring treatment again to obtain a second filler liquid.
[0136] In step (4) and step (5), the third stirring treatment is performed at 40° C. for 12 h, and the fourth stirring treatment is performed at 40° C. for 12 h. The stirring speed of the fourth stirring treatment is 400 rpm / min.
[0137] (6) performing a third coating treatment on the second filler liquid at a coating speed of 5 cm / min to obtain a third liquid film; placing the porous base film into the third liquid film for immersion treatment, taking it out, and performing a second drying treatment to form a second solid electrolyte layer (in the second solid electrolyte layer, the mass proportion of LLZTO is 6%, and the mass proportion of PEO is 80%) to obtain a second intermediate;
[0138] The blade height of the third coating process was 12 μm.
[0139] (7) performing a second coating treatment on the first filler liquid at a coating speed of 5 cm / min to obtain a second liquid film; placing the second intermediate into the second liquid film for a second immersion treatment, taking it out, and performing a second drying treatment again to form a first solid electrolyte layer (in the first solid electrolyte layer, the mass proportion of LATP is 6%, and the mass proportion of PVDF-HFP is 87%) to obtain a solid electrolyte membrane.
[0140] The scraper height of the second coating process is 8 μm, the thickness ratio of the first solid electrolyte layer to the second solid electrolyte layer is 4:6; and the thickness of the solid electrolyte membrane is 20 μm.
[0141] In step (6) and step (7), the temperature of the second drying treatment is 80° C., and the time of the second drying treatment is 12 hours.
[0142] Secondary battery:
[0143] The secondary battery includes a positive electrode, a negative electrode and the above-mentioned solid electrolyte membrane. The secondary battery is assembled in a glove box filled with argon gas, with metallic lithium as the negative electrode and lithium iron phosphate material as the positive electrode (LFP:SP:PVDF=8:1:1).
[0144] The first solid electrolyte layer and the second solid electrolyte layer in the solid electrolyte membrane are adjacent to the positive electrode and the negative electrode in the secondary battery respectively.
[0145] Example 3
[0146] The preparation method of the solid electrolyte membrane and the secondary battery in this embodiment is basically the same as that in Embodiment 2, except that:
[0147] In step (1), LLZTO is replaced with aluminum oxide (Al2O3).
[0148] Example 4
[0149] The preparation method of the solid electrolyte membrane and the secondary battery in this embodiment is basically the same as that in Embodiment 2, except that:
[0150] The LATP in the first solid electrolyte layer and the LLZTO in the second solid electrolyte layer were both replaced with titanium dioxide (TiO2).
[0151] Example 5
[0152] The preparation method of the solid electrolyte membrane and the secondary battery in this embodiment is basically the same as that in Embodiment 2, except that:
[0153] The PVDF-HFP in step (4) is replaced by PAN, and in the first solid electrolyte layer, the mass proportion of LATP is 10%, and the mass proportion of PAN is 80%.
[0154] The PEO in step (5) is replaced with PEGMA, and in the second solid electrolyte layer, the mass proportion of LLZTO is 10%, and the mass proportion of PEGMA is 70%.
[0155] Example 6
[0156] The preparation method of the solid electrolyte membrane and the secondary battery in this embodiment is basically the same as that in Embodiment 2, except that:
[0157] The PVDF-HFP in step (4) is replaced by PMMA, and in the first solid electrolyte layer, the mass proportion of LATP is 1%, and the mass proportion of PAN is 94%.
[0158] The PEO in step (5) is replaced with PET, and in the second solid electrolyte layer, the mass proportion of LLZTO is 1%, and the mass proportion of PEGMA is 89%.
[0159] Example 7
[0160] The preparation method of the solid electrolyte membrane and the secondary battery in this embodiment is basically the same as that in Embodiment 1, except that:
[0161] In step (1), 5.08 g of polyimide (PI) and 1.27 g of lithium lanthanum zirconium titanate (LLZTO) were dissolved in N,N-dimethylformamide (DMF), and stirred at 0° C. in a nitrogen atmosphere for 12 h to obtain a porous base film precursor solution.
[0162] Example 8
[0163] The preparation method of the solid electrolyte membrane and the secondary battery in this embodiment is basically the same as that in Embodiment 2, except that:
[0164] In step (6), the blade height of the third coating process is 14 μm.
[0165] In step (7), the blade height of the second coating process is 6 μm.
[0166] The thickness ratio of the first solid electrolyte layer to the second solid electrolyte layer is 3:7.
[0167] Example 9
[0168] The preparation method of the solid electrolyte membrane and the secondary battery in this embodiment is basically the same as that in Embodiment 2, except that:
[0169] In step (6), the blade height of the third coating process is 6 μm.
[0170] In step (7), the blade height of the second coating process is 14 μm, and the thickness ratio of the first solid electrolyte layer to the second solid electrolyte layer is 7:3.
[0171] Example 10
[0172] The preparation method of the solid electrolyte membrane and the secondary battery in this embodiment is basically the same as that in Embodiment 2, except that:
[0173] Replace the PVDF-HFP in step (4) with PEO;
[0174] The PEO in step (5) was replaced by PVDF-HFP.
[0175] Comparative Example 1
[0176] Solid electrolyte membrane:
[0177] (1) 2.24 g of 1S,2S,4R,5R-cyclohexanetetracarboxylic dianhydride (H'PMDA) and 3.20 g of 2,2'-bis(trifluoromethyl)diaminobiphenyl (TFMB) were dissolved in 32.92 mL of N,N-dimethylacetamide (DMAc) and subjected to a first stirring treatment in a nitrogen atmosphere at 0°C for 1 h to obtain a porous base film precursor solution.
[0178] The molar ratio of H'PMDA to TFMB is 1:1.
[0179] (2) Pour the porous base film precursor liquid onto a glass plate and perform a first coating process. Manually adjust the scraper height to 20 μm and the coating speed to 5 cm / min to obtain a first liquid film.
[0180] (3) Spray ethanol and N,N-dimethylacetamide (DMAc) in a volume ratio of 1:1 on the first liquid film, soak it at 25°C for 100 minutes, take it out, and place it in an oven at 40°C for a first drying treatment for 3 hours, and then perform a thermal imidization treatment to obtain a porous base membrane.
[0181] The heating procedure of thermal imidization treatment is as follows: stage one: heating to 100°C at 5°C / min and keeping warm for 30 minutes; stage two: heating to 200°C at 5°C / min and keeping warm for 30 minutes; stage three: heating to 300°C at 5°C / min and keeping warm for 30 minutes.
[0182] (4) Mix 0.8 g of polyethylene oxide (PEO), 0.14 g of lithium bis(fluorosulfonyl)imide (LiFSI) and 10 mL of N,N-dimethylformamide (DMF), and perform a third stirring treatment at 40° C. for 24 hours to obtain a second mixed solution; add 0.06 g of lithium lanthanum zirconate titanate (LLZTO) to the second mixed solution, and perform a fourth stirring treatment at 40° C. for 12 hours. The stirring speed of the fourth stirring treatment is 400 rpm / min to obtain a filler liquid.
[0183] The third stirring treatment was performed at 40° C. for 12 h, the fourth stirring treatment was performed at 40° C. for 12 h, and the stirring speed of the fourth stirring treatment was 400 rpm / min.
[0184] (5) placing the porous base membrane on a flat plate; filling the pores of the porous base membrane with a filler liquid, removing excess filler on the surface of the porous substrate with a scraper, and performing a second drying treatment at 80° C. for 12 hours to obtain a solid electrolyte membrane having a thickness of 20 μm.
[0185] Secondary battery:
[0186] The secondary battery includes a positive electrode, a negative electrode and the above-mentioned solid electrolyte membrane. The secondary battery is assembled in a glove box filled with argon gas, with metallic lithium as the negative electrode and lithium iron phosphate material as the positive electrode (LFP:SP:PVDF=8:1:1).
[0187] Comparative Example 2
[0188] Solid electrolyte membrane:
[0189] (1) 1.27 g of lithium lanthanum zirconium titanate (LLZTO) was dissolved in 32.92 mL of N,N-dimethylacetamide (DMAc), and a first stirring treatment was performed in a nitrogen atmosphere at 0°C for 1 h to obtain a first mixed solution; 2.24 g of 1S,2S,4R,5R-cyclohexanetetracarboxylic dianhydride (H'PMDA) and 3.20 g of 2,2'-bis(trifluoromethyl)diaminobiphenyl (TFMB) were added to the first mixed solution, and a second stirring treatment was performed at 0°C for 12 h at a stirring speed of 600 r / min to obtain a porous base film precursor solution.
[0190] The molar ratio of H'PMDA to TFMB is 1:1.
[0191] (2) Pour the porous base film precursor liquid onto a glass plate and perform a first coating process. Manually adjust the scraper height to 20 μm and the coating speed to 5 cm / min to obtain a first liquid film.
[0192] (3) Spray ethanol and N,N-dimethylacetamide (DMAc) in a volume ratio of 1:1 on the first liquid film, soak it at 25°C for 100 minutes, take it out, and place it in an oven at 40°C for a first drying treatment for 3 hours, and then perform a thermal imidization treatment to obtain a porous base membrane.
[0193] The heating procedure of thermal imidization treatment is as follows: stage one: heating to 100°C at 5°C / min and keeping warm for 30 minutes; stage two: heating to 200°C at 5°C / min and keeping warm for 30 minutes; stage three: heating to 300°C at 5°C / min and keeping warm for 30 minutes.
[0194] (4) 0.8 g of polyethylene oxide (PEO), 0.14 g of lithium bis(fluorosulfonyl)imide (LiTFSI) and mL of N,N-dimethylformamide (DMF) were mixed and subjected to a third stirring treatment at 40° C. for 24 h to obtain a filler solution.
[0195] The third stirring treatment was performed at 40° C. for 12 h, the fourth stirring treatment was performed at 40° C. for 12 h, and the stirring speed of the fourth stirring treatment was 400 rpm / min.
[0196] (5) placing the porous base membrane on a flat plate; filling the pores of the porous base membrane with a filler liquid, removing excess filler on the surface of the porous substrate with a scraper, and performing a second drying treatment at 80° C. for 12 hours to obtain a solid electrolyte membrane having a thickness of 20 μm.
[0197] Secondary battery:
[0198] The secondary battery includes a positive electrode, a negative electrode and the above-mentioned solid electrolyte membrane. The secondary battery is assembled in a glove box filled with argon gas, with metallic lithium as the negative electrode and lithium iron phosphate material as the positive electrode (LFP:SP:PVDF=8:1:1).
[0199] Performance Testing
[0200] (1) Stress-strain test
[0201] The solid electrolyte membranes obtained in the above examples and comparative examples were prepared as samples, and a tensile machine was used to apply gradually increasing tensile loads to deform the samples until they were destroyed. The maximum tensile stress required for the samples to be destroyed was the stress yield strength. The test results are shown in Table 1.
[0202] (2) Flame retardant performance test
[0203] The solid electrolyte membranes obtained in the above examples and comparative examples were tested for limiting oxygen index (LOI) according to GB / T 2406.1-2008 standard. The test results are shown in Table 1.
[0204] (3) Ionic conductivity test
[0205] The solid electrolyte membrane obtained in the above embodiments and comparative examples adopts the test structure of stainless steel sheet / solid electrolyte membrane / stainless steel sheet and the AC impedance method, and the frequency range is 10 -2 Hz-10 6 Hz, AC signal amplitude Z is 10 -2 The AC impedance test was carried out under the condition of 40°C and the ionic conductivity was calculated. The test temperature was 40°C. The test results are shown in Table 1.
[0206] (4) Electrochemical performance test
[0207] The secondary batteries obtained in the above examples and comparative examples were connected to a charge and discharge tester, and were set to charge to 4.2V at a constant current of 0.5C, and to discharge to 2.5V at a constant current of 0.5C, for more than 300 cycles, and the test temperature was 60°C. The test results are shown in Table 1.
[0208] Table 1
[0209]
[0210] As shown in Table 1, by comparing Examples 1 to 10 and Comparative Examples 1 to 2, it can be seen that the solid electrolyte membrane and secondary battery provided by the present application improve the flame retardant performance while improving the mechanical strength and ionic conductivity, thereby improving the electrochemical performance of the secondary battery.
[0211] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0212] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the present application. It should be pointed out that, for a person of ordinary skill in the art, several modifications and improvements can be made without departing from the technical concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the present application shall be subject to the attached claims.
Claims
1. A solid electrolyte membrane, characterized in that: include: A porous base film, wherein the material of the porous base film includes polyimide and an inorganic flame retardant; The solid electrolyte layer is formed in the pores of the porous base film, and the solid electrolyte layer comprises a polymer solid electrolyte, an electrolyte salt and a nano-ceramic material.
2. The solid electrolyte membrane according to claim 1, characterized in that The solid electrolyte layer comprises: A first solid electrolyte layer, the first solid electrolyte layer comprising a first polymer solid electrolyte, a first electrolyte salt and a first nano-ceramic material; A second solid electrolyte layer, the second solid electrolyte layer comprising a second polymer solid electrolyte, a second electrolyte salt and a second nano-ceramic material; The first solid electrolyte layer faces the positive electrode of the electrochemical device, the second solid electrolyte layer faces the negative electrode of the electrochemical device, and the first polymer solid electrolyte has better oxidation resistance than the second polymer solid electrolyte.
3. The solid electrolyte membrane according to claim 2, characterized in that: The thickness ratio of the first solid electrolyte layer to the second solid electrolyte layer is (3:7) to (7:3).
4. The solid electrolyte membrane according to claim 2, characterized in that: The mass percentage of the first nano-ceramic material in the first solid electrolyte layer is 1% to 10%; and / or, The mass proportion of the second nano-ceramic material in the second solid electrolyte layer is 1% to 10%.
5. The solid electrolyte membrane according to claim 2, characterized in that: The mass proportion of the first polymer solid electrolyte in the first solid electrolyte layer is 80% to 94%; and / or, The mass proportion of the second polymer solid electrolyte in the second solid electrolyte layer is 70% to 89%.
6. The solid electrolyte membrane according to claim 2, characterized in that The first polymer solid electrolyte includes at least one of poly(vinylidene fluoride-hexafluoropropylene) (PVDF-HFP), polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), polymethyl methacrylate (PMMA), and polypropylene carbonate (PPC); the second polymer solid electrolyte includes at least one of polyethylene oxide (PEO), polyethylene glycol monomethyl ether acrylate (PEGMA), polydioxolane, polyethylene carbonate, and polyethylene terephthalate (PET).
7. The solid electrolyte membrane according to any one of claims 1 to 6, characterized in that: The inorganic flame retardant accounts for 10% to 30% by weight in the porous base film.
8. The solid electrolyte membrane according to any one of claims 1 to 6, characterized in that: The solid electrolyte membrane satisfies at least one of the following characteristics: (1) The thickness of the solid electrolyte membrane is 20 μm to 60 μm; (2) The ionic conductivity (40°C) of the solid electrolyte membrane is 2.6*10 -5 S / cm~8.7*10 -4 S / cm.
9. A method for preparing a solid electrolyte membrane according to any one of claims 1 to 8, characterized in that: The following steps are involved: The dianhydride compound, the diamine compound and the inorganic flame retardant are mixed and subjected to thermal imidization treatment to prepare a porous base film; forming a solid electrolyte layer in the pores of the porous base membrane to prepare a solid electrolyte membrane; Wherein, the solid electrolyte layer comprises a polymer solid electrolyte, an electrolyte salt and a nano-ceramic material.
10. A secondary battery, characterized in that: The invention comprises the solid electrolyte membrane according to any one of claims 1 to 8 or the solid electrolyte membrane prepared by the preparation method according to claim 9.
Citation Information
Cited By
Hybrid solid electrolyte film with efficient flame retardant property and preparation method and application thereof
CN116960453A
Gradient-coated graphite composite negative electrode material, preparation method thereof and lithium ion battery
CN120565651A
Nano hard alloy composite solid-state electrolyte membrane, preparation method and solid-state lithium battery
CN122552605A