Manufacturing method of multi-layer glass substrate
Through flexible glass and magnetron sputtering coating technology, the problems of through-hole processing and insufficient thickness in glass substrate processing are solved, and efficient and low-cost multi-layer glass substrate production is achieved, which improves production efficiency and material stability. In small size and multi-module chip packages.
Patent Information
- Application Number
- CN202411013877.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
AI Technical Summary
The existing glass substrates have problems of through-hole processing and insufficient thickness during processing, resulting in high cost and low production efficiency, and flexible glass is prone to fragmentation during subsequent processing.
Using flexible glass and magnetron sputtering coating technology, multi-layer glass substrates are formed through sputtering copper plating, vacuum compression, laser drilling, chemical copper deposition and layering processes, which avoids glass fragmentation and improves production efficiency and Cost-effective.
It realizes efficient processing of glass substrates, reduces costs, improves production efficiency, avoids the use of hazardous chemicals, enhances the stability and signal transmission performance of materials, and is suitable for small-size and multi-module chip packaging.
Smart Images

Figure CN118973146A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of printed circuit board manufacturing, and in particular to a manufacturing method of a multi-layer glass substrate. Background Art
[0002] IC substrates meet the requirements of chips and packaging methods. In the current digital era, PCB requirements are thin, short, high-speed, high-density and multi-functional, specifically thin, fine lines, small holes, precise size, stable performance and low cost.
[0003] Glass substrate is also a type of IC carrier. Compared with IC carriers made of organic materials, it has significant advantages such as low cost, low high-frequency loss, high integration, and adjustable thermal expansion coefficient. It has become a hot topic of research at home and abroad.
[0004] Comparison between glass substrate and silicon adapter board: Silicon adapter board is relatively small in size, has low production efficiency and high cost. In addition, silicon adapter board technology is affected by front-end advanced wafer manufacturing, and the supply chain is relatively mature. However, the relevant silicon adapter board process development technology is only mastered by some powerful wafer manufacturing companies, so it has certain industrial chain barriers.
[0005] Glass substrate (glass adapter plate) is a relatively cutting-edge technology. Its supply chain and process development technology have not yet formed a market-scale effect. It is a high-performance application technology for the next generation of adapter plates that is highly anticipated.
[0006] Cost is the key to industrializing technological achievements and opening up the market; among the three types of adapter board technologies, once the technology matures, the cost of the glass adapter board process is the lowest, and the silicon adapter board process has the highest cost. The limited size of silicon wafers and related manufacturing costs make their overall cost much higher than glass and organic adapter boards. In the future, if the 5μm L / S and mechanical reliability issues are to be overcome, the organic substrate technology will have to add huge process costs, while the glass adapter board technology has inherent performance advantages. If the process stability can be overcome, its cost will drop significantly and be accepted by downstream application customers.
[0007] In terms of the existing process flow of organic IC substrates, the dielectric properties and thermal expansion properties of organic resin materials are not as good as those of glass, the resin roughness is large, the copper foil is relatively thick, and it cannot meet the 5μm L / S requirement and has problems with mechanical reliability. The use of glass substrate instead of organic resin as the substrate of the circuit board has higher thermal stability and dimensional stability, lower dielectric constant, higher signal transmission speed, less loss, and can significantly improve electrical and mechanical properties. The adjustable modulus and CTE are closer to silicon chips, the size is more stable, and it supports large-size and multi-module chip packaging, thereby improving product performance, density, and flexibility.
[0008] When a glass substrate is manufactured, the thickness of the glass used as the base material is generally greater than 0.2 mm, which will cause difficulties in processing glass through holes. Even if the glass through holes are processed, the thickness-to-diameter ratio is too large, making it difficult to achieve conduction of the through holes. If a flexible glass with a thickness of less than 0.2 mm is used, it is relatively easy to process the glass through holes, as shown in the prior application "CN2024108471054 A method for manufacturing a glass through hole", but flexible glass that is too thin is prone to breakage during subsequent sputtering, electroplating, photolithography and other processing. Summary of the invention
[0009] In view of the above-mentioned existing technical defects, the present invention provides a method for manufacturing a multi-layer glass substrate, which utilizes mature flexible glass and magnetron sputtering coating technology to realize the processing of the multi-layer glass substrate, with high production efficiency and low processing cost.
[0010] In a first aspect, in order to solve the above technical problem, the present invention provides a method for manufacturing a multi-layer glass substrate, comprising the following steps:
[0011] S1, performing sputtering copper plating on one surface of the flexible glass to form a glass copper-coated film;
[0012] S2, stacking two glass copper-clad films by means of a prepreg and then vacuum pressing them to form a core board, wherein a side of the glass copper-clad film having a copper layer is located on the outside of the core board;
[0013] S3, using a carbon dioxide laser to perform laser drilling on the core board to drill through holes and / or blind holes;
[0014] S4, performing chemical copper deposition on the core board to metallize the through holes and / or blind holes;
[0015] S5, firstly making an inner layer circuit pattern on the core board, and then sequentially performing electroplating, film stripping and etching to make an inner layer circuit on the core board;
[0016] S6, repeating steps S2-S5 at least once according to the layer-adding manufacturing method to manufacture a multilayer board with the required number of layers;
[0017] S7, and then sequentially carry out solder mask making, surface treatment and shape cutting processes to obtain a glass substrate.
[0018] Furthermore, the flexible glass is alkali-free glass, and the thickness of the flexible glass is 0.03-0.2 mm.
[0019] Furthermore, in step S1, a copper plating layer with a thickness of 0.2-1 μm is sputtered on a single surface of the flexible glass by a roll-to-roll vacuum coating method; and before the sputtering copper plating, a 50-100 nanometer thick aluminum transition layer or chromium transition layer is first sputtered on a single surface of the flexible glass, and then a copper plating layer is sputtered on the single surface of the flexible glass, and the copper plating layer is located on the outside of the aluminum transition layer or the chromium transition layer.
[0020] Furthermore, in step S2, after vacuum pressing, the weight of the glass component accounts for more than 80% of the total weight of the insulating material in the core board, wherein the content of the glass fiber cloth in the prepreg is 30% or more.
[0021] Furthermore, in step S3, double-sided drilling is used for drilling through holes, and the depth of laser drilling on each side is controlled to be above 60% during double-sided drilling; the blind hole drilling reaches the bottom copper layer.
[0022] Furthermore, in step S3, after laser drilling, the core board is brushed and plasma cleaned to remove the particles splashed by laser drilling vaporization and the residues at the bottom of the hole.
[0023] Furthermore, in step S4, the thickness of the electroless copper deposition is 0.2-0.4 μm, so as to metallize the through hole or blind hole wall, and the amount of copper micro-etching during the electroless copper deposition process is less than 0.1 μm.
[0024] Furthermore, in step S5, a film is first pasted on the core board, and then an inner layer circuit pattern is formed by exposure and development, and then the core board is subjected to hole filling electroplating, pattern electroplating, film stripping and micro-etching processes in sequence to form an inner layer board; and during the pattern electroplating, only copper is electroplated without tin.
[0025] Further, step S6 includes the following steps:
[0026] S61, laminating a glass-coated copper film on both sides of the core board through a prepreg and then vacuum pressing to form a four-layer multilayer board, wherein the side of the glass-coated copper film having a copper layer is located on the outside of the multilayer board;
[0027] S62, repeating steps S3 to S5 to form a four-layer multilayer board.
[0028] Furthermore, the following steps are included between step S62 and step S7:
[0029] S63, repeating steps S61 to S62 at least once to obtain a multilayer board with six layers, eight layers, ten layers or more layers.
[0030] Furthermore, during the processing of the glass substrate, no hazardous chemical such as hydrofluoric acid is used.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] The use of flexible glass-coated copper film material not only realizes the use of glass material, but also realizes the use of ultra-thin copper foil (less than 1 micron) material; the combination of these two materials in processing not only facilitates the processing of the substrate, but also facilitates the roll-to-roll mass production of the material.
[0033] In the present invention, ultra-thin flexible glass is used as the base material of the glass substrate, and a copper layer is plated on one side of the glass substrate and then the glass substrate is formed into a core plate by vacuum pressing with a semi-cured sheet. The glass thickness formed by vacuum pressing two pieces of flexible glass meets the base material thickness required by the production design, and the problem of the overly thin flexible glass being broken during the subsequent drilling, copper deposition, electroplating, photolithography and other processing processes is avoided. During the laser drilling process, the glass has a large absorption rate for carbon dioxide laser, but a very small absorption rate for laser with a wavelength of 0.2-5 microns. Therefore, the carbon dioxide laser is used for drilling in the present method, which effectively improves the production efficiency. In order to avoid the disadvantages of carbon dioxide laser drilling, both surfaces of the core plate formed after vacuum pressing are plated with The copper layer uses the sputtered copper layer as the MASK (mask) of the laser hole, which can reflect the carbon dioxide laser, reduce the range of laser heat influence, thereby reducing the generation of thermal effect cracks, and control the size of the laser hole, thereby reducing the aperture of the carbon dioxide laser processing hole, avoiding the problems of excessive laser drilling and hole cracking. Therefore, the method of the present invention uses mature flexible glass and magnetron sputtering coating technology to realize the processing of glass substrates, with high production efficiency and low processing cost; the production process of the method of the present invention does not use hazardous chemicals such as hydrofluoric acid, thereby improving the safety of the production process and reducing environmental pollution, and the equipment of existing HDI board manufacturers can be used to easily transform the production of the glass substrate, with low investment cost.
[0034] Secondly, glass accounts for more than 80% of the core board insulation material, making the expansion rate of the glass substrate material closer to the expansion rate of the chip, so that the package size can be made larger, and the material in contact with the copper layer of the manufactured circuit is all glass. The base layer of the copper wiring is a flat glass with extremely small roughness, and the roughness Ra is less than 1 nanometer. It can produce lines with a line width and line spacing less than 10 microns. The roughness level of existing organic materials can only be at the 1 micron level (1000 nanometers). This roughness of organic materials will cause large signal transmission losses and it is difficult to produce lines below 10 microns.
[0035] In addition, a multi-layer glass substrate with four, six, eight, ten or more layers can be produced by adding layers, thereby realizing the processing of the multi-layer glass substrate with high production efficiency and low processing cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1Schematic diagram of copper plating on the surface of flexible glass in the embodiment;
[0037] Figure 2 This is a schematic diagram of a core board after being pressed together in an embodiment;
[0038] Figure 3 This is a schematic diagram of drilling holes on a core board in an embodiment;
[0039] Figure 4 This is a schematic diagram of copper deposition on a core board in an embodiment;
[0040] Figure 5 This is a schematic diagram of the inner layer circuits produced on the core board in the embodiment;
[0041] Figure 6 This is a schematic diagram of a multi-layer board after being pressed into a multi-layer board by using a layer-building method in an embodiment;
[0042] Figure 7 A schematic diagram of drilling holes on a multilayer board and making circuits in an embodiment; DETAILED DESCRIPTION
[0044] In order to more fully understand the technical content of the present invention, the technical solution of the present invention will be further introduced and illustrated in conjunction with specific embodiments below.
[0045] Example 1
[0046] The method for manufacturing a multi-layer glass substrate shown in this embodiment includes the following steps in sequence:
[0047] a. Copper coating on flexible glass: prepare a roll of flexible glass, and sputter a copper plating layer 2 on one surface of the flexible glass 1, so as to compound the glass and copper foil into a material that is easy to process, and form a glass copper coating film; wherein the thickness of the flexible glass is 0.1 mm, and the thickness of the copper plating layer on the surface of the flexible glass is 0.5 μm.
[0048] In one embodiment, a copper plating layer with a thickness of 0.5 μm is sputtered on a single surface of the flexible glass by a roll-to-roll vacuum coating method.
[0049] In one embodiment, before sputtering copper, a 50-nanometer-thick aluminum transition layer is first sputtered on a single surface of the flexible glass, and then a copper-plated layer is sputtered on the single surface of the flexible glass. The copper-plated layer is located outside the aluminum transition layer. The transition layer is provided to improve the bonding strength between the copper-plated layer and the flexible glass.
[0050] In another embodiment, before sputtering copper, a 100-nanometer-thick chromium transition layer is first sputtered on a single surface of the flexible glass, and then a copper-plated layer is sputtered on the single surface of the flexible glass. The copper-plated layer is located outside the chromium transition layer. The transition layer is set to improve the bonding strength between the copper-plated layer and the flexible glass.
[0051] In one embodiment, the flexible glass is alkali-free glass, which has the characteristics of high light transmittance and good photoelectric performance.
[0052] In another embodiment, the thickness of the flexible glass may also be 0.03-0.2 mm.
[0053] In another embodiment, the thickness of the copper plating layer on the surface of the flexible glass may also be 0.2-1 μm.
[0054] b. Cutting: Cut the copper-clad glass film according to the size of the panel to form pieces of copper-clad glass film.
[0055] c. Vacuum lamination: Two glass copper films are overlapped by SI 10U prepreg and then vacuum pressed to form a core board; Figure 2 As shown, when stacked, the prepreg 3 is located between the two glass copper-clad films, and the glass surface of the glass copper-clad film without a copper layer is in contact with the prepreg, and the surface of the glass copper-clad film with a copper layer is located on the outside of the core board; wherein, the glass fiber cloth model of the prepreg is 1017, the thickness of the prepreg is 25 microns, and the content of the glass fiber cloth in the prepreg (i.e., weight percentage) is 30%.
[0056] After vacuum pressing, the weight of glass components accounts for 92% of the core board insulation material, and all materials in contact with copper are glass; the content of glass fiber cloth in the semi-cured sheet is more than 30%.
[0057] In another embodiment, after vacuum pressing, the weight of the glass component may account for more than 80% of the core board insulation material.
[0058] d. Drilling: According to the drilling data, a carbon dioxide laser is then used to perform laser drilling processing at the hole position on the core board to drill through holes 4 and / or blind holes (such as Figure 3 The core plate is then scrubbed and plasma cleaned to remove the particles and residues at the bottom of the hole caused by the laser drilling gasification.
[0059] In one embodiment, when drilling through holes, the core board is laser drilled by double-sided drilling, that is, the same hole position is double-sided drilled from both sides of the core board, so that the upper and lower apertures of the drilled through holes are relatively consistent, avoiding the hole opening at the light outlet being too small, resulting in poor copper plating on the hole wall.
[0060] In one embodiment, the depth of laser drilling on each side is controlled to be more than 60% of the thickness of the core board, so that the holes drilled on both sides have upper and lower overlapping parts.
[0061] In one embodiment, the blind vias are drilled to reach the bottom copper layer.
[0062] e. Copper deposition: Chemical copper deposition is performed on the core board to metallize the through holes and / or blind holes (such as Figure 4 As shown in the figure, the thickness of the copper layer during chemical copper deposition is 0.3 μm; because the copper layer on the surface of the core board is very thin, the micro-etching amount during chemical copper deposition is controlled at 0.1 μm.
[0063] f. Inner layer pattern production: firstly, a dry film is pasted on the core board, and then the inner layer circuit pattern is formed on the core board through exposure and development, that is, the copper surface of the inner layer circuit pattern is exposed, while the inner layer circuit pattern and the copper surface of the part other than the hole are covered and protected by the dry film, and then the copper layer of the inner layer circuit pattern is thickened by hole filling electroplating and pattern electroplating. During the pattern electroplating, only copper is electroplated without tin. After the dry film is removed, the bottom copper of the part other than the inner layer circuit pattern is removed by micro-etching to obtain the inner layer circuit 5 (such as Figure 5 shown).
[0064] g. Vacuum lamination: By adding layers, a glass copper film is laminated on both sides of the core board through a semi-cured sheet and then vacuum pressed to form a four-layer multilayer board (such as Figure 6 As shown), that is, when stacked, the prepreg is located between the glass copper clad film and the core board, and the side of the glass copper clad film without a copper layer is in contact with the prepreg, and the side of the glass copper clad film with a copper layer is located on the outside of the multilayer board.
[0065] h. Post-process: Repeat steps c to e to form a four-layer multilayer board; during laser drilling, blind holes connecting the outer layer and the second outer layer are drilled, and the blind holes are filled with via plating (such as Figure 7 shown).
[0066] i. Solder mask and silk-screen characters: After silk-screening solder mask ink on the surface of the multilayer board, it is sequentially processed through pre-curing, exposure, development and heat curing to solidify the solder mask ink into a solder mask layer; specifically, adding "UL mark" to the solder mask ink and characters on the TOP surface, thereby coating a layer on the circuits and substrates that do not require soldering to prevent bridging between circuits during soldering, provide a permanent electrical environment and a protective layer against chemical corrosion, and at the same time beautify the appearance.
[0067] j. Surface treatment (tinning): The copper surface of the pad at the solder mask opening is treated by chemical tin deposition to uniformly deposit a tin layer of a certain required thickness. The thickness of the tin layer is 1 μm, and a four-layer glass substrate is obtained.
[0068] In other embodiments, after step i, the following post-processes are also included in sequence: electrical testing, molding cutting, FQC, FQA, and packaging.
[0069] Example 2
[0070] The method for manufacturing a multi-layer glass substrate shown in this embodiment has the same steps as those in Embodiment 1, except that: a layer-adding method is adopted, and steps f and g are repeated at least once between step g and step h, so that a glass substrate with six layers, eight layers, ten layers or more can be manufactured.
[0071] The technical solutions provided by the embodiments of the present invention are introduced in detail above. Specific examples are used herein to illustrate the principles and implementation methods of the embodiments of the present invention. The description of the above embodiments is only applicable to help understand the principles of the embodiments of the present invention. At the same time, for those skilled in the art, according to the embodiments of the present invention, there will be changes in the specific implementation methods and application scopes. In summary, the content of this specification should not be understood as limiting the present invention.
Claims
1. A method for manufacturing a multi-layer glass substrate, characterized in that: The following steps are involved: S1, performing sputtering copper plating on one surface of the flexible glass to form a glass copper-coated film; S2, stacking two glass copper-clad films by means of a prepreg and then vacuum pressing them to form a core board, wherein a side of the glass copper-clad film having a copper layer is located on the outside of the core board; S3, using a carbon dioxide laser to perform laser drilling on the core board to drill through holes and / or blind holes; S4, performing chemical copper deposition treatment on the core board to metallize the through holes and / or blind holes; S5, firstly making an inner layer circuit pattern on the core board, and then sequentially performing electroplating, film stripping and etching to make an inner layer circuit on the core board; S6, repeating steps S2-S5 at least once according to the layer-adding manufacturing method to manufacture a multilayer board with the required number of layers; S7, and then sequentially carry out solder mask making, surface treatment and shape cutting processes to obtain a glass substrate.
2. The method for manufacturing a multi-layer glass substrate according to claim 1, characterized in that: The flexible glass is alkali-free glass, and the thickness of the flexible glass is 0.03-0.2 mm.
3. The method for manufacturing a multi-layer glass substrate according to claim 1, characterized in that: In step S1, a copper plating layer with a thickness of 0.2-1 μm is sputtered on a single surface of the flexible glass by a roll-to-roll vacuum coating method; and before the sputtering copper plating, a 50-100 nanometer thick aluminum transition layer or chromium transition layer is first sputtered on a single surface of the flexible glass, and then a copper plating layer is sputtered on the single surface of the flexible glass, and the copper plating layer is located on the outside of the aluminum transition layer or the chromium transition layer.
4. The method for manufacturing a multi-layer glass substrate according to any one of claims 1 to 3, characterized in that: In step S2, after vacuum pressing, the weight of the glass component accounts for more than 80% of the total weight of the insulating material in the core board, wherein the content of the glass fiber cloth in the prepreg is 30% or more.
5. The method for manufacturing a multi-layer glass substrate according to claim 1, characterized in that: In step S3, double-sided drilling is used for drilling through holes, and the depth of laser drilling on each side is controlled to be above 60% during double-sided drilling; the blind hole drilling reaches the bottom copper layer.
6. The method for manufacturing a multi-layer glass substrate according to claim 1, characterized in that: In step S3, after laser drilling, the core board is brushed and plasma cleaned to remove the particles splashed by laser drilling gasification and the residues at the bottom of the hole.
7. The method for manufacturing a multi-layer glass substrate according to claim 1, characterized in that: In step S4, the thickness of the electroless copper deposition is 0.2-0.4 μm, so as to metallize the through hole or blind hole wall, and the copper micro-etching amount during the electroless copper deposition process is less than 0.1 μm.
8. The method for manufacturing a multi-layer glass substrate according to claim 1, wherein: In step S5, a film is firstly pasted on the core board, and then an inner layer circuit pattern is formed by exposure and development, and then the core board is subjected to hole filling electroplating, pattern electroplating, film stripping and micro-etching processes in sequence to form an inner layer board; and during the pattern electroplating, only copper is electroplated without tin.
9. The method for manufacturing a multi-layer glass substrate according to claim 1, wherein step S6 comprises the following steps: S61, laminating a glass-coated copper film on both sides of the core board through a prepreg and then vacuum pressing to form a four-layer multilayer board, wherein the side of the glass-coated copper film having a copper layer is located on the outside of the multilayer board; S62, repeating steps S3 to S5 to form a four-layer multilayer board; S63, repeating steps S61 to S62 at least once again to obtain a multilayer board with six layers, eight layers, ten layers or more layers.
10. The method for manufacturing a multi-layer glass substrate according to claim 1, characterized in that: No hydrofluoric acid is used during glass substrate processing.
Citation Information
Cited By
Manufacturing method for improving flatness of BGA (Ball Grid Array) area of glass embedded outer circuit board
CN119730083A
Method for improving surface roughness of glass substrate after laser drilling
CN120023510A
High-density interconnection laminated printed circuit board and preparation method thereof
CN120583593A