Preparation method of organic photovoltaic active layer and solar device

By forming an active layer of the fiber network loading donor and acceptor in an organic photovoltaic device, the aramid nanofiber network is used to inhibit the aggregation and phase separation of the donor/acceptor after heating, the problem of low battery efficiency of organic photovoltaic devices is solved. , improves the performance of solar devices.

CN118973354AInactive Publication Date: 2024-11-15SHENZHEN TECH UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411029023.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The active layer of organic photovoltaic devices is prone to displacement/acceptor movement under heat, affecting molecular orientation, crystallization and phase separation, resulting in low battery efficiency.

Method used

The network layer is formed by spin-coating aramid nanofiber solution on the electron transport layer, and spin-coating BTP-eC9 and PM6 solutions in turn, annealing to form the active layer of the fiber network load donor and acceptor, and the aramid nanofiber network is introduced to inhibit heat-receiving. /Aggregation and phase separation of receptors.

Benefits of technology

It effectively inhibits the movement of the feed/receptor after heating of the active layer, reduces the negative impact on exciton dissociation and carrier transmission, and improves the battery efficiency of solar devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118973354A_ABST
    Figure CN118973354A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of an organic photovoltaic active layer, comprising the following steps: spin-coating an aramid nanofiber solution on an electron transport layer to form a network layer, spin-coating a BTP-eC9 solution on the network layer, annealing to form a receptor on the network layer, spin-coating a PM6 solution on the network layer forming the receptor, and annealing to form an active layer, the organic photovoltaic active layer comprises an electron transport layer and an active layer which are arranged in sequence. The organic photovoltaic active layer obtained by the preparation method provided by the invention is beneficial to inhibiting aggregation and phase separation caused by heat movement of a donor / receptor in the active layer. The invention further provides a solar device beneficial to improving the battery efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of organic photovoltaics, and in particular to a method for preparing an organic photovoltaic active layer and a solar device. Background Art

[0002] Recent studies have shown that organic photovoltaics based on organic semiconductors have a very high weak light effect, especially a very high indoor photoelectric conversion efficiency.

[0003] Organic photovoltaic materials usually have a large π-conjugated structure, and their thermal decomposition temperature is much higher than the device operating temperature, and they have good thermal stability. However, the morphology of the active layer is easily changed under heat, and the donor / acceptor in the active layer is prone to movement, which affects the molecular orientation, crystallization, phase separation scale, interpenetrating network, etc. of the active layer, thereby affecting the processes of exciton dissociation, carrier transport and collection in organic photovoltaic devices, and thus leading to low cell efficiency of solar devices. Summary of the invention

[0004] In order to overcome the deficiencies of the prior art, the present invention aims to provide a method for preparing an organic photovoltaic active layer, so that the organic photovoltaic active layer is conducive to inhibiting the aggregation and phase separation caused by the thermal migration of donors / acceptors in the active layer.

[0005] In addition, the present application also provides a solar device comprising an organic photovoltaic active layer prepared by the method, thereby facilitating improving the cell efficiency of the solar device.

[0006] To solve the above problems, the technical solution adopted by the present invention is as follows:

[0007] A method for preparing an organic photovoltaic active layer, comprising:

[0008] Spin-coating an aramid nanofiber solution on the electron transport layer to form a network layer;

[0009] Spin-coating a BTP-eC9 solution on the network layer and annealing to form receptors on the network layer;

[0010] The PM6 solution is spin-coated on the network layer forming the receptor, and annealed to form an active layer. The organic photovoltaic active layer includes the electron transport layer and the active layer arranged in sequence.

[0011] In some possible implementations, the concentration of the BTP-eC9 solution is 8-10 mg / ml, the concentration of the PM6 solution is 8-10 mg / ml, and the mixing ratio of the aramid nanofibers and the solvent of the aramid nanofiber solution is 1:1 by volume.

[0012] In some possible implementations, the spin coating speed of the aramid nanofiber solution is 1000-4000 rpm, the spin coating speed of the BTP-eC9 solution is 1000-4000 rpm, and the spin coating speed of the PM6 solution is 1000-4000 rpm.

[0013] In some possible implementations, the annealing temperature for forming the receptor is 48° C.-52° C., and the annealing time is 10 minutes. The annealing temperature for forming the organic photovoltaic active layer is 48° C.-52° C., and the annealing time is 10 minutes.

[0014] In some possible embodiments, the solvent of the aramid nanofiber solution is dimethyl sulfoxide, the solvent in the BTP-eC9 solution is chlorobenzene, the solvent dispersant in the BTP-eC9 solution is 1,8-diiodooctane, and the ratio of the chlorobenzene to the 1,8-diiodooctane is 3:2 by volume, and the solvent of the PM6 solution is chlorobenzene.

[0015] In some possible implementations, the electron transport layer is a ZnO layer, and the thickness of the electron transport layer is 20 nm-30 nm.

[0016] In some possible embodiments, the preparation of the electron transport layer includes:

[0017] The ZnO precursor solution was coated on the ITO conductive substrate by blade coating at a speed of 10 mm s -1 -20mm s -1 , the coating temperature is 43℃-60℃, and the distance between the scraper and the ITO conductive substrate is 18μm-30μm;

[0018] Annealing is performed so that the ZnO precursor solution forms the ZnO layer. The annealing temperature is 40-60° C. and the annealing time is 10-20 minutes.

[0019] In some possible implementations, the thickness of the electron transport layer is 20 nm to 28 nm, and the coating speed of the ZnO precursor solution is 15 mm s -1 -18mm s -1 .

[0020] The present application also provides a solar device, comprising a hole transport layer and an electrode layer stacked in sequence, characterized in that the solar device also includes an organic photovoltaic active layer obtained by the preparation method of the organic photovoltaic active layer, and the hole transport layer covers the active layer.

[0021] In some possible implementations, the hole transport layer is a MoO3 layer, the electrode layer is an Ag layer, the thickness of the hole transport layer is 3-6 nm, and the thickness of the electrode layer is 90-115 nm.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] In the present application, after the electron transport layer is spin-coated with an aramid nanofiber solution to form a network layer, the network layer is sequentially spin-coated with a BTP-eC9 solution and a PM6 solution and sequentially annealed, thereby forming an active layer of a fiber network loaded with donors and acceptors. The additionally introduced aramid nanofiber network can inhibit the severe aggregation of donors / acceptors and the increase in the scale of phase separation after the active layer is heated.

[0024] In the present application, a solar device introduces an organic photovoltaic active layer that forms a network-loaded donor and acceptor. When the active layer is heated, the movement of the donor / acceptor is inhibited, thereby helping to reduce the negative impact on the physical processes of exciton dissociation, carrier transport and collection of the solar device, thereby helping to improve the battery efficiency of the solar device.

[0025] The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 A flow chart of a method for preparing an organic photovoltaic active layer provided in one embodiment of the present application;

[0027] Figure 2 Schematic diagram of the molecular structure of PM6 and BTP-eC9;

[0028] Figure 3 A cross-sectional view of a solar device provided in accordance with an embodiment of the present application.

[0029] Description of Figure Numbers:

[0030] 100 - organic photovoltaic active layer; 10 - electron transport layer; 20 - active layer; 30 - ITO conductive substrate; 40 - hole transport layer; 50 - electrode layer; 200 - solar device; S101, S102, S103 - steps. DETAILED DESCRIPTION

[0031] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0032] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0033] Some embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the absence of conflict, the following embodiments and features in the embodiments can be combined with each other.

[0034] Reference Figure 1 , a method for preparing an organic photovoltaic active layer, comprising:

[0035] Step S101, in the electron transport layer 10 (refer to Figure 3 )Spin-coat the aramid nanofiber solution to form a network layer.

[0036] In some embodiments, in order to uniformly mix the aramid nanofibers and the solvent of the aramid nanofiber solution, the ratio is set to 1:1 by volume. In some embodiments, the solvent of the aramid nanofiber solution is dimethyl sulfoxide.

[0037] In another embodiment, the aramid nanofibers may be dissolved in a mixed solvent of N,N-dimethylacetamide and a chloride salt. Exemplarily, the chloride salt may include lithium chloride.

[0038] In some embodiments, the spin coating speed of the aramid nanofiber solution is 1000-4000 rpm to obtain a uniform network layer and improve energy conversion efficiency.

[0039] In some embodiments, the electron transport layer 10 is a ZnO layer, and the thickness of the electron transport layer 10 is 20 nm to 30 nm. The thickness of the electron transport layer 10 is conducive to further improving the battery efficiency.

[0040] In some embodiments, the preparation of the electron transport layer 10 includes:

[0041] The ZnO precursor solution is coated on an ITO (indium tin oxide) conductive substrate 30 (refer to Figure 3 ), the coating speed is 10 mm s -1 -20mm s -1 The coating temperature is 43° C. to 60° C., and the distance between the scraper and the ITO conductive substrate is 18 μm to 30 μm. For example, the ZnO precursor solution can be coated on one side of the ITO conductive substrate 30 .

[0042] Annealing is performed so that the ZnO precursor solution forms the ZnO layer, the annealing temperature is 40-60° C., and the annealing time is 10-20 minutes. After annealing, the ITO conductive substrate coated with the ZnO layer can be transferred to a N2 glove box.

[0043] The process parameters of the electron transport layer 10 provided in the present application are conducive to obtaining a uniform and stable electron transport layer 10. The stable electron transport layer 10 is conducive to electron transport and inhibits electron backflow, reduces charge recombination, and thus helps to improve the overall performance of the device.

[0044] In some embodiments, the thickness of the electron transport layer 10 is 20 nm to 28 nm, and the coating speed of the ZnO precursor solution is 15 mm s -1 -18mm s -1 , further limiting the above parameters can further help improve battery efficiency.

[0045] In some embodiments, before coating the ZnO precursor solution, the surface of the ITO conductive substrate can be sequentially treated with deionized water, acetone, and isopropanol for 30 minutes by ultrasonic treatment, then cleaned with a UV cleaner for 20 minutes, and dried with a nitrogen stream for later use.

[0046] In another embodiment, the electron transport layer and the ITO conductive substrate 30 which are arranged in sequence may be purchased and used as a substrate to spin-coat the aramid nanofiber solution.

[0047] Step S102, spin coating the BTP-eC9 solution on the network layer, and annealing to form receptors in the network layer.

[0048] In some embodiments, the concentration of the BTP-eC9 solution is 9 mg / ml.

[0049] In some embodiments, the solvent in the BTP-eC9 solution is chlorobenzene, and the solvent dispersant in the BTP-eC9 solution is 1,8-diiodooctane. By volume, the chlorobenzene and 1,8-diiodooctane are used in a ratio of 3:2. The selection of the above solvents and additives is conducive to improving the dispersibility of BTP-eC9.

[0050] In another embodiment, one of chloroform and o-dichlorobenzene can be used as the solvent of the BTP-eC9 solution.

[0051] In some embodiments, the spin coating speed of the BTP-eC9 solution is 1000-4000 rpm.

[0052] In some embodiments, the annealing temperature for forming the receptor is 48° C. to 52° C., and the annealing time is 10 minutes.

[0053] Step S103, spin-coating PM6 solution on the network layer forming the acceptor, and annealing to form an active layer 20, wherein the organic photovoltaic active layer 100 includes the electron transport layer 10 and the active layer 20 arranged in sequence, and the active layer 20 forms a network layer structure loaded with acceptors and donors.

[0054] In some embodiments, the organic photovoltaic active layer 100 includes the ITO conductive substrate 30 , the electron transport layer 10 , and the active layer 20 which are sequentially arranged.

[0055] In some embodiments, the concentration of the PM6 solution is 9 mg / ml.

[0056] In some embodiments, the solvent of the PM6 solution is chlorobenzene.

[0057] In another embodiment, at least one of chloroform and dichlorobenzene can be used as the solvent of the PM6 solution.

[0058] In some embodiments, the spin coating speed of the PM6 solution is 1000-4000 rpm.

[0059] In some embodiments, the annealing temperature for forming the organic photovoltaic active layer 100 is 48° C. to 52° C., and the annealing time is 10 minutes.

[0060] In the present application, after the electron transport layer 10 is spin-coated with an aramid nanofiber solution to form a network layer, a BTP-eC9 solution and a PM6 solution are sequentially spin-coated on the network layer and annealed sequentially, thereby forming an active layer 20 of a fiber network loaded with donors and acceptors. The additionally introduced aramid nanofiber network can inhibit the serious aggregation of donors / acceptors and the increase in the scale of phase separation after the active layer 20 is heated.

[0061] Reference Figure 3 Another embodiment of the present application further provides a solar device 200, which includes a hole transport layer 40 and an electrode layer 50 stacked in sequence, and further includes an organic photovoltaic active layer 100 obtained by the method for preparing an organic photovoltaic active layer. The hole transport layer 40 covers the active layer 20.

[0062] In some embodiments, the organic photovoltaic active layer 100 can be placed in a vapor deposition chamber and then -5 The hole transport layer is evaporated under a vacuum degree of 10 Pa. Then, the organic photovoltaic active layer 100 with the hole transport layer 40 evaporated is put into the evaporation chamber again, and then -5 The electrode layer is evaporated under a vacuum degree of Pa, thereby obtaining the solar device 200.

[0063] In some embodiments, the hole transport layer 40 is a MoO3 layer, the electrode layer 50 is an Ag layer, the hole transport layer 40 has a thickness of 3-6 nm, and the electrode layer 50 has a thickness of 90-115 nm. The material selection and thickness selection of the above layers can further help improve the cell efficiency of the solar device 200.

[0064] In the present application, the solar device 200 introduces an organic photovoltaic active layer 100 that forms a network-loaded donor and acceptor. After the active layer 20 is heated, the movement of the donor / acceptor is inhibited, thereby helping to reduce the negative impact on the physical processes of exciton dissociation, carrier transport and collection of the solar device 200, thereby helping to improve the battery efficiency of the solar device 200.

[0065] By combining the organic photovoltaic active layer 100 with the hole transport layer 40 and the electrode layer 50 of specific materials and specific thicknesses, the cell efficiency of the solar device 200 may be as high as 18.5% or more.

[0066] In some embodiments, when the thickness of the hole transport layer 40 is 3-5 nm and the thickness of the electrode layer 50 is 100-110 nm, further limiting the thickness can further help improve the battery efficiency of the solar device 200, so that the battery efficiency of the solar device 200 may be as high as 19.3% or above.

[0067] Specific:

[0068] Embodiment 1:

[0069] The surface of the ITO conductive substrate 30 is treated with deionized water, acetone, and isopropanol ultrasonically for 30 minutes in sequence, then cleaned with an ultraviolet light cleaner for 20 minutes, and dried with a nitrogen flow for later use.

[0070] The ZnO precursor solution was coated on one side of the ITO conductive substrate 30 by a doctor blade coating method at a coating speed of 15 mm s -1 The coating temperature is 43° C., and the distance between the scraper and the ITO conductive substrate 30 is 18 μm.

[0071] Annealing is performed so that the ZnO precursor solution forms an electron transport layer 10, wherein the electron transport layer 10 is a ZnO layer, the annealing temperature is 60° C., and the annealing time is 15 minutes. After annealing, the ITO conductive substrate 30 coated with the ZnO layer can be transferred to an N2 glove box. The thickness of the electron transport layer 10 is 20 nm.

[0072] A aramid nanofiber solution is spin-coated on the electron transport layer 10 to form a network layer. The aramid nanofiber can be dissolved in a dimethyl sulfoxide solvent and stirred for 24 hours to form an aramid nanofiber solution. The mixing ratio of the aramid nanofiber and the dimethyl sulfoxide solvent is 1:1 by mass. The aramid nanofiber is purchased from Jiangsu Runfeng Synthetic Technology Co., Ltd., and the corresponding CAS number is 308069-56-9. The dimethyl sulfoxide solvent is purchased from Changzhou Puhua Chemical Technology Co., Ltd., and the corresponding CAS number is 67-68-5. The spin coating speed of the aramid nanofiber solution is 2000-2500 rpm.

[0073] Spin-coat the BTP-eC9 solution on the network layer and anneal to form receptors on the network layer. The concentration of the BTP-eC9 solution is 9 mg / ml, the solvent in the BTP-eC9 solution is chlorobenzene, the solvent dispersant in the BTP-eC9 solution is 1,8-diiodooctane, and the volume ratio of the chlorobenzene to the 1,8-diiodooctane is 3:2. The spin-coating speed of the BTP-eC9 solution is 2000-2500 rpm. In this step, the annealing temperature is 50°C. BTP-eC9 is purchased from Henan Weitixi Chemical Technology Co., Ltd., and the corresponding CAS number is 2598965-39-8, chlorobenzene is purchased from Nanjing Chemical Reagent Co., Ltd., and the corresponding CAS number is 108-90-7, and 1,8-diiodooctane is purchased from Hubei Jusheng Technology Co., Ltd., and the corresponding CAS number is 24772-63-2.

[0074] The PM6 solution is spin-coated on the network layer forming the receptor, and annealed to form the active layer 20. The organic photovoltaic active layer 100 includes the ITO conductive substrate 30, the electron transport layer 10 and the active layer 20 arranged in sequence. The concentration of the PM6 solution is 9 mg / ml, and the solvent of the PM6 solution is chlorobenzene. The spin coating speed of the PM6 solution is 1300-1800 rpm. In this step, the annealing temperature is 50°C. PM6 is purchased from Henan Weitixi Chemical Technology Co., Ltd., and the corresponding CAS number is 1802013-83-7.

[0075] The organic photovoltaic active layer 100 is placed in a vapor deposition chamber, and then -5 The hole transport layer 40 is evaporated under a vacuum degree of 10 Pa, and the hole transport layer 40 is a MoO3 layer. Then, the organic photovoltaic active layer 100 with the hole transport layer 40 evaporated is put into the evaporation chamber again, and then -5The electrode layer 50 is evaporated under a vacuum degree of Pa, and the electrode layer 50 is an Ag layer, thereby obtaining a solar device 200. In this embodiment, the thickness of the hole transport layer 40 is 3nm, and the thickness of the electrode layer 50 is 105nm. That is, the solar device 200 of this embodiment includes the hole transport layer 40 and the electrode layer 50 stacked in sequence, and also includes an organic photovoltaic active layer 100. The hole transport layer 40 covers the active layer 20.

[0076] Embodiment 2:

[0077] The difference between this embodiment and embodiment 1 is that the ultrasonic treatment time of the ITO conductive substrate 30 is 25 minutes, and the coating speed of the ZnO precursor solution is 13 mm s -1 The coating temperature is 45° C., the distance between the scraper and the ITO conductive substrate 30 is 20 μm, and the thickness of the electron transport layer 10 is 25 nm. The electron transport layer 10 is formed, the annealing temperature is 42-50° C., and the annealing time is 10 minutes.

[0078] The spin coating speed of the aramid nanofiber solution is 1300-1800 rpm. The spin coating speed of the BTP-eC9 solution is 1300-1800 rpm.

[0079] The thickness of the hole transport layer 40 is 6 nm, and the thickness of the electrode layer 50 is 97 nm.

[0080] Embodiment 3:

[0081] The difference between this embodiment and embodiment 1 is that the cleaning time of the ITO conductive substrate 30 by the UV cleaning machine is 15 minutes, the coating temperature is 55°C, the distance between the scraper and the ITO conductive substrate 30 is 25 μm, and the thickness of the electron transport layer 10 is 25 nm. The annealing temperature for forming the electron transport layer 10 is 42-50°C.

[0082] The spin coating speed of the aramid nanofiber solution is 1700-2000 rpm. The spin coating speed of the BTP-eC9 solution is 1700-2000 rpm.

[0083] The spin coating speed of the PM6 solution is 1200-1700 rpm.

[0084] The thickness of the hole transport layer 40 is 5 nm, and the thickness of the electrode layer 50 is 100 nm.

[0085] Embodiment 4:

[0086] The difference between this embodiment and embodiment 1 is that the ultrasonic treatment time of the ITO conductive substrate 30 is 20 minutes, the UV cleaning time is 10 minutes, and the coating speed of the ZnO precursor solution is 10 mms-1 The coating temperature is 50° C., the distance between the scraper and the ITO conductive substrate 30 is 20 μm, the annealing temperature for forming the electron transport layer 10 is 42-50° C., and the annealing time is 10 minutes.

[0087] The spin coating speed of the aramid nanofiber solution is 2500-3000 rpm. The spin coating speed of the BTP-eC9 solution is 2500-3000 rpm.

[0088] The spin coating speed of the PM6 solution is 3000-3500 rpm.

[0089] The thickness of the electrode layer 50 is 90 nm.

[0090] Embodiment 5:

[0091] The difference between this embodiment and embodiment 1 is that the ultrasonic treatment time of the ITO conductive substrate 30 is 25 minutes, the UV cleaning time is 15 minutes, and the coating speed of the ZnO precursor solution is 13 mm / s. -1 The coating temperature is 53° C., the distance between the scraper and the ITO conductive substrate 30 is 23 μm, the thickness of the electron transport layer is 23 nm, the annealing temperature for forming the electron transport layer 10 is 42-50° C., and the annealing time is 13 minutes.

[0092] The spin coating speed of the aramid nanofiber solution is 3000-3500 rpm. The spin coating speed of the BTP-eC9 solution is 3000-3500 rpm. The spin coating speed of the PM6 solution is 3500-4000 rpm.

[0093] The thickness of the hole transport layer 40 is 4 nm, and the thickness of the electrode layer 50 is 95 nm.

[0094] Embodiment 6:

[0095] The difference between this embodiment and embodiment 1 is that the ultrasonic treatment time of the ITO conductive substrate 30 is 35 minutes, and the coating speed of the ZnO precursor solution is 18 mm s -1 The coating temperature is 58° C., the distance between the scraper and the ITO conductive substrate 30 is 28 μm, the thickness of the electron transport layer 10 is 28 nm, the annealing temperature for forming the electron transport layer 10 is 42-45° C., and the annealing time is 17 minutes.

[0096] The spin coating speed of the aramid nanofiber solution is 3000-3500 rpm. The spin coating speed of the BTP-eC9 solution is 3000-3500 rpm. The spin coating speed of the PM6 solution is 1300-1500 rpm.

[0097] The thickness of the hole transport layer 40 is 4 nm, and the thickness of the electrode layer 50 is 110 nm.

[0098] Embodiment 7:

[0099] The difference between this embodiment and embodiment 1 is that the ultrasonic treatment time of the ITO conductive substrate 30 is 35 minutes, the cleaning time of the UV cleaning machine is 15 minutes, and the coating speed of the ZnO precursor solution is 20 mms -1 The coating temperature is 60° C., the distance between the scraper and the ITO conductive substrate 30 is 30 μm, the thickness of the electron transport layer 10 is 30 nm, the annealing temperature for forming the electron transport layer 10 is 45-50° C., and the annealing time is 20 minutes.

[0100] The spin coating speed of the PM6 solution is 1000-1300 rpm.

[0101] The thickness of the hole transport layer 40 is 5 nm, and the thickness of the electrode layer 50 is 115 nm.

[0102] The cell efficiency of the solar device 200 obtained in Examples 1-7 was tested by the following method:

[0103] Photovoltaic performance test: The short-circuit current density-voltage curve is tested by Agilent B2912A precision source meter measurement unit. With a solar simulator, the light power is 100 mW / cm2. Single crystal silicon (SRC-2020-KG1-RTD) is used as the standard cell. Each device has an area of ​​0.05 cm2, and the average data is calculated from at least 20 independent devices. The external quantum efficiency test (EQE) is tested by the solar cell spectral response measurement system QE-R3011 (Guangyan Technology). The light intensity of each wavelength is calibrated by a single crystal silicon detector.

[0104] Thermal stability test: The device thermal stability test is a test of the photovoltaic performance of the device at a certain temperature. The test conditions are generally to heat the organic photovoltaic device to 85 degrees Celsius in a glove box, test the current density-voltage curve every 10 minutes and record the open circuit voltage (VOC), short circuit current density (JSC), fill factor (FF), battery efficiency (PCE) and other parameters. The VOC, JSC, FF, PCE values ​​are used as the vertical coordinates and the test time is used as the horizontal coordinates.

[0105] The test results of battery efficiency are shown in the following table.

[0106]

[0107] The above-mentioned embodiments are only preferred embodiments of the present invention and cannot be used to limit the scope of protection of the present invention. Any non-substantial changes and substitutions made by technicians in this field on the basis of the present invention shall fall within the scope of protection required by the present invention.

Claims

1. A method for preparing an organic photovoltaic active layer, characterized in that: include: Spin-coating an aramid nanofiber solution on the electron transport layer to form a network layer; Spin-coating a BTP-eC9 solution on the network layer and annealing to form receptors on the network layer; The PM6 solution is spin-coated on the network layer forming the acceptor, and annealed to form an active layer. The organic photovoltaic active layer includes the electron transport layer and the active layer arranged in sequence.

2. The preparation method according to claim 1, characterized in that The concentration of the BTP-eC9 solution is 8-10 mg / ml, the concentration of the PM6 solution is 8-10 mg / ml, and the mixing ratio of the aramid nanofiber and the solvent of the aramid nanofiber solution is 1:1 by volume.

3. The preparation method according to claim 2, characterized in that: The spin coating speed of the aramid nanofiber solution is 1000-4000 rpm, the spin coating speed of the BTP-eC9 solution is 1000-4000 rpm, and the spin coating speed of the PM6 solution is 1000-4000 rpm.

4. The preparation method according to claim 3, characterized in that: The annealing temperature for forming the receptor is 48° C.-52° C., and the annealing time is 10 minutes. The annealing temperature for forming the organic photovoltaic active layer is 48° C.-52° C., and the annealing time is 10 minutes.

5. The preparation method according to claim 2, characterized in that: The solvent of the aramid nanofiber solution is dimethyl sulfoxide, the solvent in the BTP-eC9 solution is chlorobenzene, the solvent dispersant in the BTP-eC9 solution is 1,8-diiodooctane, the usage ratio of the chlorobenzene and the 1,8-diiodooctane is 3:2 by volume, and the solvent of the PM6 solution is chlorobenzene.

6. The preparation method according to claim 1, characterized in that: The electron transport layer is a ZnO layer, and the thickness of the electron transport layer is 20nm-30nm.

7. The preparation method according to claim 6, characterized in that: The preparation of the electron transport layer comprises: The ZnO precursor solution was coated on the ITO conductive substrate by blade coating at a speed of 10 mm s -1 -20mm s -1 , the coating temperature is 43℃-60℃, and the distance between the scraper and the ITO conductive substrate is 18μm-30μm; Annealing is performed so that the ZnO precursor solution forms the ZnO layer. The annealing temperature is 40-60° C. and the annealing time is 10-20 minutes.

8. The preparation method according to claim 6, characterized in that: The thickness of the electron transport layer is 20nm-28nm, and the coating speed of the ZnO precursor solution is 15mm s -1 -18mm s -1 .

9. A solar device comprising a hole transport layer and an electrode layer stacked in sequence, characterized in that: The solar device further comprises an organic photovoltaic active layer obtained by the method for preparing an organic photovoltaic active layer according to any one of claims 1 to 8, and the hole transport layer covers the active layer.

10. The solar device according to claim 9, characterized in that: The hole transport layer is a MoO3 layer, the electrode layer is an Ag layer, the thickness of the hole transport layer is 3-6 nm, and the thickness of the electrode layer is 90-115 nm.

Citation Information

Patent Citations

  • Preparation method of organic solar cell active layer

    CN108598265A

  • Organic solar cell optical active layer and manufacturing method and application thereof

    CN116546863A

  • Active layer of flexible organic solar cell based on polymer toughening and preparation method thereof

    CN117355154A