Photosensitive resin composition and method for producing printed wiring board
By using a combination of a carboxyl-containing resin, an α-aminoacetophenone-based photopolymerization initiator and a specific organic solvent in the photosensitive resin composition, the problem of crystallization of the component of the photosensitive resin under the hot and cold cycle is solved, and printing is realized High-performance manufacturing of wiring boards.
Patent Information
- Application Number
- CN202380031229.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-29
- Filing Date
- 2023-03-28
- Publication Date
- 2024-11-15
AI Technical Summary
The composition of the photosensitive resin composition crystallizes under the hot and cold cycles of normal temperature and low temperature environment, resulting in poor performance of the solder resist layer and unable to meet the high-density and high-precision printed wiring board manufacturing needs.
The combination of carboxyl-containing resin, α-aminoacetophenone-based photopolymerization initiator, petroleum-based solvent, carbitol acetate, and dipropylene glycol monomethyl ether is used to inhibit the crystallization of the photopolymerization initiator and maintain the resin composition. Stability and performance.
It effectively inhibits the crystallization of the resin composition under the hot and cold cycle, maintains its composition and properties, meets various characteristics of printed wiring board manufacturing, and improves the quality and stability of the finished product.
Smart Images

Figure BDA0005063935240000201
Abstract
Description
Technical Field
[0001] The present invention relates to a photosensitive resin composition, and more particularly to a photosensitive resin composition suitable for forming a solder resist layer. Furthermore, the present invention also relates to a method for producing a printed wiring board having a cured product formed using the photosensitive resin composition. Background Art
[0002] In recent years, as electronic devices have become thinner, smaller, and more functional, the need for higher density and higher precision in mounting components in printed wiring boards constituting electronic devices has increased. To meet such a need, it has become mainstream to form a solder resist layer by applying a photosensitive resin composition on a substrate and drying it to form a pattern, and then mainly curing the patterned photosensitive resin composition by heating or light irradiation, that is, using a so-called photo solder resist.
[0003] On the other hand, the photosensitive resin composition used to form the solder resist layer is usually placed in various environments from its production to actual use. In many cases, it is not only exposed to a normal temperature environment before and after room temperature, but also sometimes exposed to an environment where a normal temperature environment and a low temperature environment are repeatedly exposed.
[0004] Usually, the photosensitive resin composition is adjusted to fully maintain the storage stability in the normal temperature environment, but in the case of being exposed to the environment of the normal temperature environment and the low temperature environment for repeated exposure, the composition and properties of the photosensitive resin composition are sometimes damaged. Moreover, if the composition and properties of the photosensitive resin composition are damaged, the solder resist layer formed has the problem of not being able to exert sufficient performance. In particular, as mentioned above, in the manufacture of printed wiring boards with components mounted at high density and high precision, since it is necessary to form a delicate and reliable solder resist layer, the change of the composition and properties of such a photosensitive resin composition may become a big problem. Therefore, in the photosensitive resin composition, in most cases, not only the storage stability in the normal temperature environment is required, but also the storage stability in the environment of the normal temperature environment and the low temperature environment for repeated exposure. For such a requirement, it is proposed that, for example, a photosensitive resin composition having excellent stability even when the temperature environment changes is provided by further reacting the reaction product of a polynuclear epoxy compound having a specific structure and a monocarboxylic acid containing an unsaturated group with a polyacid anhydride (e.g., patent document 1).
[0005] However, the environment in which the photosensitive resin composition is placed varies, and different problems occur depending on the environment. Therefore, in the photosensitive resin composition, improving the storage stability according to the use environment of the photosensitive resin composition remains as an ongoing technical issue.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Publication No. 2001-278947. Summary of the invention
[0009] Problems to be solved by the invention
[0010] When the photosensitive resin composition is repeatedly exposed to a room temperature environment and a low temperature environment, some of its components crystallize, and the original composition and homogeneity of the photosensitive resin composition are destroyed. As a result, there is a problem that the formed solder resist layer cannot exhibit sufficient performance.
[0011] Therefore, an object of the present invention is to provide a photosensitive resin composition which can suppress the crystallization of components even when repeatedly exposed to a normal temperature environment and a low temperature environment and has various good properties required for manufacturing a printed wiring board. In addition, another object of the present invention is to provide a method for manufacturing a printed wiring board having a cured product formed using the photosensitive resin composition having the above-mentioned various good properties.
[0012] Means for solving problems
[0013] As a result of intensive research, the inventors have found that the above-mentioned problems can be solved by adding an α-aminoacetophenone-based photopolymerization initiator as a photopolymerization initiator and adding a petroleum-based solvent, carbitol acetates and dipropylene glycol monomethyl ether as an organic solvent to a photosensitive resin composition containing a carboxyl group-containing resin, a photopolymerization initiator and an organic solvent. The present invention is based on this finding. That is, the gist of the present invention is as follows.
[0014] [1] A photosensitive resin composition, characterized in that:
[0015] The photosensitive resin composition is a photosensitive resin composition comprising a carboxyl resin, a photopolymerization initiator and an organic solvent.
[0016] The photopolymerization initiator contains an α-aminoacetophenone-based photopolymerization initiator.
[0017] The organic solvent contains petroleum-based solvents, carbitol acetates and dipropylene glycol monomethyl ether.
[0018] [2] The photosensitive resin composition according to [1], wherein the mass ratio of the petroleum solvent to the carbitol acetate in the organic solvent is 1:0.5 to 1:1.
[0019] [3] The photosensitive resin composition according to [1], wherein the mass ratio of the petroleum solvent to dipropylene glycol monomethyl ether in the organic solvent is 1:0.7 to 1:1.2.
[0020] [4] The photosensitive resin composition according to [1], wherein the total content of the petroleum solvent, carbitol acetate and dipropylene glycol monomethyl ether is 50 to 90 parts by mass based on 100 parts by mass of the carboxyl group-containing resin.
[0021] [5] The photosensitive resin composition according to [1], wherein the α-aminoacetophenone-based photopolymerization initiator comprises 2-dimethylamino-2-(4-methylbenzyl)-1-(4-morpholin-4-yl-phenyl)-butan-1-one.
[0022] [6] The photosensitive resin composition according to [1], wherein the photosensitive resin composition is used to form a solder resist layer.
[0023] [7] A method for producing a printed wiring board including a solder resist layer, the method comprising: forming the solder resist layer by curing the photosensitive resin composition according to [1].
[0024] Effects of the Invention
[0025] According to the present invention, a photosensitive resin composition can be provided, which can suppress the crystallization of components even when repeatedly exposed to a normal temperature environment and a low temperature environment, and has various good properties required when manufacturing a printed wiring board. Furthermore, according to the present invention, a method for manufacturing a printed wiring board having a cured product formed using the photosensitive resin composition having the above-mentioned various good properties can be provided. DETAILED DESCRIPTION
[0026] [Photosensitive resin composition]
[0027] The photosensitive resin composition of the present invention is characterized in that it contains a carboxyl-containing resin, a photopolymerization initiator and an organic solvent as essential components, the photopolymerization initiator contains an α-aminoacetophenone-based photopolymerization initiator, and the organic solvent contains a petroleum-based solvent, carbitol acetate and dipropylene glycol monomethyl ether. The photosensitive resin composition of the present invention is formulated by combining a specific photopolymerization initiator with a specific organic solvent, so that even if the photosensitive resin composition is repeatedly exposed to a normal temperature environment and a low temperature environment (hereinafter also referred to as (hot and cold cycle)), the crystallization of components such as the photopolymerization initiator can be suppressed. That is, by formulating an α-aminoacetophenone-based photopolymerization initiator as a photopolymerization initiator in the photosensitive resin composition, and further formulating at least three of a petroleum-based solvent, carbitol acetate and dipropylene glycol monomethyl ether as an organic solvent, the excellent effect as described above is exerted. As a result, the photosensitive resin composition of the present invention can maintain its composition and properties even after being used in a hot and cold cycle, and has various good properties required when manufacturing a printed wiring board. In addition, the generation of crystals in the photosensitive resin composition may cause pinholes, shrinkage (cissing), clogging of the printing plate, etc. during printing, and further cause unevenness on the surface of the cured product (solder resist layer), and thus, as a result, the yield of the photosensitive resin composition itself, the cured product obtained using the same, and the printed wiring board having the cured product may decrease. Therefore, it can be said that the photosensitive resin composition of the present invention can solve these problems by inhibiting crystallization after the above-mentioned cold and hot cycles.
[0028] Hereinafter, each component of the photosensitive resin composition of the present invention will be described in detail.
[0029] (Carboxyl resin)
[0030] In the photosensitive resin composition of the present invention, various resins known in the past having a carboxyl group in the molecule can be used as carboxyl-containing resins. By making the photosensitive resin composition contain a carboxyl-containing resin, alkali developability can be given to the photosensitive resin composition. In particular, from the viewpoint of photocurability and development resistance, a carboxyl-containing resin having an ethylenically unsaturated double bond in the molecule is preferred. The ethylenically unsaturated double bond in the molecule is preferably a double bond from acrylic acid or methacrylic acid or their derivatives. The carboxyl-containing resin can be used alone or in combination of two or more. It should be noted that, in the case of using only a carboxyl-containing resin without an ethylenically unsaturated double bond as a carboxyl-containing resin, a compound having a plurality of ethylenically unsaturated groups in the molecule as described later, i.e., a photopolymerizable monomer, is used to make the photosensitive resin composition photocurable. As specific examples of carboxyl-containing resins, the following compounds (which can be any one of oligomers and polymers) can be cited. In the present specification, “(meth)acrylate” is a term that collectively refers to acrylate, methacrylate, and a mixture thereof. The same applies to other similar expressions such as “(meth)acrylic acid” and “(meth)acryloyl”.
[0031] (1) Carboxyl group-containing resins obtained by copolymerization of an unsaturated carboxylic acid such as (meth)acrylic acid and a compound containing an unsaturated group such as styrene, α-methylstyrene, a lower alkyl (meth)acrylate, or isobutylene.
[0032] (2) Carboxyl-containing urethane resins produced by the addition polymerization of diisocyanates such as aliphatic diisocyanates, branched aliphatic diisocyanates, alicyclic diisocyanates, and aromatic diisocyanates with diol compounds containing carboxyl groups such as dimethylol propionic acid and dimethylol butyric acid, and dihydroxy compounds such as polycarbonate polyols, polyether polyols, polyester polyols, polyolefin polyols, acrylic polyols, bisphenol A-based alkylene oxide adduct diols, and compounds having phenolic hydroxyl groups and alcoholic hydroxyl groups.
[0033] (3) Carboxyl-containing photosensitive urethane resins produced by the addition polymerization of diisocyanates with difunctional epoxy resins such as bisphenol A epoxy resin, hydrogenated bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, biphenyl epoxy resin, and monocarboxylic acid compounds having ethylenically unsaturated double bonds such as (meth)acrylic acid, carboxyl-containing diol compounds, and dihydroxy compounds.
[0034] (4) In the synthesis of the resin of (2) or (3) above, a compound having one hydroxyl group and one or more (meth)acryloyl groups in the molecule such as hydroxyalkyl (meth)acrylate is added to obtain a carboxyl-containing photosensitive urethane resin that is terminally (meth)acryloylated.
[0035] (5) In the synthesis of the resin of (2) or (3) above, a compound having one isocyanate group and one or more (meth)acryloyl groups in the molecule, such as equimolar reactants of isophorone diisocyanate and pentaerythritol triacrylate, is added to produce a carboxyl-containing photosensitive urethane resin that is terminally (meth)acryloylated.
[0036] (6) A carboxyl group-containing photosensitive resin obtained by reacting a bifunctional or higher polyfunctional (solid) epoxy resin with (meth)acrylic acid to add a dibasic acid anhydride to a hydroxyl group present in a side chain.
[0037] (7) A carboxyl group-containing photosensitive resin obtained by reacting a polyfunctional epoxy resin obtained by epoxidizing the hydroxyl groups of a bifunctional (solid) epoxy resin with epichlorohydrin with (meth)acrylic acid, and adding a dibasic acid anhydride to the generated hydroxyl groups.
[0038] (8) A carboxyl-containing polyester resin obtained by reacting a bifunctional oxetane resin with a dicarboxylic acid such as adipic acid, phthalic acid, or hexahydrophthalic acid, and adding a dibasic acid anhydride such as phthalic anhydride, tetrahydrophthalic anhydride, or hexahydrophthalic anhydride to the generated primary hydroxyl group.
[0039] (9) A carboxyl-containing photosensitive resin is obtained by reacting an epoxy compound having a plurality of epoxy groups in one molecule with a compound having at least one alcoholic hydroxyl group and one phenolic hydroxyl group in one molecule such as p-hydroxyphenylethanol and a monocarboxylic acid containing an unsaturated group such as (meth)acrylic acid, so that the alcoholic hydroxyl group of the reaction product reacts with a polyacid anhydride such as maleic anhydride, tetrahydrophthalic anhydride, trimellitic anhydride, pyromellitic anhydride, adipic acid, etc.
[0040] (10) A carboxyl group-containing photosensitive resin obtained by reacting a compound having a plurality of phenolic hydroxyl groups in one molecule with an alkylene oxide such as ethylene oxide or propylene oxide to obtain a reaction product with an unsaturated group-containing monocarboxylic acid, and then reacting the reaction product with a polybasic acid anhydride.
[0041] (11) A carboxyl group-containing photosensitive resin obtained by reacting a compound having a plurality of phenolic hydroxyl groups in one molecule with a cyclic carbonate compound such as ethylene carbonate or propylene carbonate, the resulting reaction product with an unsaturated group-containing monocarboxylic acid, and reacting the resulting reaction product with a polyacid anhydride.
[0042] (12) A carboxyl-containing photosensitive resin obtained by further adding a compound having one epoxy group and one or more (meth)acryloyl groups in one molecule to the resins of (1) to (11) above.
[0043] The acid value of the carboxyl-containing resin is preferably 30 to 150 mgKOH / g, more preferably 50 to 120 mgKOH / g. By making the acid value of the carboxyl-containing resin 30 mgKOH / g or more, the alkali developability of the photosensitive resin composition becomes good. In addition, by making the acid value 150 mgKOH / g or less, a good resist pattern can be easily drawn.
[0044] The weight average molecular weight of the carboxyl group-containing resin varies depending on the resin skeleton, and is generally preferably 2000 to 150000, and more preferably 5000 to 100000. By making the weight average molecular weight 2000 or more, the surface drying performance and resolution can be improved. In addition, by making the weight average molecular weight 150000 or less, the developability and storage stability of the photosensitive resin composition can be improved.
[0045] The content of the carboxyl resin in the photosensitive resin composition is preferably 10 to 40% by mass, more preferably 20 to 35% by mass, based on solid content. By making the content of the carboxyl resin more than 10% by mass, the coating film strength can be improved. In addition, by making the content of the carboxyl resin less than 40% by mass, the viscosity of the photosensitive resin composition becomes appropriate and the processability is improved.
[0046] (Photopolymerizable monomer)
[0047] In the photosensitive resin composition of the present invention, a photopolymerizable monomer can be added as needed. A photopolymerizable monomer is a monomer having an ethylenically unsaturated double bond. As such a photopolymerizable monomer, for example, conventionally known polyester (meth) acrylates, polyether (meth) acrylates, urethane (meth) acrylates, carbonate (meth) acrylates, epoxy (meth) acrylates, etc. can be cited. Specifically, alkyl acrylates such as 2-ethylhexyl acrylate and cyclohexyl acrylate; hydroxyalkyl acrylates such as 2-hydroxyethyl acrylate and 2-hydroxypropyl acrylate; monoacrylates or diacrylates of alkylene oxide derivatives such as ethylene glycol, propylene glycol, diethylene glycol, and dipropylene glycol; acrylamides such as N,N-dimethylacrylamide, N-hydroxymethylacrylamide, and N,N-dimethylaminopropylacrylamide; aminoalkyl acrylates such as N,N-dimethylaminoethyl acrylate and N,N-dimethylaminopropyl acrylate; polyols such as hexanediol, trimethylolpropane, pentaerythritol, di(trimethylol)propane, dipentaerythritol, and trihydroxyethyl isocyanurate; Polyacrylates such as alkylene oxide adducts or ε-caprolactone adducts of some; polyacrylates such as phenols such as phenoxy acrylate and bisphenol A diacrylate or alkylene oxide adducts of these; acrylates of glycidyl ethers such as glycerol diglycidyl ether, trimethylolpropane triglycidyl ether, and triglycidyl isocyanurate; not limited to the above, it can be appropriately selected from acrylates obtained by directly acrylated polyols such as polyether polyols, polycarbonate diols, hydroxyl-terminated polybutadiene, and polyester polyols, or urethane acrylated via diisocyanates, and melamine acrylates, and at least any one of the methacrylates corresponding to the above acrylates. Such photopolymerizable monomers can also be used as reactive diluents. Photopolymerizable monomers can be used alone or in combination of two or more.
[0048] The content of the photopolymerizable monomer in the photosensitive resin composition is preferably 10 to 100 parts by mass relative to 100 parts by mass of the carboxyl-containing resin. By making the content of the photopolymerizable monomer 10 parts by mass or more, the photocurability of the photosensitive resin composition becomes good, and it is easy to form a pattern in the alkali development after irradiation with active energy rays. On the other hand, by making the content of the photopolymerizable monomer 100 parts by mass or less, it is difficult to produce halation, and good resolution can be obtained.
[0049] When a non-photosensitive carboxyl-containing resin having no ethylenically unsaturated double bond is used as the carboxyl-containing resin, the photopolymerizable monomer is required to be used together to make the photosensitive resin composition photocurable, which is effective.
[0050] (Photopolymerization Initiator)
[0051] In the photosensitive resin composition of the present invention, the photopolymerization initiator includes an α-aminoacetophenone-based photopolymerization initiator. As the α-aminoacetophenone-based photopolymerization initiator, any known one can be used. As specific examples of the α-aminoacetophenone-based photopolymerization initiator, for example, 2-dimethylamino-2-(4-methylbenzyl)-1-(4-morpholin-4-yl-phenyl)-butane-1-one, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholin-1-propanone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butane-1-one, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholino)phenyl]-1-butanone, N,N-dimethylaminoacetophenone, etc. The α-aminoacetophenone-based photopolymerization initiator can be used alone or in combination of two or more.
[0052] The photosensitive resin composition contains an α-aminoacetophenone-based photopolymerization initiator having a structure in which a strong electron-donating group such as an alkylthio group or a dialkylamino group is substituted at the para-position of the benzoyl group as a photopolymerization initiator, thereby obtaining high curability.
[0053] The photosensitive resin composition may further include a photopolymerization initiator (hereinafter, also referred to as "other photopolymerization initiators") in addition to the above-mentioned α-aminoacetophenone-based photopolymerization initiator. As other photopolymerization initiators, hydroxyacetophenone-based photopolymerization initiators, acylphosphine oxide-based photopolymerization initiators, benzoin alkyl ether-based photopolymerization initiators, benzophenone-based photopolymerization initiators, acetophenone-based photopolymerization initiators, thioxanthone-based photopolymerization initiators, anthraquinone-based photopolymerization initiators, ketal-based photopolymerization initiators, benzoate-based photopolymerization initiators, oxime ester-based photopolymerization initiators, and titanocene-based photopolymerization initiators may be cited. Other photopolymerization initiators may be used alone or in combination of two or more.
[0054] It is preferred that the photopolymerization initiator only contains an α-aminoacetophenone-based photopolymerization initiator. In addition, it is preferred to use 2-dimethylamino-2-(4-methyl-benzyl)-1-(4-morpholin-4-yl-phenyl)-butan-1-one as the α-aminoacetophenone-based photopolymerization initiator. Examples of commercially available α-aminoacetophenone-based photopolymerization initiators include Omnirad (registered trademark) 907 (2-methyl-1-[4-(methoxythio)phenyl]-2-morpholinopropane-1-one), 369 (2-benzyl-2-(dimethylamino)-4′-morpholinobutyrophenone), 369E (2-benzyl-2-(dimethylamino)-4′-morpholinobutyrophenone), and 379 (2-dimethylamino-2-(4-methyl-benzyl)-1-(4-morpholin-4-yl-phenyl)-butan-1-one) manufactured by IGM Resins BV.
[0055] The content of the photopolymerization initiator in the photosensitive resin composition is preferably 1 to 20 parts by mass, more preferably 5 to 15 parts by mass, relative to 100 parts by mass of the carboxyl group-containing resin, as the content of the α-aminoacetophenone-based photopolymerization initiator, in terms of solid content conversion. When the photopolymerization initiator contains the above-mentioned other photopolymerization initiator and the other photopolymerization initiator is a photopolymerization initiator other than the oxime ester-based photopolymerization initiator, the content of the other photopolymerization initiator in the photosensitive resin composition is preferably 1 to 20 parts by mass, more preferably 5 to 15 parts by mass, relative to 100 parts by mass of the carboxyl group-containing resin. In addition, when the photopolymerization initiator contains the above-mentioned other photopolymerization initiator and the other photopolymerization initiator is an oxime ester-based photopolymerization initiator, the content of the oxime ester-based photopolymerization initiator in the photosensitive resin composition is preferably 0.01 to 5 parts by mass, more preferably 0.1 to 5 parts by mass, relative to 100 parts by mass of the carboxyl group-containing resin, in terms of solid content conversion. By making the contents of the α-aminoacetophenone-based photopolymerization initiator and other photopolymerization initiators within the above ranges, the photocurability of the photosensitive resin composition becomes good, the coating properties such as peeling resistance, heat resistance, and chemical resistance also become good, and the effect of reducing outgassing can be obtained, and the light absorption of the surface of the solder resist coating becomes good, and the deep curability is unlikely to decrease. Furthermore, since the content of each photopolymerization initiator is within the above range, the photopolymerization initiator is fully dissolved in the organic solvent, and the crystallization of the photopolymerization initiator can be suppressed even under the cold and hot cycle. As a result, even when the photosensitive resin composition of the present invention is used in the cold and hot cycle, its composition or properties can be maintained, and it has various good properties required when manufacturing a printed wiring board.
[0056] In the photosensitive resin composition of the present invention, a photoinitiator auxiliary agent or a sensitizer may also be used in combination with the above-mentioned photopolymerization initiator. Examples of the photoinitiator auxiliary agent or sensitizer include benzoin compounds, acetophenone compounds, anthraquinone compounds, thioxanthone compounds, ketal compounds, benzophenone compounds, tertiary amine compounds, and xanthone compounds. From the viewpoint of the deep curing property of the cured product of the photosensitive resin composition, it is preferred to use thioxanthone compounds and tertiary amine compounds as the photoinitiator auxiliary agent or sensitizer, and it is more preferred to use thioxanthone compounds. The above-mentioned photoinitiator auxiliary agent and sensitizer may be used alone or in combination of two or more.
[0057] (Thermosetting component)
[0058] In the photosensitive resin composition of the present invention, a thermosetting component can be added as needed. As the thermosetting component used in the present invention, known and commonly used substances such as isocyanate compounds, blocked isocyanate compounds, amino resins, maleimide compounds, benzoxazine resins, carbodiimide resins, cyclocarbonate compounds, epoxy compounds, oxetane compounds, and episulfide resins can be cited. The thermosetting component can be used alone or in combination of two or more. Among them, the preferred thermosetting component is epoxy resin.
[0059] Examples of the epoxy resin include bisphenol A type epoxy resin, bisphenol F type epoxy resin, hydrogenated bisphenol A type epoxy resin, brominated bisphenol A type epoxy resin, bisphenol S type epoxy resin, novolac type epoxy resin, phenol novolac type epoxy resin, cresol novolac type epoxy resin, bisphenol A novolac type epoxy resin, biphenyl type epoxy resin, naphthalene type epoxy resin, dicyclopentadiene type epoxy resin, triphenylmethane type epoxy resin, glycidylamine type epoxy resin, alicyclic epoxy resin, trihydroxyphenylmethane type epoxy resin, biphenylene type or biphenol type epoxy resin, tetrahydroxyphenylethane type epoxy resin, heterocyclic epoxy resin, diglycidyl phthalate resin, tetraglycidyl xylenoyl ethane (tetraglycidyl xylenoyl ethane) ethane) resin, glycidyl methacrylate copolymer epoxy resin, cyclohexylmaleimide and glycidyl methacrylate copolymer epoxy resin, CTBN modified epoxy resin, etc.
[0060] Examples of commercially available epoxy resins include jER (registered trademark) 828, 834, 1001, and 1004 manufactured by Mitsubishi Chemical Corporation, EPICLON (registered trademark) 840, 850, 850-S, 1050, and 2055 manufactured by DIC Corporation, Epotohto (registered trademark) YD-011, YD-013, YD-127, and YD-128 manufactured by NIPPON STEEL CHEMICAL & MATERIAL CO., LTD., DER (registered trademark) 317, 331, 661, and 664 manufactured by Dow Chemical Company, and Sumiepoxy (registered trademark) manufactured by Sumitomo Chemical Co., Ltd. Bisphenol A epoxy resins such as ESA-011, ESA-014, ELA-115, and ELA-128; jERYL903 manufactured by Mitsubishi Chemical Corporation, EPICLON 152 and 165 manufactured by DIC Corporation, and Epotohto manufactured by NIPPONSTEEL CHEMICAL & MATERIAL CO., LTD. Brominated epoxy resins such as YDB-400, YDB-500, DER542 manufactured by The Dow Chemical Company, Sumiepoxy (registered trademark) ESB-400, ESB-700 manufactured by Sumitomo Chemical Co., Ltd.; jER (registered trademark) 152, 154 manufactured by Mitsubishi Chemical Corporation, DEN (registered trademark) 431, 438 manufactured by The Dow Chemical Company, EPICLON (registered trademark) N-730, N-770, N-865 manufactured by DIC Corporation, NIPPON STEEL CHEMICAL & MATERIAL Co., Ltd. CO.,LTD.) Epotohto (registered trademark) YDCN-701, YDCN-704, Nippon Kayaku Co., Ltd. EPPN-201, EOCN-1025, EOCN-1020, EOCN-104S, RE-306, NC-3000, Sumiepoxy (registered trademark) ESCN-195X, ESCN-220, Sumitomo Chemical Co., Ltd. NIPPON STEEL CHEMICAL & MATERIAL CO., LTD.) produced by YDCN-700-2, YDCN-700-3, YDCN-700-5, YDCN-700-7, YDCN-700-10, YDCN-704, YDCN-704A, EPICLON (registered trademark) N-680, N-690, N-695 and other novolac epoxy resins produced by DIC Corporation; EPICLON (registered trademark) 830 produced by DIC Corporation, jER (registered trademark) 807 produced by Mitsubishi Chemical Corporation, bisphenol F type epoxy resins such as Epotohto (registered trademark) YDF-170, YDF-175, YDF-2004 produced by NIPPON STEEL CHEMICAL & MATERIAL CO., LTD.; NIPPON STEEL CHEMICAL & MATERIAL CO., LTD. CO., LTD.) Epotohto (registered trademark) ST-2004, ST-2007, ST-3000, YX8034 made by Mitsubishi Chemical Corporation, hydrogenated bisphenol A type epoxy resins such as; jER (registered trademark) 604 made by Mitsubishi Chemical Corporation, NIPPON STEEL CHEMICAL & MATERIAL Glycidylamine epoxy resins such as Epotohto (registered trademark) YH-434 manufactured by Sumitomo Chemical Co., Ltd. and Sumiepoxy (registered trademark) ELM-120 manufactured by Sumitomo Chemical Co., Ltd.; hydantoin epoxy resins; alicyclic epoxy resins such as CELLOXIDE (registered trademark) 2021 and EPOLEAD (registered trademark) PB3600 manufactured by Daicel Corporation; trihydroxyphenylmethane epoxy resins such as YL-933 manufactured by Mitsubishi Chemical Corporation and EPPN-501 and EPPN-502 manufactured by Nippon Kayaku Co., Ltd.; and allantoin epoxy resins such as YL-6056, YX-4000 and YL-6121 manufactured by Mitsubishi Chemical Corporation. xylenol type or biphenol type epoxy resin or a mixture thereof; bisphenol S type epoxy resins such as EBPS-200 manufactured by Nippon Kayaku Co., Ltd., EPX-30 manufactured by ADEKA Co., Ltd., and EXA-1514 manufactured by DIC Corporation; bisphenol A novolac type epoxy resins such as jER (registered trademark) 157S manufactured by Mitsubishi Chemical Corporation; tetrahydroxyphenylethane type epoxy resins such as jER (registered trademark) YL-931 manufactured by Mitsubishi Chemical Corporation; heterocyclic epoxy resins such as TEPIC (registered trademark) manufactured by Nissan Chemical Co., Ltd.; diglycidyl phthalate resins such as BLEMMER (registered trademark) DGT manufactured by NOF Corporation; NIPPON STEEL CHEMICAL & MATERIAL CO., LTD.) tetraglycidyl xylenoyl ethane resins such as ZX-1063 manufactured by NIPPON STEEL CHEMICAL & MATERIAL CO., LTD.; naphthalene-type epoxy resins such as ESN-190 and ESN-360 manufactured by NIPPON STEEL CHEMICAL & MATERIAL CO., LTD., HP-4032, EXA-4750 and EXA-4700 manufactured by DIC Corporation; dicyclopentadiene-type epoxy resins such as HP-7200 and HP-7200H manufactured by DIC Corporation; methacrylic acid glycidyl copolymer epoxy resins such as CP-50S and CP-50M manufactured by NOF Corporation; in addition, copolymer epoxy resins of cyclohexyl maleimide and methacrylic acid glycidyl ester; CTBN-modified epoxy resins (for example, NIPPON STEEL CHEMICAL & MATERIAL CO., LTD.) CO., LTD.) and other products.
[0061] The content of the thermosetting component in the photosensitive resin composition is preferably 0.3 to 3.0 mol, more preferably 0.5 to 2.5 mol, of the number of functional groups of the thermosetting component that reacts per 1 mol of the carboxyl group contained in the carboxyl group-containing resin.
[0062] In particular, when an epoxy resin is used as a thermosetting component, the equivalent of the epoxy group of the epoxy resin in the photosensitive resin composition is preferably 0.3 to 3.0 in terms of solid content relative to 1 equivalent of the carboxyl group of the carboxyl-containing resin. By making the epoxy group of the epoxy resin 0.3 equivalent or more, it is possible to prevent the carboxyl group from remaining in the cured film, thereby obtaining good heat resistance, alkali resistance, electrical insulation, etc. On the other hand, by making the epoxy group of the epoxy resin 3.0 equivalent or less, it is possible to prevent low molecular weight cyclic (sulfide) ether groups from remaining in the dried coating, thereby ensuring good strength of the cured film, etc.
[0063] (Thermal Curing Catalyst)
[0064] The photosensitive resin composition of the present invention may be mixed with a thermosetting catalyst as required. Examples of the thermosetting catalyst used in the present invention include imidazole derivatives such as imidazole, 2-methylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 4-phenylimidazole, 1-cyanoethyl-2-phenylimidazole, and 1-(2-cyanoethyl)-2-ethyl-4-methylimidazole; amine compounds such as dicyandiamide, benzyldimethylamine, 4-(dimethylamino)-N,N-dimethylbenzylamine, 4-methoxy-N,N-dimethylbenzylamine, and 4-methyl-N,N-dimethylbenzylamine; hydrazine compounds such as adipic acid dihydrazide and sebacic acid dihydrazide; and phosphorus compounds such as triphenylphosphine. Commercially available products of the heat curing catalyst include, for example, 2MZ-A, 2MZ-OK, 2PHZ, 2P4BHZ, 2P4MHZ (all trade names of imidazole compounds) manufactured by Shikoku Chemical Industry Co., Ltd., U-CAT 3513N (trade name of dimethylamine compounds) manufactured by San-Apro Ltd., DBU, DBN, U-CAT SA (registered trademark) 102 (all bicyclic amidine compounds and salts thereof), etc. The heat curing catalyst is not limited to these, and any heat curing catalyst for epoxy resins or oxetane compounds, or a compound that promotes the reaction of at least one of an epoxy group and an oxetane group with a carboxyl group may be used. In addition, guanamine, acetoguanamine, benzoguanamine, melamine, 2,4-diamino-6-methacryloyloxyethyl-S-triazine, 2-vinyl-2,4-diamino-S-triazine, 2-vinyl-4,6-diamino-S-triazine / isocyanuric acid adduct, 2,4-diamino-6-methacryloyloxyethyl-S-triazine / isocyanuric acid adduct and other S-triazine derivatives can also be used, and it is preferred to use these compounds that also function as adhesion-imparting agents in combination with a thermosetting catalyst. The thermosetting catalyst may be used alone or in combination of two or more.
[0065] The content of the thermosetting catalyst in the photosensitive resin composition is preferably 0.1 to 20 parts by mass, more preferably 0.5 to 15 parts by mass, relative to 100 parts by mass of the carboxyl-containing resin. By making the content of the thermosetting catalyst 0.1 parts by mass or more, the heat resistance of the cured product of the photosensitive resin composition is excellent. On the other hand, by making the content of the thermosetting catalyst 20 parts by mass or less, the storage stability of the photosensitive resin composition is improved.
[0066] (Organic Solvent)
[0067] The photosensitive resin composition of the present invention contains petroleum solvents, carbitol acetates and dipropylene glycol monomethyl ether as organic solvents. Petroleum solvents, carbitol acetates and dipropylene glycol monomethyl ether can be used alone or in combination of two or more. By using these three organic solvents in combination, the components of the photosensitive resin composition can be fully dissolved even when exposed to a cold and hot cycle of an environment such as a normal temperature environment and a low temperature environment, and the crystallization and precipitation of the components can be suppressed. As a result, the composition and properties of the photosensitive resin composition can be maintained, and the photosensitive resin composition has various good properties required when manufacturing a printed wiring board. By using the above three organic solvents in combination, the crystallization of the components of the photosensitive resin composition can be suppressed. The reason why the crystallization of the components can be suppressed under the cold and hot cycle by using the above three organic solvents in combination is still uncertain, but the following inference can be made. That is, it is believed that when the three organic solvents contained in the photosensitive resin composition, namely, petroleum-based solvents, carbitol acetates, and dipropylene glycol monomethyl ether, are used, the change in solubility with respect to temperature change is small (slow), and even under the cold and hot cycle, the components of the photosensitive resin composition can be stably dissolved in these organic solvents, and therefore, the crystallization of the components under the cold and hot cycle can be suppressed. On the other hand, even if the solvent has a higher solubility in a normal temperature environment than the above three organic solvents, when the change in solubility with respect to temperature change is large (fast), the dissolved state of the components of the photosensitive resin composition under the cold and hot cycle is unstable, and therefore, as a result, the crystallization of the components under the cold and hot cycle cannot be fully suppressed.
[0068] In this specification, petroleum-based solvents specifically refer to hydrocarbon-based solvents containing aromatic hydrocarbons derived from petroleum such as petroleum ether, petroleum naphtha, hydrogenated petroleum naphtha, solvent naphtha, or mixtures thereof. The boiling point of the petroleum-based solvent is not particularly limited, and for example, 150 to 200° C. can be cited. The number of carbon atoms in the petroleum-based solvent is also not particularly limited, and for example, the number of carbon atoms can be 10 or more. In addition, aromatic hydrocarbons with a carbon number of 10 or more can also be formed by replacing one or more hydrogen atoms of aromatic compounds such as benzene, naphthalene, and anthracene with an alkyl group such as methyl, ethyl, propyl, or butyl, or an alkylene group such as ethylene, propylene, or tetramethylene.
[0069] Examples of the aromatic hydrocarbons contained in the petroleum-based solvent include benzene, naphthalene, anthracene, cumene, n-propylbenzene, 1-methyl-3-ethylbenzene, 1-methyl-4-ethylbenzene, 1,3,5-trimethylbenzene, 1-methyl-2-ethylbenzene, tert-butylbenzene, 1,2,4-trimethylbenzene, isobutylbenzene, sec-butylbenzene, 1-methyl-3-isopropylbenzene, 1,2,3-trimethylbenzene, 1-methyl-4-isopropylbenzene, indane, 1-methyl-2-isopropylbenzene, 1,3-diethylbenzene, 1-methyl-3-propylbenzene, n-butylbenzene, 1-methyl-4-propylbenzene, 1,2- diethylbenzene, 1,4-diethylbenzene, 1,3-dimethyl-5-ethylbenzene, 1-methyl-2-propylbenzene, 1,4-dimethyl-2-ethylbenzene, 2-methylindane, 1-methylindane, 1,2-dimethyl-4-ethylbenzene, 1,3-dimethyl-2-ethylbenzene, 1,2-dimethyl-3-ethylbenzene, 4-methylindane, 5-methylindane, 1,2,3,4-tetramethylbenzene, 1,3-dimethyl-4-ethylbenzene, 1,2,4,5-tetramethylbenzene, 1,2,3,5-tetramethylbenzene, tetralin, 1-methylnaphthalene, 2-methylnaphthalene, etc. The petroleum-based solvent may contain one or more of the aromatic hydrocarbons alone or in combination of two or more.
[0070] Commercially available products of petroleum-based solvents include, for example, Ipsol (registered trademark) #100 and #150 manufactured by Idemitsu Kosan Co., Ltd., T-SOL (trademark) 100 and 150 manufactured by ENEOS Co., Ltd., Cactus Solvent P-100 and P-150, SWAZOLE (trade name) (registered trademark) 310 and 1000 manufactured by Maruzen Petrochemical Co., Ltd., SOLVESSO (registered trademark) 100, 150 and 200 manufactured by ANDOH PARACHEMIE CO., LTD., and ShellSol A100, ShellSol A150 and ShellSol S manufactured by Shell Chemicals Japan K.K.
[0071] In this specification, carbitol acetate refers to the ester of acetic acid and diethylene glycol alkyl ether. As carbitol acetate, for example, the ester of acetic acid and diethylene glycol monomethyl ether, i.e., diethylene glycol monomethyl ether acetate (methyl carbitol acetate), the ester of acetic acid and diethylene glycol monoethyl ether, i.e., diethylene glycol monoethyl ether acetate (ethyl carbitol acetate), the ester of acetic acid and diethylene glycol monobutyl ether, i.e., diethylene glycol monobutyl ether acetate (butyl carbitol acetate), etc. can be cited. Carbitol acetate can be used alone or in combination of two or more. As carbitol acetate, diethylene glycol monoethyl ether acetate (ethyl carbitol acetate) is preferably used, and diethylene glycol monoethyl ether acetate (ethyl carbitol acetate) is particularly preferably used alone.
[0072] In the photosensitive resin composition of the present invention, the mass ratio of the petroleum solvent to the carbitol acetate in the organic solvent (mass of the petroleum solvent:mass of the carbitol acetate) is preferably 1:0.5 to 1:1.2, more preferably 1:0.5 to 1:1.
[0073] In the photosensitive resin composition of the present invention, the mass ratio of the petroleum solvent to dipropylene glycol monomethyl ether in the organic solvent (mass of the petroleum solvent:mass of dipropylene glycol monomethyl ether) is preferably 1:0.7 to 1:1.2.
[0074] The three organic solvents can be added separately when preparing the photosensitive resin composition of the present invention, can be added when preparing the components such as the carboxyl group-containing resin constituting the photosensitive resin composition of the present invention, or can be contained as solvents for the components. Preferably, the three organic solvents are added when preparing the photosensitive resin composition of the present invention.
[0075] In addition to the above-mentioned petroleum-based solvents, carbitol acetates and dipropylene glycol monomethyl ether, the organic solvent may also contain other solvent components. As other solvent components, ketones such as methyl ethyl ketone and cyclohexanone; glycol ethers such as cellosolve, methyl cellosolve, butyl cellosolve, propylene glycol monomethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol diethyl ether, tripropylene glycol monomethyl ether; esters such as ethyl acetate, butyl acetate, butyl lactate, cellosolve acetate, butyl cellosolve acetate, propylene glycol monomethyl ether acetate, dipropylene glycol monomethyl ether acetate, propylene carbonate; aliphatic hydrocarbons such as octane and decane, and other well-known and commonly used solvent components can be used. These other components can be used alone or in combination of two or more.
[0076] The content of the organic solvent in the photosensitive resin composition is not particularly limited as long as the effect of the present invention is exerted. The total content of the petroleum-based solvent, carbitol acetate and dipropylene glycol monomethyl ether is preferably adjusted to 50 to 90 parts by mass relative to 100 parts by mass of the carboxyl-containing resin (solid content). In addition, when the organic solvent contains the above-mentioned other solvent components, the content of the organic solvent in the photosensitive resin composition is adjusted so that the total content of the petroleum-based solvent, carbitol acetate and dipropylene glycol monomethyl ether is within the above-mentioned range, and the total content of all organic solvent components is preferably 100 to 150 parts by mass relative to 100 parts by mass of the carboxyl-containing resin.
[0077] In the present invention, the volatilization drying of the organic solvent can be carried out using a hot air circulation drying furnace, an IR furnace, a hot plate, a convection oven, etc. (a device using a heat source with a steam-based air heating method, a method of making the hot air in the dryer contact by convection, and a method of spraying to the support through a nozzle).
[0078] (filler)
[0079] The photosensitive resin composition of the present invention may contain fillers as required to improve the physical strength of the coating film. As such fillers, known inorganic or organic fillers can be used, and barium sulfate, spherical silica, hydrotalcite and talc are particularly preferred. Furthermore, in order to obtain flame retardancy, metal hydroxides such as metal oxides and aluminum hydroxide can also be used as extender pigment fillers.
[0080] The content of the filler is preferably 40% by mass or less in terms of solid content relative to the total mass of the photosensitive resin composition. When the content of the filler is greater than 40% by mass, the viscosity of the photosensitive resin composition increases, the coating and molding properties decrease, and the cured product becomes brittle. It is more preferably 5 to 40% by mass.
[0081] (Other added ingredients)
[0082] In the photosensitive resin composition of the present invention, colorants, photoinitiator aids, cyanate compounds, elastomers, mercapto compounds, urethanization catalysts, thixotropic agents, adhesion promoters, block copolymers, chain transfer agents, polymerization inhibitors, copper poison inhibitors, antioxidants, rust inhibitors, thickeners such as organic bentonite and montmorillonite, silicone-based, fluorine-based, polymer-based defoamers and leveling agents, at least one of imidazole-based, thiazole-based, triazole-based silane coupling agents, phosphonates, phosphate derivatives, phosphorus compounds such as phosphazene compounds, and other flame retardants can be further added as needed. These can use substances known in the field of electronic materials.
[0083] The photosensitive resin composition of the present invention may be used in a liquid state or may be used after being dried as described below. When used in a liquid state, it may be a single liquid or a two-liquid or more liquid state.
[0084] [Dry film]
[0085] The photosensitive resin composition of the present invention can also be set to the form of a dry film having a first film and a resin layer composed of a photosensitive resin composition formed on the first film. The first film of the present invention refers to a film that is at least bonded to the resin layer when laminated and integrally molded in a manner such as by heating with a substrate such as a substrate in contact with the layer (resin layer) side composed of a photosensitive resin composition formed on the dry film. The first film can be peeled off from the resin layer in the process after lamination. In particular, in the present invention, it is preferably peeled off from the resin layer in the process after exposure. When the dry film is formed, the photosensitive resin composition of the present invention is diluted with the above-mentioned organic solvent and adjusted to a suitable viscosity, and is applied to the first film with a uniform thickness by a comma coater, a blade coater, a lip coater, a rod coater, an extrusion coater, a reverse coater, a transfer roller coater, a gravure coater, a spray coater, etc., and is usually dried at a temperature of 50 to 130°C for 1 to 30 minutes, so that a film can be obtained. The coating film thickness is not particularly limited, but is usually appropriately selected within the range of 1 to 150 μm, preferably 10 to 60 μm, as the film thickness after drying.
[0086] As the first film, any known film can be used without particular limitation, and for example, films made of thermoplastic resins such as polyester films such as polyethylene terephthalate or polyethylene naphthalate, polyimide films, polyamide-imide films, polypropylene films, and polystyrene films can be appropriately used. Among them, polyester films are preferred from the viewpoints of heat resistance, mechanical strength, and operability. In addition, a laminate of these films can also be used as the first film.
[0087] Furthermore, from the viewpoint of improving mechanical strength, the thermoplastic resin film as described above is preferably a film stretched in a uniaxial direction or a biaxial direction.
[0088] The thickness of the first film is not particularly limited, and can be, for example, 10 μm to 150 μm.
[0089] After forming the resin layer of the photosensitive resin composition of the present invention on the first film, further, for the purpose of preventing dust from adhering to the surface of the resin layer, etc., it is preferred to laminate a second film that can be peeled off on the surface of the resin layer. The second film refers to a film that is peeled off from the resin layer before lamination when a substrate such as a substrate is laminated and integrally formed in a way that the side of the layer (resin layer) formed by the photosensitive resin composition formed on the dry film is contacted by heating, etc. As a second film that can be peeled off, for example, a polyethylene film, a polytetrafluoroethylene film, a polypropylene film, a surface-treated paper, etc. can be used. For the second film, as long as the adhesion between the resin layer and the second film is smaller than the adhesion between the resin layer and the first film when the second film is peeled off.
[0090] The thickness of the second film is not particularly limited, and can be, for example, 10 μm to 150 μm.
[0091] In addition, the dry film may be a material obtained by coating the photosensitive resin composition of the present invention on the second film and drying to form a resin layer, and laminating the first film on the surface thereof. That is, when the dry film is produced in the present invention, as the film coated with the photosensitive resin composition of the present invention, either the first film or the second film may be used.
[0092] (cured material)
[0093] The cured product of the present invention is obtained by curing the resin layer of the photosensitive resin composition or dry film of the present invention, and has good resolution required for a solder resist layer. In addition, since the photosensitive resin composition of the present invention can suppress crystallization of components even under thermal cycling and maintain its composition and properties, the formed cured product can maintain good resolution even when used after exposure to thermal cycling.
[0094] (Printed Wiring Board)
[0095] The printed wiring board of the present invention has a cured product obtained from the resin layer of the photosensitive resin composition or dry film of the present invention. As a method for manufacturing the printed wiring board of the present invention, for example, the photosensitive resin composition of the present invention is adjusted to a viscosity suitable for the coating method by using the above-mentioned organic solvent, and after coating on a substrate by a dip coating method, a flow coating method, a roll coating method, a rod coating method, a screen printing method, a curtain coating method, etc., the organic solvent contained in the composition is volatilized and dried (pre-dried) under a temperature condition of 60 to 100° C., thereby forming a surface-dried resin layer. In addition, in the case of a dry film, after being attached to a substrate in a manner that the resin layer contacts the substrate by a laminator, the first film is peeled off, thereby forming a resin layer on the substrate.
[0096] As the substrate of the printed wiring board, in addition to the printed wiring board or flexible printed wiring board in which the circuit is pre-formed with copper or the like, there can be cited copper-clad laminates of all grades (FR-4, etc.) for high-frequency circuits using materials such as paper phenolic resin, paper epoxy resin, glass cloth epoxy resin, glass polyimide, glass cloth / non-woven fabric epoxy resin, glass cloth / paper epoxy resin, synthetic fiber epoxy resin, fluororesin-polyethylene-polyphenylene ether, polyphenylene ether-cyanate ester, etc., as well as metal substrates, polyimide films, polyethylene terephthalate films, polyethylene naphthalate (PEN) films, glass substrates, ceramic substrates, chip boards, etc.
[0097] The lamination of the dry film on the substrate is preferably performed under pressure and heating conditions using a vacuum laminator or the like. By using such a vacuum laminator, when a substrate having a circuit is used, even if there are irregularities on the surface of the circuit substrate, the dry film is closely attached to the circuit substrate, so that bubbles are not mixed in, and the filling property of the recessed portion on the surface of the substrate is also improved. The pressure condition is preferably about 0.1 to 2.0 MPa, and the heating condition is preferably 40 to 120°C.
[0098] The volatilization drying after coating the photosensitive resin composition of the present invention can be carried out using a hot air circulation drying furnace, an IR oven, a hot plate, a convection oven, etc. (a method using a device with a heat source of a steam-based air heating method, a method of making hot air in the dryer convectively contact, and a method of spraying toward the support through a nozzle).
[0099] After forming a resin layer on a substrate, a photomask having a prescribed pattern is formed and selectively exposed using active energy rays, and the unexposed portion is developed using a dilute alkali aqueous solution (e.g., a 0.3-3% by mass sodium carbonate aqueous solution) to form a pattern of a cured product. In the case of a dry film, after exposure, the first film is peeled off from the dry film for development, thereby forming a patterned cured product on the substrate. It should be noted that, as long as it is within the range that does not damage the characteristics, the first film can be peeled off from the dry film before exposure and the exposed resin layer can be exposed and developed. Furthermore, the cured product is irradiated with active energy rays and then heat-cured (e.g., 100-220°C), or irradiated with active energy rays after heat-curing, or finally fine-cured (main cure) by heat-curing alone, thereby forming a cured film having excellent characteristics such as adhesion and hardness.
[0100] As an exposure machine for irradiating the above-mentioned active energy rays, any device equipped with a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a metal halide lamp, a mercury short arc lamp, etc., and irradiating ultraviolet rays in the range of 350 to 450 nm can be used. Furthermore, a direct drawing device (for example, a laser direct imaging device that directly draws an image with a laser using CAD data from a computer) can also be used. The lamp light source or laser light source of the direct drawing machine can be a light source with a maximum wavelength in the range of 350 to 450 nm. The exposure amount used to form an image varies depending on the film thickness, etc., and can usually be set to 10 to 1000 mJ / cm 2 , preferably, it can be set to 20 to 800 mJ / cm 2 within the range.
[0101] As the developing method, immersion, showering, spraying, brushing or the like can be used, and as the developing solution, an alkaline aqueous solution of potassium hydroxide, sodium hydroxide, sodium carbonate, potassium carbonate, sodium phosphate, sodium silicate, ammonia, amines or the like can be used.
[0102] When curing the photosensitive resin composition of the present invention, it is possible to irradiate ultraviolet rays after the exposure and development based on the above-mentioned active energy rays to promote further curing (post-UV), or to heat to promote thermal curing (post-curing) as needed. By performing post-UV and post-curing treatments, the various properties of the cured product of the photosensitive resin composition, such as heat resistance, chemical resistance, moisture absorption resistance, adhesion, and electrical properties, can be further improved.
[0103] Example
[0104] The present invention will be described in further detail below with reference to Examples, but the present invention is not limited to these Examples. It should be noted that in the Examples, unless otherwise specified, the descriptions of "parts" and "%" are based on mass.
[0105] [Preparation of photosensitive resin composition]
[0106] (Synthesis Example of Carboxyl Group-Containing Resin)
[0107] Before preparing the photosensitive resin composition, the carboxyl group-containing resin used in this example was prepared according to the following procedure.
[0108] First, 220 parts of cresol novolac epoxy resin (EPICLON (registered trademark) N-695, manufactured by Dainippon Ink & Chemicals Co., Ltd., epoxy equivalent 220) are placed in a four-necked flask with a stirrer and a reflux cooler, and 206 parts of 3-methoxy-3-methyl-1-butyl acetate (Solfit AC) are added to heat and dissolve. Then, 0.1 parts of a polymerization inhibitor (hydroquinone) and 2.0 parts of a reaction catalyst (triphenylphosphine) are added. The obtained mixture is heated to 95-105°C, 72 parts of acrylic acid are slowly added dropwise, and the reaction is carried out for 16 hours. The obtained reaction product is cooled to 80-90°C, 91.2 parts of tetrahydrophthalic anhydride are added, the reaction is carried out for 8 hours, and the reaction is cooled to obtain a photosensitive prepolymer having both ethylenically unsaturated bonds and carboxyl groups. The obtained photosensitive prepolymer has a non-volatile content of 65% and an acid value of 87.8 mgKOH / g in solid matter.
[0109] Then, the components shown in Table 1 below were mixed in the amounts shown in the table (solid content, the organic solvents described in the table are the amounts added when preparing the photosensitive resin composition), pre-mixed with a stirrer, and then kneaded with a three-roll mill to prepare the photosensitive resin compositions of Examples 1 to 4 and Comparative Examples 1 to 2. It should be noted that the details of the components in Table 1 are as follows.
[0110] Carboxyl-containing resin (carboxyl-containing resin obtained from the above synthesis example)
[0111] Thermosetting component 1: phenol novolac type epoxy resin (RE-306-SA9, manufactured by Nippon Kayaku Co., Ltd.).
[0112] Thermosetting component 2: alicyclic epoxy resin (EPOLEAD (registered trademark) PB3600, manufactured by Daicel Corporation).
[0113] Thermosetting component 3: biphenol type epoxy resin (YX-4000, manufactured by Mitsubishi Chemical Corporation).
[0114] Photopolymerizable monomer: dipentaerythritol hexaacrylate.
[0115] Other added components 1: defoaming agent (KS-66, manufactured by Shin-Etsu Chemical Co., Ltd.).
[0116] Other added components 2: thickener (ORBEN-MF, manufactured by Shiraishi Industries, Ltd.).
[0117] Other added ingredients 3: blue pigment.
[0118] Other added ingredients 4: yellow pigment.
[0119] Heat curing catalyst: melamine.
[0120] Filler: surface-treated barium sulfate (B-30, manufactured by Sakai Chemical Industry Co., Ltd.).
[0121] Photopolymerization initiator 1: α-aminoacetophenone-based photopolymerization initiator (Omnirad (registered trademark) 379, manufactured by IGM Resins BV).
[0122] Photopolymerization initiator 2: α-aminoacetophenone-based photopolymerization initiator (Omnirad (registered trademark) 369E, manufactured by IGM Resins BV).
[0123] Photopolymerization initiator 3: α-hydroxyacetophenone-based photopolymerization initiator (liquid photopolymerization initiator, Omnirad (registered trademark) 1173, manufactured by IGM Resins BV).
[0124] Organic solvent 1: alcohol solvent (Solfit AC, manufactured by Kuraray Co., Ltd.).
[0125] Organic solvent 2: carbitol acetate (ethyl carbitol acetate (diethylene glycol monoethyl ether acetate)).
[0126] Organic solvent 3: a petroleum-based solvent (Ipsol #150, manufactured by Idemitsu Kosan Co., Ltd.).
[0127] Organic solvent 4: dipropylene glycol monomethyl ether.
[0128] Organic solvent 5: methyl ethyl ketone.
[0129] [Table 1]
[0130]
[0131] *“-” indicates no rating.
[0132] [Evaluation of crystallization caused by thermal cycling]
[0133] The crystallization of each photosensitive resin composition of the examples and comparative examples due to the thermal cycle was evaluated according to the following procedure. 50 g of each photosensitive resin composition of the examples and comparative examples was weighed, placed at room temperature for one day, and then placed at 4°C or below for another day, which was considered as one cycle, and photosensitive resin compositions after each cycle were prepared 1 to 3 times.
[0134] The photosensitive resin composition obtained after each cycle was applied to a glass substrate using a coating glass rod with a 200 μm gap formed by wrapping tape around both ends of the glass rod, and dried at 80°C for 20 minutes to prepare a substrate for evaluating crystallization caused by thermal cycling. Each evaluation substrate was visually observed to confirm whether there was crystallization in each evaluation substrate, and the crystallization caused by thermal cycling in each photosensitive resin composition was evaluated according to the following evaluation criteria. The results are shown in Table 1.
[0135] ⊚: Crystals with a maximum diameter of 200 μm or less were not observed.
[0136] ○: One or more and two or less crystals having a maximum diameter of 200 μm or less were observed.
[0137] ×: Three or more crystals having a maximum diameter of 200 μm or less were observed.
[0138] [Evaluation of Drying Management Range]
[0139] On the surface of a polished FR-4 substrate having a length of 150 mm, a width of 95 mm and a thickness of 1.6 mm and having a circuit pattern formed thereon, each photosensitive resin composition of the embodiment and the comparative example after three cycles of hot and cold was screen-printed and applied to a film thickness of 20 μm after drying, and dried at 80° C. under three conditions of 60 minutes, 65 minutes and 70 minutes, respectively, to produce a substrate for evaluating the drying management width having a dried coating film.
[0140] For each drying management width evaluation substrate, a 1 mass % sodium carbonate aqueous solution at a liquid temperature of 30° C. was used as a developer, and development was performed for 60 seconds using a printed wiring board developer. After development, each drying management width evaluation substrate was visually observed to confirm the presence or absence of a dry coating film (development residue), and the drying management width of each photosensitive resin composition was evaluated according to the following evaluation criteria. The results are shown in Table 1.
[0141] ○: No development residue was observed in the evaluation substrates dried at 80° C. for 60 minutes, 65 minutes, and 70 minutes.
[0142] Δ: Among the drying management width evaluation substrates dried at 80° C. for 60 minutes, 65 minutes, and 70 minutes, one drying management width evaluation substrate had development residue.
[0143] ×: Development residues occurred in at least two of the drying management width evaluation substrates dried at 80° C. for 60 minutes, 65 minutes, and 70 minutes.
[0144] [Collapsibility evaluation]
[0145] On the surface of a copper-clad laminate having a length of 150 mm, a width of 95 mm and a thickness of 1.6 mm, 0.15 mL of each photosensitive resin composition after three cold and hot cycles was dripped using a syringe, and the copper-clad laminate was stood up against a bracket after being left for 1 minute. It should be noted that the copper-clad laminate was stood up against a bracket in a manner such that the angle between the surface on the opposite side of the surface to which the photosensitive resin composition was dripped and the horizontal plane was 80°. Then, the photosensitive resin composition was dried at 150°C for 30 minutes in a state of standing up against the bracket to prepare a substrate for collapse evaluation.
[0146] The slump length of the photosensitive resin composition (the length from the end on the dripping side to the end on the side where the photosensitive resin composition slumps and extends) was measured for each slump evaluation substrate, and the slump of each photosensitive resin composition was evaluated according to the following evaluation criteria. The results are shown in Table 1.
[0147] ◎: The collapsed length is within 1 cm.
[0148] ○: The collapsed length is greater than 1 cm and within 2 cm.
[0149] ×: The collapsed length is greater than 2 cm.
[0150] [Printability (off-plate) evaluation]
[0151] On the surface of a polished FR-4 substrate of 150 mm in length, 95 mm in width and 1.6 mm in thickness, each photosensitive resin composition of the embodiment and the comparative example after three hot and cold cycles was printed by screen printing in a manner that the film thickness after drying was 20 μm. The time from the moment the photosensitive resin composition was printed to the moment the photosensitive resin composition was separated from the printing plate was measured, and the printability (off-plate) of each photosensitive resin composition was evaluated according to the following evaluation criteria. The results are shown in Table 1.
[0152] ⊚: The time from the photosensitive resin composition to the separation from the printing plate after printing was within 1 second.
[0153] ◯: The time until the photosensitive resin composition and the printing plate were separated after printing was more than 1 second and within 2 seconds.
[0154] ×: The time until the photosensitive resin composition and the printing plate were separated after printing was longer than 2 seconds.
[0155] [Evaluation of dryness to touch]
[0156] On the surface of a polished copper-clad laminate having a length of 150 mm, a width of 95 mm and a thickness of 1.6 mm, each photosensitive resin composition of the embodiment and the comparative example after three hot and cold cycles was printed on the entire surface by screen printing so that the film thickness after drying was 20 μm, and dried at 80° C. for 30 minutes to prepare a substrate for evaluating the dryness to touch having a dry coating film of the photosensitive resin composition.
[0157] After pressing each substrate for evaluation of dryness to touch with a finger (index finger) for 3 seconds with such strength that the entire fingertip made contact, the contacted portion was visually observed to confirm the presence or absence of fingerprints, and dryness to touch of each photosensitive resin composition was evaluated according to the following evaluation criteria.
[0158] ○: No fingerprint remains after finger contact for 3 seconds.
[0159] △: Part of the fingerprint remains after the finger touches for 3 seconds.
[0160] From the evaluation results shown in Table 1, it can be seen that in the photosensitive resin composition of each embodiment, the crystallization caused by the cold and hot cycle is fully suppressed, and even when used after the cold and hot cycle, various good properties (drying management range, collapse and printability) required for the manufacture of printed wiring boards can be achieved. That is, it can be seen that in the photosensitive resin composition containing a carboxyl resin, a photopolymerization initiator and an organic solvent, by using an α-aminoacetophenone-based photopolymerization initiator as a photopolymerization initiator, and using a petroleum-based solvent, carbitol acetate and dipropylene glycol monomethyl ether as an organic solvent, it is possible to fully suppress the crystallization caused by the cold and hot cycle and achieve various good properties required for the manufacture of printed wiring boards. On the other hand, it can be seen that in the photosensitive resin composition of each comparative example, it is not possible to take into account both the sufficient suppression of the crystallization caused by the cold and hot cycle and the various good properties required for the manufacture of printed wiring boards.
Claims
1. A photosensitive resin composition, It is characterized in that The photosensitive resin composition is a photosensitive resin composition comprising a carboxyl resin, a photopolymerization initiator and an organic solvent. The photopolymerization initiator comprises an α-aminoacetophenone-based photopolymerization initiator, The organic solvent includes petroleum-based solvents, carbitol acetates and dipropylene glycol monomethyl ether.
2. The photosensitive resin composition according to claim 1, in, The mass ratio of the petroleum solvent to the carbitol acetate in the organic solvent is 1:0.5 to 1:1.
2.
3. The photosensitive resin composition according to claim 1, in, The mass ratio of the petroleum solvent to dipropylene glycol monomethyl ether in the organic solvent is 1:0.7 to 1:1.
2.
4. The photosensitive resin composition according to claim 1, in, The total content of the petroleum-based solvent, carbitol acetate and dipropylene glycol monomethyl ether is 50 to 90 parts by mass based on 100 parts by mass of the carboxyl group-containing resin.
5. The photosensitive resin composition according to claim 1, in, The α-aminoacetophenone-based photopolymerization initiator includes 2-dimethylamino-2-(4-methylbenzyl)-1-(4-morpholin-4-yl-phenyl)-butan-1-one.
6. The photosensitive resin composition according to claim 1, in, The photosensitive resin composition is used to form a solder resist layer.
7. A method for producing a printed wiring board, the method comprising producing a printed wiring board having a solder resist layer. in, The manufacturing method includes the step of forming the solder resist layer by curing the photosensitive resin composition according to claim 1 .