Nanocrystalline alloy ribbon and magnetic sheet

The nanocrystalline alloy thin strip composed of Fe1-xAx)aSibBcCudMe combined with quench coolant and high-temperature and high-speed heat treatment, the shortcomings of the nanocrystalline alloy thin strip in saturated magnetic flux density, magnetostriction and loss are solved, and high-efficiency magnetic characteristics are achieved and low loss, suppressing the embrittlement problem in heat treatment.

CN118974849APending Publication Date: 2024-11-15PROTERIAL LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202380031958.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-30
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

While the existing nanocrystalline alloy thin strips increase saturation flux density and reduce magnetostriction, it is difficult to maintain low loss and isotropic characteristics, and wrinkles and brittle problems are easily caused during the heat treatment process.

Method used

The thin strip of nanocrystalline alloy composed of Fe1-xAx)aSibBcCudMe, A is Ni and Co, M is the elements in Nb, Mo, V, Zr, Hf and W. The average crystal grain size is controlled by quench solidification and high-temperature and high-speed heat treatment. It is below 50 nm, and the design of the adhesive layer is combined to achieve high saturation flux density, low magnetostriction and low loss.

Benefits of technology

A thin nanocrystal alloy band with high saturation flux density, low magnetostriction, low loss and isotropy are achieved, which suppresses wrinkles and brittleness, and improves the excellent magnetic characteristics and duty cycle of the thin nanocrystal alloy band.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118974849A_ABST
    Figure CN118974849A_ABST
Patent Text Reader

Abstract

Provided is a nanocrystalline alloy ribbon having excellent magnetic properties, which has high saturation magnetic flux density and high magnetic permeability. The present invention relates to a sintered body which is represented by the compositional formula (Fe1-xAx) aSibBcCudMe, in which A is at least one of Ni and Co, M is at least one element selected from the group consisting of Nb, Mo, V, Zr, Hf and W, in atomic%, 75.0 < = a < = 81.0, 9.0 < = b < = 17.5, 5.0 < = c < = 10.0, 0.02 < = d < = 1.5, 0.1 < = e < = 3.5, and 0 < = x < = 0.1, in which an [alpha] Fe crystal phase having an average crystal grain size of 50 nm or less accounts for 40% or more in volume fraction, the saturation magnetic flux density is 1.36 T or more, the ratio Br / B8000 of the residual magnetic flux density Br to the magnetic flux density B8000 of a 8000 and the maximum magnetic permeability is more than 4000.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Cross-reference to related applications

[0002] The present international application claims the priority based on Japanese Patent Application No. 2022-055679 filed with the Japan Patent Office on March 30, 2022, the entire contents of which are hereby incorporated by reference into the present international application. Technical Field

[0003] The present disclosure relates to a nanocrystalline alloy ribbon having a nanocrystalline structure and a magnetic sheet using the same. Background Art

[0004] Nanocrystalline alloy ribbons with low magnetostriction and nanocrystalline structure are known. Nanocrystalline alloy ribbons have excellent magnetic properties such as high magnetic permeability and low loss, and exhibit these excellent magnetic properties over a wide frequency band. Nanocrystalline alloy ribbons are used in magnetic components such as transformers, motors, choke coils, magnetic shields, and current sensors.

[0005] As these magnetic components, with the high frequency of semiconductors, etc., the number of components with higher operating frequency specifications has also increased, and with this, the situation of replacing the soft magnetic materials used with nanocrystalline alloy strips has gradually increased. At this time, in order to achieve further miniaturization of the components, it is required to further increase the saturation flux density of the nanocrystalline alloy strip with low magnetostriction of about 1.2T.

[0006] In addition, in recent years, non-contact charging is being adopted or studied in the charging methods of mobile phones, small electronic products, electronic devices and electric vehicles. In non-contact charging devices, nanocrystalline alloy thin strips are sometimes used as soft magnetic materials for the magnetic core or magnetic shield of the transmitting and receiving coils. The main characteristics required of soft magnetic materials for non-contact charging are high magnetic permeability, low loss, high saturation magnetic flux density and thinness.

[0007] At present, the main frequency band used in contactless charging power transmission is about 100kHz, and the main soft magnetic materials used are limited to ferrite and nanocrystalline alloy ribbons. In nanocrystalline alloy ribbons, the thickness of the ribbon is about 20μm or less, which is very thin, and the saturation flux density is about 3 times that of ferrite. Therefore, nanocrystalline alloy ribbons are excellent in miniaturization and thinness, which greatly contributes to the miniaturization and thinness of receiving / transmitting coil groups. For this reason, nanocrystalline alloy ribbons are used or studied for use in contactless charging coils for various products.

[0008] In contactless charging, in order to shorten the charging time, there is a tendency to increase the charging output power. In this case, the magnetic flux flowing through the soft magnetic body can be increased. As a method to supplement the increase in magnetic flux, it is considered to increase the amount of nanocrystalline alloy ribbon used or replace it with a nanocrystalline alloy ribbon with a higher saturation magnetic flux density without changing the amount used, and the latter is particularly needed. In addition, in contactless charging, the magnetic flux flows from the coil to the thickness direction of the alloy ribbon, and then gradually flows from the center to the inside and outside of the surface, so the nanocrystalline alloy ribbon preferably has isotropic magnetic properties.

[0009] Japanese Patent Publication No. 2008-196006 discloses an Fe-based nanocrystalline soft magnetic alloy, characterized in that it is composed of the general formula: Fe 100-x-a-y-z A x M a Si y B z (atomic %), wherein A represents at least one element selected from Cu and Au, M represents at least one element selected from Ti, V, Zr, Nb, Mo, Hf, Ta, and W, and x, a, y, and z respectively satisfy 0≤x≤2, 0≤a≤1.5, 13≤y≤18, 4≤z≤10, and x+a+y+z≤25. The structure is composed of bcc Fe-Si grains with an average grain size of less than 120 nm and an amorphous phase, wherein the bcc Fe-Si grains account for more than 50% of the structure by volume fraction, the saturation magnetic flux density Bs is more than 1.4 T, and the saturation magnetostriction constant λs is -3.5×10 -6 Above and +3.5×10 -6 Within the following range.

[0010] Japanese Patent Publication No. 2014-516386 discloses an alloy in the form of a ribbon, which is composed of Fe 100-a-b-c-d-x-y-z Cu a Nb b M c T d Si x B y Z zcomposed of up to 1 at% of impurities, M is one or more of the elements Mo, Ta, or Zr, T is one or more of the elements V, Mn, Cr, Co, or Ni, Z is one or more of the elements C, P, or Ge, and 0 at% ≤ a < 1.5 at%, 0 at% ≤ b < 2 at%, 0 at% ≤ (b + c) < 2 at%, 0 at% ≤ d < 5 at%, 10 at% < x < 18 at%, 5 at% < y < 11 at%, and 0 at% ≤ z < 2 at%, and having: a nanocrystalline structure with an average diameter of less than 100 nm for at least 50 vol% of the particles, a hysteresis loop with a central linear portion, a remanence ratio Jr / Js < 0.1, and a ratio of coercive force Hc to anisotropy field strength Ha < 10%.

[0011] Prior art documents

[0012] Patent documents

[0013] Patent Document 1: Japanese Unexamined Patent Application Publication No. 2008-196006

[0014] Patent Document 2: Japanese Patent Application Laid-Open No. 2014-516386 Summary of the invention

[0015] Problems to be solved by the invention

[0016] The saturation magnetic flux density of the nanocrystalline alloy thin strip depends on the amount of Fe contained. In addition, in order for the nanocrystalline alloy thin strip to have excellent magnetic properties, it is necessary to have a fine nanocrystalline structure with an average grain size of 50 nm or less. For this purpose, it is necessary to add Cu that promotes nucleation and Nb that inhibits grain growth. In addition, in order for the nanocrystalline alloy thin strip to maintain low magnetostriction, it is necessary to add a certain amount of Si. Although it also depends on the required value of the magnetic properties, by maintaining a fine nanocrystalline structure with an average grain size of 50 nm or less and adjusting the amounts of Cu, Nb, and Si so that the magnetostriction is 7 ppm or less, it is possible to achieve a saturation magnetic flux density of about 1.20 T to 1.35 T.

[0017] In Patent Document 1, a nanocrystalline alloy thin strip with a saturation magnetic flux density of 1.4 T or more and low magnetostriction is disclosed. However, in order to increase the saturation magnetic flux density, the amounts of Cu and Nb are reduced, and the heating rate during heat treatment is also as slow as 10,000 °C / min. (166 K / sec.) or less, and it is impossible to obtain a fine nanocrystalline structure with an average crystal grain size of 50 nm or less required for exhibiting excellent magnetic properties.

[0018] In the method described in the patent document 1, the average crystal grain size is about 100nm. Therefore, in the embodiment of the patent document 1, the iron loss of 20kHz and 0.2T is more than 10W / kg. As described in Table 1 of the patent document 1, it is known that the core loss of the invention example is greatly deteriorated compared with the nanocrystalline material of the comparative example. The Fe-based nanocrystalline soft magnetic alloy of the patent document 1 can be used for the product use that attaches importance to the saturation flux density, but is not suitable for the use of the material that needs good core loss.

[0019] In patent document 2, nanocrystalline alloy ribbons of more than 1.4T are disclosed, but since tension is applied to the alloy and heat treatment is performed, anisotropy is imparted. Furthermore, the magnetic permeability is also below 3000, and the remanence Jr / Js (Br / Bs) is as low as below 0.1. Therefore, except for a part of products that require low magnetic permeability, the alloy of patent document 2 is not suitable for use. In addition, since the alloy ribbon is not bound during heat treatment, the ribbon is prone to wrinkles, stripes, etc. in the nanocrystalline state, and characteristics such as plate thickness deviation and space factor are prone to deterioration. In addition, the portion where wrinkles, stripes, etc. are generated becomes very brittle, and problems such as disconnection due to tension may occur.

[0020] The present invention discloses a nanocrystalline alloy ribbon having excellent magnetic properties with high saturation flux density and high magnetic permeability, and further obtains a nanocrystalline alloy ribbon with low magnetostriction, low loss and isotropy. In addition, a nanocrystalline alloy ribbon with suppressed wrinkles and stripes and a high space factor is obtained, or a magnetic sheet using them is provided.

[0021] Methods for solving problems

[0022] The nanocrystalline alloy ribbon of the first embodiment of the present invention has a composition formula (Fe 1-x A x ) a Si b B c Cu d M e Indicates that A is at least one of Ni and Co, M is at least one element selected from Nb, Mo, V, Zr, Hf and W, and is composed of 75.0≤a≤81.0, 9.0≤b≤18.0, 5.0≤c≤10.0, 0.02≤d≤1.2, 0.1≤e≤1.5, 0≤x≤0.1 in atomic %, an αFe crystal phase with an average grain size of less than 50nm accounts for more than 40% by volume, a saturation magnetic flux density is more than 1.36T, and a residual magnetic flux density Br is equal to the magnetic flux density B of a magnetic field of 8000A / m 8000 Ratio Br / B 8000 The maximum magnetic permeability is above 0.20 and above 4000.

[0023] The second mode of the magnetic sheet disclosed in the present invention comprises the nanocrystalline alloy strip disclosed in the present invention and an adhesive layer; the adhesive layer comprises a support body formed in a strip shape and an adhesive arranged on at least one of the first surface and the second surface of the above-mentioned support body; the above-mentioned nanocrystalline alloy strip is bonded to the above-mentioned adhesive of the above-mentioned adhesive layer, and the thickness of the above-mentioned adhesive layer is 1 to 10 μm.

[0024] Furthermore, the magnetic sheet may be formed such that the adhesive layer has an adhesive on the first surface and the second surface, and the plurality of nanocrystalline alloy thin strips are formed into a multilayer structure with the adhesive layer interposed therebetween.

[0025] Effects of the Invention

[0026] According to the present disclosure, a nanocrystalline alloy ribbon having high saturation flux density and high magnetic permeability and excellent magnetic properties can be obtained. Furthermore, a nanocrystalline alloy ribbon having low magnetostriction, low loss and isotropy can be obtained. In addition, wrinkles, stripes, etc. can be suppressed, and a nanocrystalline alloy ribbon having a high space factor can be obtained. In addition, a magnetic sheet using them can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a conceptual diagram showing one embodiment of the heat treatment method disclosed in the present invention.

[0028] Figure 2 It is a cross-sectional view explaining the structure of the magnetic sheet of the present disclosure.

[0029] Figure 3 It is a cross-sectional view explaining the structure of the magnetic sheet of the present disclosure.

[0030] Figure 4 It is a schematic diagram explaining the manufacturing method of the magnetic sheet of this disclosure.

[0031] Figure 5 It is a cross-sectional view explaining the structure of the laminated body supplied from the first delivery roll.

[0032] Figure 6 This is a cross-sectional view for explaining the structure of the laminated body from which the resin sheet is fed and peeled off from the first delivery roll.

[0033] Figure 7 It is a cross-sectional view illustrating the structure of the nanocrystalline alloy ribbon supplied from the second unwinding roll.

[0034] Figure 8 It is a cross-sectional view explaining the structure of the magnetic sheet of the present disclosure. DETAILED DESCRIPTION

[0035] Hereinafter, embodiments of the present disclosure will be described in detail. The present disclosure is not limited to the following embodiments, and can be implemented by appropriately adding modifications within the scope of the gist of the present disclosure.

[0036] The nanocrystalline alloy ribbon disclosed in the present invention has a composition formula (Fe 1-x A x ) a Si b B c Cu d M e It indicates that A is at least one of Ni and Co, M is at least one element selected from Nb, Mo, V, Zr, Hf and W, and is composed of 75.0≤a≤81.0, 9.0≤b≤18.0, 5.0≤c≤10.0, 0.02≤d≤1.2, 0.1≤e≤1.5, and 0≤x≤0.1 in atomic %.

[0037] The composition of the nanocrystalline alloy ribbon disclosed in the present invention is described in detail below.

[0038] The content of Fe (iron) is 75.0% or more and 81.0% or less in atomic %.

[0039] A high saturation magnetic flux density can be obtained by setting the Fe content to 75.0% or more, preferably 76% or more, and more preferably 77% or more.

[0040] If the Fe content exceeds 81.0%, it is difficult to reduce magnetostriction, so the Fe content is made 81.0% or less, preferably 80% or less, and more preferably 78% or less.

[0041] In addition, part of Fe may be replaced by at least one element selected from Ni and Co. 1-x A x ), A is at least one of Ni and Co, and x is 0.1 or less. When part of Fe is replaced by at least one of Ni and Co, (Fe 1-x A x ) a The a represented by the formula is in the range of 75.0%≤a≤81.0%. (Fe 1-x A x The content a of ) is preferably 76% or more, more preferably 77% or more. Also, it is preferably 80% or less, more preferably 78% or less.

[0042] The content of Si (silicon) is 9.0% or more and 18.0% or less in atomic %.

[0043] By making the Si content 9.0% or more, low magnetostriction can be achieved. The Si content is preferably 10% or more, more preferably 13% or more, and more preferably 15% or more. If it exceeds 18.0%, the amorphous forming ability decreases, crystallization occurs during casting, and the soft magnetic properties are significantly reduced. It is preferably 17.0% or less, and more preferably 16.5% or less.

[0044] The content of B (boron) is 5.0% or more and 10.0% or less in atomic %.

[0045] When the content of B is less than 5.0%, it is difficult to form an amorphous structure, so the content of B is set to 5.0% or more, preferably 5.5% or more, and more preferably 6.0% or more.

[0046] If the B content exceeds 10.0%, the Fe content and the Si content decrease, so the saturation magnetic flux density decreases and the magnetostriction increases. Therefore, the B content is set to 10.0% or less. It is preferably 8.5% or less, more preferably 7.5% or less, and further preferably 7.0% or less.

[0047] The content of Cu (copper) is 0.02% or more and 1.2% or less in atomic %.

[0048] By containing Cu, it is easy to obtain a uniform and fine nanocrystalline structure. When the Cu content is less than 0.02%, it is difficult to make the average particle size less than 50nm. Therefore, the Cu content is set to 0.02% or more. Preferably, it is 0.05% or more, preferably 0.2% or more, preferably 0.3% or more, and more preferably 0.5% or more.

[0049] When the Cu content exceeds 1.2%, the steel tends to become brittle and the saturation magnetic flux density decreases. Therefore, the Cu content is set to 1.5% or less, preferably 1.0% or less, more preferably 0.75% or less, and even more preferably 0.65% or less.

[0050] The M element is at least one selected from the group consisting of Nb, Mo, V, Zr, Hf, and W, and the content of the M element is 0.1% to 1.5% in atomic %.

[0051] By containing the M element, the precipitation starting temperature of the FeB compound that causes significant deterioration of soft magnetic properties can be moved to the high temperature side. As a result, the difference between the bcc Fe (αFe) crystallization starting temperature and the FeB precipitation starting temperature can be expanded, which can have the effect of expanding the optimal heat treatment temperature range and easing the heat treatment conditions. The content of the M element is preferably 0.3% or more, and more preferably 0.4% or more.

[0052] Since the M element is expensive, if the content of the M element increases, the price of the nanocrystalline alloy ribbon increases. Therefore, it is preferred that the content of the M element is small. Therefore, the content of the M element is set to 1.5% or less. It is preferably 1.0% or less, more preferably 0.9% or less, more preferably 0.8% or less, and more preferably 0.7% or less.

[0053] The nanocrystalline alloy ribbon disclosed herein may contain C (carbon). C has the effect of improving the melt fluidity of the molten metal, and improves castability by containing a trace amount. On the other hand, if a large amount is added, the ribbon becomes brittle, so the content of C is preferably less than 1% by mass. In addition, C may be contained as an impurity of the raw material.

[0054] The lower the amount of C, the higher the raw material price, so it is preferably allowed to be 0.01 mass % or more. In order to enhance the effect of C, the C content is preferably 0.1 mass % or more.

[0055] Furthermore, the nanocrystalline alloy ribbon disclosed herein may contain impurities other than the above-mentioned elements.

[0056] Examples of impurities include S (sulfur), O (oxygen), N (nitrogen), Cr, Mn, P, Ti, Al, etc. For example, the S content is preferably 200 mass ppm or less, the O content is preferably 5000 mass ppm or less, and the N content is preferably 1000 mass ppm or less.

[0057] The content of P is preferably 2000 mass ppm or less. The total content of these impurities is preferably 0.5 mass % or less. In addition, elements corresponding to impurities may be added as long as they are within the above range.

[0058] A preferred embodiment of the method for producing a nanocrystalline alloy ribbon disclosed herein will be described.

[0059] The nanocrystalline alloy ribbon disclosed in the present invention is obtained by spraying a molten alloy having the above alloy composition onto a rotating cooling roll and rapidly solidifying the alloy ribbon on the cooling roll. Then, the alloy ribbon is heat treated to obtain a nanocrystalline alloy ribbon.

[0060] The alloy ribbon obtained by rapidly cooling and solidifying the alloy melt becomes an alloy structure in an amorphous state, becoming an amorphous alloy ribbon. By heat treating the amorphous alloy ribbon, a nanocrystalline alloy ribbon can be obtained. The amorphous alloy ribbon obtained by rapidly cooling and solidifying the alloy melt can have a crystalline phase composed of fine crystals.

[0061] In order to obtain a molten alloy, various materials, i.e., various element sources (pure iron, ferroboron, ferrosilicon, etc.) for forming a target alloy composition may be combined. In addition, the various materials are heated in an induction heating furnace to a temperature above the melting point, thereby melting to form a molten alloy.

[0062] The alloy strip can be obtained by ejecting the alloy melt from a slit-shaped nozzle of a specified shape onto a rotating cooling roller, and rapidly solidifying the alloy melt on the cooling roller. The outer diameter of the cooling roller can be 350 to 1000 mm, the width can be 100 to 400 mm, and the peripheral speed of rotation can be 20 to 35 m / s. The cooling roller is internally provided with a cooling mechanism (water cooling, etc.) for suppressing the temperature rise of the outer periphery.

[0063] The outer periphery of the cooling roller is preferably made of a Cu alloy having a thermal conductivity of 120 W / (m·K) or more. By setting the thermal conductivity of the outer periphery to 120 W / (m·K) or more, the cooling rate of the alloy melt when casting the alloy strip can be increased.

[0064] This can suppress the embrittlement of the alloy strip, achieve thickening of the alloy strip (increase the thickness), and suppress surface crystallization during casting. Therefore, it is possible to suppress grain coarsening during heat treatment and reduce iron loss.

[0065] Furthermore, the thermal conductivity of the outer peripheral portion is preferably 150 W / (m·K) or more, and more preferably 180 W / (m·K) or more.

[0066] The outer peripheral portion of the cooling roller is a portion that can contact the alloy melt, and its thickness may be about 5 to 15 mm. The inner side may be made of a structural material that maintains the roller structure.

[0067] A nanocrystalline alloy ribbon can be obtained by heat treating an amorphous alloy ribbon produced by the above-mentioned rapid cooling method (a method of obtaining an alloy ribbon by rapidly cooling an alloy melt).

[0068] Regarding the heat treatment method in the present disclosure, preferred embodiments are described below.

[0069] In the present disclosure, the heat treatment is preferably performed at a temperature of 500 to 700° C. The heating rate is preferably 15000° C. / min. or more.

[0070] In the heat treatment disclosed herein, the amorphous alloy thin strip is preferably heat treated by contacting the amorphous alloy thin strip with a heating body set to a desired temperature (heat treatment temperature, 500 to 700° C.).

[0071] At this time, the contact time (holding time) of the amorphous alloy thin strip and the heating body is preferably 0.1 seconds to 30 seconds. The lower limit of the contact time is more preferably 0.2 seconds. The upper limit of the contact time is more preferably 10 seconds, further more preferably 5 seconds, and most preferably 2 seconds. In order to improve mass production, in the case of achieving high speed and stabilization, the contact time is preferably set to 0.2 seconds to 2 seconds.

[0072] In the heat treatment disclosed in the present invention, it is more preferable to set the heating rate to 30,000°C / min or more. The upper limit of the heating rate can be determined according to the equipment capacity of the heat treatment device, the temperature of the heating body and the thin strip pressing member, the contact state between the heating body and the thin strip pressing member and the thin strip, etc., but is substantially about 240,000°C / min. and preferably 100,000°C / min.

[0073] By applying a magnetic field or applying tension during heat treatment, the magnetic permeability and B80 can be adjusted. L / B80 W and other characteristics.

[0074] In the present disclosure, when the amorphous alloy thin ribbon is brought into contact with a heating body to perform heat treatment, the heat treatment is preferably performed in a state where the amorphous alloy thin ribbon is pressed against the heating body.

[0075] As a method for heat treatment in a state where the amorphous alloy ribbon is pressed against a heating body, a ribbon pressing member can be made to contact the opposite surface of the surface of the amorphous alloy ribbon that contacts the heating body, so that the amorphous alloy ribbon is pressed against the heating body. The ribbon pressing member is configured to pressurize the amorphous alloy ribbon, so that the amorphous alloy ribbon is pressed against the heating body. The ribbon pressing member is preferably a soft member.

[0076] As the soft member, a metal member is preferable. It should be noted that the soft member refers to a member that can be deformed along the roller.

[0077] In addition, a belt or a roller may be used as the thin strip pressing member.

[0078] An example of the heat treatment method disclosed in the present invention will be described using the drawings.

[0079] Figure 1 This is a conceptual diagram showing one embodiment of the heat treatment method disclosed in the present invention.

[0080] Figure 1 The heat treatment method shown in the figure comprises a heating roller 2 as a heating body, a thin strip pressing metal belt 3 (thin strip pressing member), and rollers 4 and 5 supporting the thin strip pressing metal belt 3. The thin strip pressing metal belt 3 (thin strip pressing member) is an example of a structure (element) in which an amorphous alloy thin strip (hereinafter also referred to as a thin strip) 1 is pressed against the heating roller 2 as a heating body.

[0081] In the heat treatment method, the amorphous alloy thin strip 1 is passed between the heating roller 2 (heating body) and the thin strip pressing metal belt 3, and the amorphous alloy thin strip 1 is heated while being pressed against the heating body (heating roller 2). Figure 1 The arrows in show the operation of each part, and the heating roller 2, rollers 4, and 5 are cylindrical and rotate. Thus, the amorphous alloy thin strip 1 is heated while being pressed against the heating roller 2 while being conveyed.

[0082] Here, the amorphous alloy ribbon 1 heated by the heating roller 2 becomes a nanocrystalline alloy ribbon.

[0083] As the rollers 4 and 5, it is preferable to use heated rollers that can be heated. Therefore, it is preferable to preheat the ribbon pressing metal belt 3 before contacting the amorphous alloy thin strip 1. When the rollers 4 and 5 are used as heated rollers, it is preferable to set the temperature of the ribbon pressing metal belt 3 (the temperature when the ribbon pressing metal belt 3 contacts the amorphous alloy thin strip 1) to a temperature that is equal to or slightly lower than the heating temperature of the amorphous alloy thin strip 1.

[0084] The temperature of the rollers 4 and 5 may be set to a temperature appropriate for pressing the thin strip against the metal strip 3. For example, it is also preferable to set the temperature of the rollers 4 and 5 to be about 50° C. higher than the temperature of the heating body. As the temperature of the thin strip against the metal strip 3 and the rollers 4 and 5, a temperature suitable for heat treatment of the amorphous alloy thin strip 1 can be selected.

[0085] The thin strip pressing metal belt 3 is an example of a soft member, and from the viewpoint of flexibility and strength, the soft member is preferably a metal member. For example, it is more preferable to use a material having excellent heat resistance, such as heat-resistant stainless steel and nickel-based super heat-resistant alloy.

[0086] According to the above heat treatment method, a structure is formed in which the soft member (strip pressing metal belt 3) is pressed against the opposite surface of the surface of the amorphous alloy strip 1 that contacts the heating body, thereby the amorphous alloy strip 1 is pressed against the heating body (heating roller 2). The amorphous alloy strip 1 is preferably in close contact with the heating roller 2 through the strip pressing metal belt 3, and the amorphous alloy strip 1, the strip pressing metal belt 3 and the heating roller 2 are operated as a whole.

[0087] Here, the heating roller 2 is a heating body for directly contacting the amorphous alloy thin strip and heating the amorphous alloy thin strip. The amorphous alloy thin strip 1 is heated by contacting (contacting) a portion of the outer peripheral surface (a portion of the circumferential direction) of the cylindrical heating roller 2. The heating roller 2 may also have a conveying driving force for the amorphous alloy thin strip.

[0088] As rollers for driving the thin strip to press the metal strip 3, both rollers 4 and 5 may be used, or only one of them may be used. It is also possible to configure the roller 5 to have a driving force and the roller 4 to be mechanically subordinate. In this way, it is possible to avoid complex control such as electrical synchronous operation of the rollers 4 and 5, and it is also unnecessary to correct the synchronization deviation caused by the thermal expansion difference between the rollers 4 and 5.

[0089] The heating roller 2 is an example of a heating body having a convex surface for contacting and heating the amorphous alloy thin strip 1. In addition, the "convex surface" refers to a surface that is raised on the side of the amorphous alloy thin strip. Figure 1 In addition to the curved surface formed by the cylindrical side surface, the roller shown in FIG. 1 may also have a curved surface that is a part of the member, such as the curved surface portion of a substantially D-shaped member, as long as the amorphous alloy strip follows and ensures sufficient contact. It should be noted that the heating body of the present disclosure may be a non-rotating structure or a structure in which the strip moves (slides) on the heating body.

[0090] In the nanocrystalline alloy ribbon disclosed herein, the αFe crystal phase having an average crystal grain size of 50 nm or less accounts for 40% or more in terms of volume ratio.

[0091] In addition, the saturation magnetic flux density of the nanocrystalline alloy ribbon disclosed in the present invention is above 1.36T, and the residual magnetic flux density Br is similar to the magnetic flux density B at a magnetic field of 8000A / m. 8000 Ratio Br / B 8000 The maximum magnetic permeability is 0.20 or more, and the maximum magnetic permeability is 4000 or more. The saturation magnetic flux density is preferably 1.37 T or more, and more preferably 1.40 T or more. The maximum magnetic permeability is preferably 5000 or more.

[0092] The nanocrystalline alloy ribbon of the present invention preferably has a magnetic flux density B80 when a magnetic field of 80 A / m is applied along the length direction of the nanocrystalline alloy ribbon. L The magnetic flux density B80 when a magnetic field of 80 A / m is applied along the width direction orthogonal to the length direction W Ratio (B80 L / B80 W ) is 0.60~1.40, and B80 L 、B80 W All are above 0.4T. L / B80 W ) is more preferably 0.70 to 1.30. In addition, B80 is more preferably L 、B80 W All are above 0.5T.

[0093] The saturation magnetostriction of the nanocrystalline alloy ribbon disclosed in the present invention is preferably 7 ppm or less, and more preferably 5 ppm or less.

[0094] In addition, the saturation magnetostriction is most preferably 0 ppm.

[0095] Composition formula (Fe 1-x A x ) a Si b B c Cu d M e Indicates that A is at least one of Ni and Co, M is at least one element selected from Nb, Mo, V, Zr, Hf and W, and when, in atomic %, 75.0≤a≤77.0, 15.0≤b≤18.0, 5.0≤c≤7.5, 0.02≤d≤1.2, 0.6≤e≤1.5, 0≤x≤0.1, a nanocrystalline alloy ribbon having a saturation magnetostriction of approximately 0 ppm (-2.0 ppm or more and 2.0 ppm or less) can be obtained. In addition, at this time, preferably 0.190≤b / a≤0.225.

[0096] The thickness of the nanocrystalline alloy ribbon disclosed in the present invention is preferably 25 μm or less, more preferably 20 μm or less. In addition, the thickness is preferably 5 μm or more, more preferably 10 μm or more. The width is preferably 5 mm or more, more preferably 20 mm or more, and more preferably 30 mm or more.

[0097] The wrinkle height of the nanocrystalline alloy ribbon disclosed herein is preferably 0.15 mm or less, more preferably 0.10 mm or less, and even more preferably 0.08 mm or less.

[0098] In addition, the nanocrystalline alloy ribbon disclosed herein preferably has a space factor of 68.0% or more, more preferably 70% or more, and even more preferably 75% or more.

[0099] The space factor can be measured by the following method in accordance with JIS C 2534:2017.

[0100] 20 pieces of thin strips cut into lengths of 120 mm were stacked and placed on a flat sample table. A flat anvil with a diameter of 16 mm was placed on the stacked thin strips at a pressure of 50 kPa, and the height was measured at intervals of 10 mm in the width direction. The maximum height at this time was set as hmax (μm), and the duty cycle LF was calculated by the following calculation formula.

[0101] LF(%)=sample weight(g) / density(g / cm 3 ) / hmax(μm) / sample length(240cm) / strip width(cm)×10000

[0102] At this time, the density (g / cm 3) is the density of the alloy strip after heat treatment. This density can be set to 7.4 g / cm 3 .

[0103] The nanocrystalline alloy ribbon disclosed in the present invention is suitable for use in magnetic cores, shielding materials, etc. used in electronic components, motors, etc. Thus, a magnetic core or sheet having excellent magnetic properties can be obtained.

[0104] The nanocrystalline alloy ribbon disclosed in the present disclosure can constitute a magnetic sheet that can be used as a magnetic sheet for contactless charging, for example.

[0105] The magnetic sheet disclosed in the present invention comprises a nanocrystalline alloy thin strip and an adhesive layer, wherein the adhesive layer comprises a support body formed into a strip shape and an adhesive provided on at least one of a first surface and a second surface of the support body, wherein the nanocrystalline alloy thin strip is bonded to the adhesive of the adhesive layer, and the thickness of the adhesive layer is 1 to 10 μm. The adhesive layer is preferably configured to have an adhesive on both surfaces of the support body.

[0106] In addition, it is preferred to make a magnetic sheet formed by stacking a plurality of nanocrystalline alloy strips via an adhesive layer. Specifically, a plurality of magnetic sheets with an adhesive layer attached to one side of the nanocrystalline alloy strips are prepared. By attaching a nanocrystalline alloy strip of another magnetic sheet to the side of the adhesive layer in the first magnetic sheet to which the nanocrystalline alloy strip is not attached, a magnetic sheet stacked with nanocrystalline alloy strips can be formed. At this time, the number of stacked nanocrystalline alloy strips can be appropriately selected in order to obtain the desired characteristics.

[0107] When a sample is collected from a magnetic sheet on which nanocrystalline alloy thin strips are stacked and measured, the magnetic sheet of the present disclosure preferably has an iron loss of 2000 kW / m at 128 kHz and 0.2 T. 3 Below, the real part of the complex permeability at 128kHz and 0.03V is greater than 1500.

[0108] The iron loss is preferably lower, more preferably 1800kW / m 3 Below, more preferably 1700kW / m 3 Below, more preferably 1500kW / m 3 the following.

[0109] When the magnetic sheet of the present disclosure is used for non-contact charging, the greater the charging output, the greater the magnetic flux generated. Therefore, in order to suppress magnetic saturation of the magnetic sheet and reduce eddy current loss, it is preferred to form cracks in the nanocrystalline alloy ribbon.

[0110] When a sample of the magnetic sheet of the present disclosure is collected from a stack of nanocrystalline alloy thin strips having cracks formed therein and measured, the iron loss at 128 kHz and 0.2 T is preferably 2000 kW / m 3Below, the real part of the complex permeability at 128kHz and 0.03V is 400 to 3000.

[0111] [Example 1]

[0112] In Example 1, the alloy composition is Fe 76.4 Si 16 B 6.5 Cu 0.6 Nb 0.5 The element source is combined in a manner, the combination is heated to 1350°C to produce an alloy melt, and the alloy melt is ejected onto a cooling roller with an outer diameter of 400mm and a width of 200mm rotating at a peripheral speed of 30m / sec, and is rapidly solidified on the cooling roller to produce an amorphous alloy thin strip. The outer periphery of the cooling roller is composed of a Cu alloy with a thermal conductivity of 150W / (m·K), and a cooling mechanism for controlling the temperature of the outer periphery is provided inside.

[0113] The amorphous alloy thin strip was heat treated under the conditions of a heating rate of 6°C / min., a heat treatment temperature of 470°C, and a holding time of 1 hour (Comparative Example 1) and a heat treatment under the conditions of a heating rate of 79200°C / min., a heat treatment temperature of 660°C, and a holding time of 1.2 seconds (Example 1). Figure 1 The heat treatment method shown in the figure. The samples of Example 1 and Comparative Example 1 after heat treatment are nanocrystalline alloy ribbons.

[0114] In addition, the nanocrystalline alloy ribbons of Example 1 and Comparative Example 1 had a width of 50 mm and a thickness of 16.4 μm.

[0115] For Example 1 and Comparative Example 1, the average grain size, iron loss at 20 kHz and 0.2 T, Br / B 8000 The maximum magnetic permeability is shown in Table 1. 8000 (Bs) is equivalent to 1.41T.

[0116] In Example 1, by setting the heating rate to 15000°C / min. or more, the average crystal grain size can be set to 50 nm or less. In addition, the iron loss at 20 kHz and 0.2 T is also excellent, being 10 W / kg or less. In addition, Br / B 8000 The value is 0.20 or more, and the maximum magnetic permeability is 4000 or more. In Example 1, a nanocrystalline alloy ribbon having high saturation magnetic flux density, low loss, and high magnetic permeability can be realized. The measurement method is described in Example 2.

[0117] [Table 1]

[0118]

[0119] [Example 2]

[0120] In Example 2, the element sources are combined in a manner to form the compositions shown in Table 2, and the combination is heated to 1350°C to prepare an alloy melt, which is then sprayed onto a cooling roller having an outer diameter of 400 mm and a width of 200 mm and rotating at a peripheral speed of 30 m / s, and is rapidly condensed and solidified on the cooling roller to prepare an amorphous alloy strip.

[0121] The width and thickness of the amorphous alloy ribbon are shown in Table 3. The outer peripheral portion of the cooling roller is made of a Cu alloy having a thermal conductivity of 150 W / (m·K), and a cooling mechanism for controlling the temperature of the outer peripheral portion is provided inside.

[0122] Amorphous alloy ribbons of various materials shown in Table 2 were heat treated under the conditions shown in Table 3. Evaluation results are shown in Tables 3 and 4. In addition, blank columns in the tables mean that no measurement was performed.

[0123] [Table 2]

[0124]

[0125] [Table 3]

[0126]

[0127] [Table 4]

[0128]

[0129] [Average grain size]

[0130] The average crystal grain size is obtained by using the integrated width of the diffraction peak from the (110) plane in the X-ray diffraction pattern obtained by the X-ray diffraction experiment, and is obtained by the Scherrer formula. The integrated width of the diffraction peak from the (110) plane is obtained by performing peak decomposition using a pseudo-Voigt function for the diffraction pattern, and D is obtained by the Scherrer formula (formula 1) given below, when the average grain size is set to D, the integrated width is set to β, the diffraction angle is set to θ, the Scherrer constant is set to K, and the wavelength of the X-ray is set to λ.

[0131] However, in this case, it is assumed that the wavelength λ of the applied X-ray is 0.154050 nm and the Scherrer constant K is 1.333. In addition, the integral width is corrected so that the integral width becomes narrower by the spread of the diffraction line width from the device.

[0132] [Number 1]

[0133]

[0134] [Volume rate]

[0135] The volume ratio is the volume ratio of the nanocrystals, and the portion other than the nanocrystals is an amorphous portion.

[0136] The volume fraction is obtained by the ratio of the integrated intensity of the diffraction peak from the (110) surface of Fe to the integrated intensity of the halo pattern. The integrated intensity of the halo pattern is the integrated intensity of the diffraction peak from the (110) surface of Fe + the integrated intensity near 2θ = 44°. The integrated intensity of the peak shown in the nanocrystal and the halo pattern shown in the amorphous are obtained by performing peak decomposition using a pseudo-Voigt function for the X-ray diffraction pattern.

[0137] When the integrated intensity of the (110) peak of the nanocrystal is set to Ic and the integrated intensity of the halo pattern near 2θ=44° is set to Ia, the volume fraction V is obtained by the formula (number 2) given below. However, in the case of the composition of this embodiment, the peaks of the integrated intensity of Fe and Fe2B overlap and are difficult to decompose, so Ic and Ia may also include the integrated intensity of the precipitated trace Fe2B.

[0138] [Number 2]

[0139]

[0140] [Saturation magnetic flux density Bs]

[0141] The saturation magnetic flux density Bs is obtained by applying a magnetic field of 8000A / m to the nanocrystalline alloy ribbon (single plate sample) after heat treatment using a DC magnetization characteristic test device manufactured by Metron Technology Co., Ltd. and measuring the maximum magnetic flux density at this time. The nanocrystalline alloy ribbon disclosed in the present invention has the characteristic of being relatively easy to saturate, so it will reach saturation when the magnetic field of 8000A / m is applied. 8000 Since it is approximately the same value as the saturation magnetic flux density Bs, B is used 8000 Indicates the saturation magnetic flux density Bs.

[0142] [Maximum magnetic permeability]

[0143] Regarding the maximum magnetic permeability, a DC magnetization characteristic testing device manufactured by Metron Giken Co., Ltd. was used to apply a magnetic field of 800 A / m to the nanocrystalline alloy strip (single plate sample) after heat treatment, and the magnetic permeability relative to the magnetic field H at this time was measured. The magnetic permeability showing the maximum at this time was used.

[0144] [Magnetic flux density B80]

[0145] A DC magnetization characteristic test device manufactured by Metron Giken Co., Ltd. was used to apply a magnetic field of 80 A / m in the length direction (casting direction) and in the width direction orthogonal to the length direction of the nanocrystalline alloy thin strip. The maximum magnetic flux density at this time was set as B80 L 、B80W Then, calculate the ratio B80 L / B80 W , for isotropic evaluation.

[0146] [Saturation magnetostriction]

[0147] A 5kOe magnetic field was applied to a sample (nanocrystalline alloy ribbon) with a strain gauge made by Kyowa Electric Co., Ltd. attached by an electromagnet. Then, the electromagnet was rotated 360°, and the maximum change in the elongation and contraction of the sample when the direction of the magnetic field applied to the sample was changed by 360° was measured based on the change in the resistance value of the strain gauge. Saturation magnetostriction = 2 / 3 × maximum change.

[0148] The relationship between saturation magnetostriction and Si / Fe (at% ratio) is shown in Table 5. As shown in Table 5, when the composition formula (Fe1-xAx)aSibBcCudMe is represented, A is at least one of Ni and Co, M is at least one element selected from Nb, Mo, V, Zr, Hf and W, and when, in terms of atomic %, 75.0≤a≤77.0, 15.0≤b≤18.0, 5.0≤c≤7.5, 0.02≤d≤1.2, 0.6≤e≤1.5, 0≤x≤0.1, a nanocrystalline alloy ribbon having a saturation magnetostriction of approximately 0 ppm (above -2.0 ppm and below 2.0 ppm) is obtained. In addition, at this time, 0.190≤b / a≤0.225.

[0149] [Table 5]

[0150]

[0151] [Wrinkle height]

[0152] The wrinkle height is the height of the stripes and wrinkles formed on the ribbon surface. The height of the nanocrystalline alloy ribbon surface was measured by using a laser microscope VR3200 manufactured by KEYENCE Corporation while the ribbon was sandwiched between glass plates, and the difference between the maximum and minimum values ​​was calculated as the wrinkle height.

[0153] The reason for sandwiching the nanocrystalline alloy ribbon between the glass plates is that if the ribbon is very thin and is simply placed on a measuring table, the ribbon will partially float due to undulations, etc., which will affect the height measurement, so the purpose is to minimize these effects.

[0154] [Magnetic flux density Br]

[0155] A magnetic field of 8000 A / m was applied to the nanocrystalline alloy ribbon (single plate sample) after the heat treatment using a DC magnetization characteristics tester manufactured by Metron Giken Co., Ltd., and the value of the magnetic flux density B when the magnetic field was 0 was defined as Br.

[0156] [Iron loss]

[0157] A toroidal core with an inner diameter of 8.8 mm and an outer diameter of 19.9 mm was punched out from a 15-layer nanocrystalline alloy ribbon using a BH analyzer SY8218 manufactured by Iwasaki Communication Equipment Co., Ltd. The core was placed in a housing and iron loss was measured. The measurement conditions were 15 turns of primary and secondary windings, a frequency of 20 kHz, and a magnetic flux density of 0.2 T.

[0158] As described above, according to the present disclosure, a nanocrystalline alloy ribbon with an average grain size of 50 nm or less and an αFe crystal phase accounting for more than 40% by volume and a saturation magnetic flux density of 1.36 T or more is obtained. In addition, the residual magnetic flux density Br and the magnetic flux density B at a magnetic field of 8000 A / m are obtained. 8000 Ratio Br / B 8000 The nanocrystalline alloy thin strip has a magnetic permeability of more than 0.20 and a maximum magnetic permeability of more than 4000.

[0159] In addition, according to the present disclosure, the magnetic flux density B80 when a magnetic field of 80 A / m is applied in the length direction of the nanocrystalline alloy thin strip is L and the magnetic flux density B80 when a magnetic field of 80 A / m is applied in the width direction perpendicular to the length direction. W Ratio (B80 L / B80 W ) is 0.60-1.40, and a nanocrystalline alloy ribbon showing isotropic properties is obtained.

[0160] In addition, according to the present disclosure, a nanocrystalline alloy ribbon having a saturation magnetostriction of 7 ppm or less is obtained.

[0161] In addition, according to the present disclosure, a nanocrystalline alloy ribbon having a wrinkle height of 0.15 mm or less and a space factor of 68.0% or more is obtained.

[0162] Therefore, according to the present disclosure, a nanocrystalline alloy ribbon with excellent magnetic properties having high saturation flux density and high magnetic permeability can be obtained. In addition, a nanocrystalline alloy ribbon with low magnetostriction, low loss and isotropy can be obtained. In addition, wrinkles, stripes, etc. can be suppressed, and a nanocrystalline alloy ribbon with a high space factor can be obtained.

[0163] [Example 3]

[0164] In Example 3, a 3 μm thick adhesive layer was attached to one side of the nanocrystalline alloy ribbon of Example 1 to produce a magnetic sheet.

[0165] Figure 2 It is a cross-sectional view cut along the width direction for explaining the structure of the magnetic sheet.

[0166] like Figure 2As shown, the magnetic sheet has a structure in which one adhesive layer 10 , one resin sheet 15 , and one nanocrystalline alloy thin strip 20 are stacked.

[0167] A support 11 and an adhesive 12 are provided on the adhesive layer 10. The support 11 is a film member formed in a long strip shape, for example, a film member formed in a rectangular shape. The support 11 is formed using a flexible resin material. As the resin material, polyethylene terephthalate (PET) can be used.

[0168] For example, a pressure-sensitive adhesive can be used as the adhesive 12. For example, a known adhesive such as an acrylic adhesive, a silicone adhesive, a polyurethane adhesive, a synthetic rubber, a natural rubber, etc. can be used as the adhesive 12. Acrylic adhesives are excellent in heat resistance and moisture resistance and can bond a wide range of materials, so they are preferably used as the adhesive 12.

[0169] Adhesive 12 is provided in a film or layer form on first surface 11A and second surface 11B of support 11. Here, the total thickness of adhesive 12 on first surface 11A side of adhesive layer 10 and adhesive 12 on support 11 and second surface 11B side is 3 μm.

[0170] Moreover, by removing the resin sheet 15 , the magnetic sheet can be attached to another member using the adhesive 12 on the second surface 11B side.

[0171] In addition, a plurality of the magnetic sheets are prepared to produce a magnetic sheet in which a plurality of nanocrystalline alloy thin strips are stacked. The plurality of magnetic sheets are used so that the nanocrystalline alloy thin strips are stacked with an adhesive layer interposed therebetween.

[0172] Specifically, first, the resin sheet 15 (15B) is peeled off from the side of the adhesive layer 10 of the first magnetic sheet where the nanocrystalline alloy thin strip 20 is not attached. Then, the nanocrystalline alloy thin strip 20 of another magnetic sheet is attached to the exposed portion of the adhesive 12 of the adhesive layer 10. This operation is repeated to form a magnetic sheet having 15 layers of nanocrystalline alloy thin strips stacked.

[0173] A magnetic sheet having 15 layers of nanocrystalline alloy thin strips was used and punched into a ring shape having an inner diameter of 8.8 mm and an outer diameter of 19.9 mm. The iron loss at 128 kHz and 0.2 T and the real part of the complex permeability at 128 kHz and 0.03 V were evaluated using the ring-shaped magnetic sheet. The results are shown in Table 6.

[0174] Similarly, 15-layer magnetic sheets were prepared for Nos. 1 to 11 of Example 2, and the iron loss at 128 kHz and 0.2 T and the real part of the complex permeability at 128 kHz and 0.03 V were evaluated. The results are shown in Table 6.

[0175] According to the present disclosure, the iron loss at 128kHz and 0.2T is 2000kW / m 3 A magnetic sheet having a real part of complex permeability of 1500 or more at 128kHz and 0.03V or less.

[0176] According to the present disclosure, a magnetic sheet having excellent magnetic properties can be configured.

[0177] [Table 6]

[0178]

[0179] [Example 4]

[0180] In Example 4, a 3 μm thick adhesive layer 10 is attached to one side of the nanocrystalline alloy ribbon of Example 1, and then cracks 21 are formed in the nanocrystalline alloy ribbon to produce a magnetic sheet.

[0181] Figure 3 It is a cross-sectional view cut along the width direction for explaining the structure of the magnetic sheet 100 .

[0182] like Figure 3 As shown, the magnetic sheet 100 has a structure in which one adhesive layer 10, one resin sheet 15, and one nanocrystalline alloy ribbon 20 are stacked. Here, cracks 21 are formed in the nanocrystalline alloy ribbon 20, and the nanocrystalline alloy ribbon 20 is divided into small pieces 22 by the cracks 21.

[0183] In addition, a plurality of the magnetic sheets are prepared to produce a magnetic sheet having a plurality of nanocrystalline alloy thin strips stacked thereon. The plurality of magnetic sheets are used to form a structure in which the nanocrystalline alloy thin strips 20 are stacked with the adhesive layer 10 interposed therebetween.

[0184] Specifically, first, the resin sheet 15 is peeled off on the side of the adhesive layer 10 of the first magnetic sheet 100 where the nanocrystalline alloy thin strip 20 is not attached. Next, the nanocrystalline alloy thin strip 20 of another magnetic sheet 100 is attached to the exposed portion of the adhesive 12 of the adhesive layer 10. This operation is repeated to form a magnetic sheet having 15 layers of nanocrystalline alloy thin strips stacked.

[0185] A magnetic sheet having 15 layers of nanocrystalline alloy thin strips was used and punched into a ring shape having an inner diameter of 8.8 mm and an outer diameter of 19.9 mm. The iron loss at 128 kHz and 0.2 T and the real part of the complex permeability at 128 kHz and 0.03 V were evaluated using the ring-shaped magnetic sheet. The results are shown in Table 7.

[0186] Similarly, a 15-layer magnetic sheet was prepared for No. 4 of Example 2, and the iron loss at 128 kHz and 0.2 T and the real part of the complex permeability at 128 kHz and 0.03 V were evaluated. The results are shown in Table 7.

[0187] According to the present disclosure, the iron loss at 128kHz and 0.2T is 2000kW / m 3 The following are magnetic sheets having a real part of complex permeability of 400 to 3000.

[0188] [Table 7]

[0189]

[0190] In Examples 3 and 4, the methods for measuring the iron loss and the real part of the complex permeability are as follows.

[0191] [Iron loss]

[0192] A toroidal core with an inner diameter of 8.8 mm and an outer diameter of 19.9 mm was punched out from a 15-layer magnetic sheet using a BH analyzer SY8218 manufactured by Iwasaki Communication Equipment Co., Ltd. The core was placed in a housing and iron loss was measured. The iron loss was measured under the conditions of 15 turns of primary and secondary windings, 128 kHz, and a magnetic flux density of 0.2 T.

[0193] [Complex permeability]

[0194] A toroidal core with an inner diameter of 8.8 mm and an outer diameter of 19.9 mm was punched out from a 15-layer magnetic sheet using a BH analyzer SY8218 manufactured by Iwasaki Communication Equipment Co., Ltd., and placed in a housing to measure the real part of the complex permeability. The measurement conditions were 15 turns of primary and secondary windings, a frequency of 128 kHz, and a voltage of 0.03 V.

[0195] Figure 4 Schematic diagram for explaining the method for manufacturing a magnetic sheet 100 having a single layer of nanocrystalline alloy thin strip according to the present disclosure. Figure 4 , a method of continuously attaching the adhesive layer 10 to the nanocrystalline alloy thin strip 20 is shown.

[0196] Magnetic sheet 100 use Figure 4 The manufacturing device 500 is shown in the figure. In the manufacturing device 500, a first unwinding roller 510, a first winding roller 520, a second unwinding roller 530, a plurality of attaching rollers 540, a crack section 550, a flattening roller 560, and a third winding roller 570 are provided from upstream to downstream of the manufacturing process. A plurality of guide rollers 580 may also be provided in the manufacturing device 500. The guide rollers 580 may also be arranged at positions not shown in the figure as required.

[0197] Figure 5 It is a cross-sectional view for explaining the structure of the stacked body supplied from the first delivery roll 510 .

[0198] like Figure 5As shown, a laminated body in which resin sheets 15A and 15B are laminated on the first surface 11A and the second surface 11B of the adhesive layer 10 is wound around the first delivery roll 510 .

[0199] The resin sheet 15A disposed on the first surface 11A is a protective sheet. The resin sheet 15B disposed on the second surface 11B is also referred to as a spacer. The resin sheet 15A is a sheet thinner than the resin sheet 15B disposed on the second surface 11B.

[0200] Figure 6 This is a cross-sectional view for explaining the structure of the laminated body in which the resin sheet 15A is supplied from the first unwinding roll 510 and peeled off.

[0201] like Figure 6 As shown in FIG. 1 , the resin sheet 15A is peeled off from the laminate unrolled from the first unrolling roller 510. Figure 4 As shown, the peeled resin sheet 15A is taken up by the first take-up roller 520 .

[0202] Figure 7 It is a cross-sectional view illustrating the structure of the nanocrystalline alloy strip 20 supplied from the second unwinding roll 530 .

[0203] The laminated body from which the resin sheet 15A is peeled off is guided to the attaching roller 540 by a plurality of guide rollers 580. The nanocrystalline alloy thin strip 20 unwound from the second unwinding roller 530 is further guided to the attaching roller 540. Figure 7 As shown, cracks 21 are not formed in the nanocrystalline alloy strip 20 guided to the attachment roller 540 .

[0204] Figure 2 It is a cross-sectional view illustrating a state where the nanocrystalline alloy thin strip 20 is bonded to the adhesive layer 10 by the bonding roller 540 .

[0205] As the attachment roller 540, Figure 4 As shown, two cylindrical rollers are provided which are arranged opposite to each other. The two rollers each have a smooth peripheral surface without protrusions. The two rollers press and adhere the nanocrystalline alloy ribbon 20 to the laminated body from which the resin sheet 15A has been peeled.

[0206] Specifically, the laminate and the nanocrystalline alloy thin strip 20 are guided between two rollers arranged opposite to each other, and two rollers are used, such as Figure 2 As shown, the nanocrystalline alloy thin strip 20 is pressed and bonded to the first surface 11A of the adhesive layer 10. Figure 4 As shown, the stacked body to which the nanocrystalline alloy strips 20 are bonded is guided from the attachment roller 540 to the crack portion 550 .

[0207] In addition, when the crack 21 is not formed, the strand may be wound up by the third winding roller 570 instead of being guided to the crack portion 550, or may be cut into a desired length.

[0208] Figure 3 This is a cross-sectional view illustrating a state in which cracks 21 are formed in crack portion 550 of nanocrystalline alloy ribbon 20 .

[0209] The crack section 550 forms cracks 21 in the nanocrystalline alloy ribbon 20 bonded to the adhesive layer 10. Specifically, the crack section 550 includes two rollers disposed opposite to each other. That is, the crack section 550 includes a crack roller 550A and a support roller 550B.

[0210] The manufacturing device 500 guides the laminated body bonded with the nanocrystalline alloy thin strip 20 between the two rollers. The crack roller 550A is a cylindrical roller with protrusions on the circumference. The support roller 550B is a cylindrical roller without protrusions on the circumference. The manufacturing device 500 presses the protrusion of the crack roller 550A against the nanocrystalline alloy thin strip 20, as shown in FIG. Figure 3 As shown, cracks 21 are formed.

[0211] The support roll 550B is disposed on the laminated body side from which the resin sheet 15 has been peeled. The nanocrystalline alloy ribbon 20 having the cracks 21 formed therein includes a plurality of small pieces 22. The plurality of small pieces 22 are bonded to the adhesive layer 10.

[0212] Here, the structure of the crack roller 550A is described. On the crack roller 550A, a plurality of convex members are arranged on the circumferential surface as the above-mentioned protrusions. The front end shape of the end of the convex member of the crack roller 550A can also be flat, conical, inverted conical with a central depression, or cylindrical. The plurality of convex members can be arranged regularly or irregularly.

[0213] The laminated body guided from the crack portion 550 to the flattening roller 560 is flattened by the flattening roller 560. The flattening roller 560 is also referred to as a reforming roller.

[0214] Specifically, the laminate is guided between two rollers of the flattening rollers 560 that are arranged opposite to each other, and the laminate is sandwiched and pressed by the two rollers. Thus, the surface of the nanocrystalline alloy ribbon 20 having the cracks 21 formed therein is flattened.

[0215] The laminated body after the flattening treatment becomes the magnetic sheet 100. The magnetic sheet 100 is guided to the third winding roller 570 via the guide roller 580. The magnetic sheet 100 is wound on the third winding roller 570. The magnetic sheet 100 wound on the third winding roller 570 and in a ring or spiral shape is a wound body-shaped magnetic sheet 200.

[0216] The magnetic sheet 100 may be wound up, or may be cut into a predetermined length without being wound up.

[0217] Here, the width B of the nanocrystalline alloy ribbon 20 and the width A of the adhesive layer 10 preferably have a shape satisfying the following relationship (see Figure 8 ).

[0218] 0.2mm≤(width A-width B)≤3mm

[0219] Width A is a dimension related to the adhesive layer 10, and more preferably a dimension related to the region of the adhesive layer 10 where the adhesive 12 for bonding the nanocrystalline alloy strip 20 is provided. Width B is a dimension related to the nanocrystalline alloy strip 20. In the case where the adhesive 12 is provided on the entire surface of the support 11 of the adhesive layer 10, width A is a dimension related to the adhesive layer 10 or the support 11.

[0220] Here, the lower limit of (width A-width B) is preferably 0.5 mm, and more preferably 1.0 mm. In addition, the upper limit of (width A-width B) is preferably 2.5 mm, and more preferably 2.0 mm.

[0221] The nanocrystalline alloy thin strip 20 may be arranged so that the center of the nanocrystalline alloy thin strip 20 is aligned with the adhesive layer 10 in the width direction, or may be arranged so that the center is separated. In this case, the relationship of 0 mm < gap a and 0 mm < gap b is satisfied (see Figure 8 ) method.

[0222] The gap a and the gap b are the distances from the end of the adhesive layer 10 to the end of the nanocrystalline alloy thin strip 20. Specifically, the gap a is the distance from the first adhesive layer end 10X of the adhesive layer 10 to the first thin strip end 20X of the nanocrystalline alloy thin strip 20. The gap b is the distance from the second adhesive layer end 10Y of the adhesive layer 10 to the second thin strip end 20Y of the nanocrystalline alloy thin strip 20.

[0223] The first thin strip end 20X is the end on the same side as the first adhesive layer end 10X in the nanocrystalline alloy thin strip 20. The second adhesive layer end 10Y is the end on the opposite side of the first adhesive layer end 10X of the adhesive layer 10. The second thin strip end 20Y is the end on the same side as the second adhesive layer end 10Y in the nanocrystalline alloy thin strip 20.

[0224] The width A, the width B, the gap a, and the gap b are dimensions in a direction intersecting, more preferably orthogonal to, the length direction of the magnetic sheet 100. The length direction of the magnetic sheet 100 is the same as the length direction of the adhesive layer 10. In addition, the length direction of the magnetic sheet 100 is the same as the length direction of the nanocrystalline alloy ribbon 20.

[0225] In the magnetic sheet 100, the width A of the region where the adhesive 12 is provided in the adhesive layer 10 is set to be wider than the width B of the nanocrystalline alloy ribbon 20. According to such a configuration, when the nanocrystalline alloy ribbon 20 is attached to the adhesive layer 10, even if the adhesive layer 10 and the nanocrystalline alloy ribbon 20 meander, the adhesive 12 of the adhesive layer 10 can be easily arranged on the entire surface of the nanocrystalline alloy ribbon 20. In addition, by arranging the adhesive layer 10 on the entire surface of the nanocrystalline alloy ribbon 20, it is possible to suppress the falling of the small pieces 22 after the cracks 21 are formed in the nanocrystalline alloy ribbon 20.

[0226] The value obtained by subtracting the width B from the width A of the magnetic sheet 100 is set to be 0.2 mm or more. With such a configuration, when the nanocrystalline alloy ribbon 20 is attached to the adhesive layer 10 , it is easy to suppress the occurrence of a portion on the nanocrystalline alloy ribbon 20 where the adhesive 12 is not disposed.

[0227] The value obtained by subtracting the width B from the width A of the magnetic sheet 100 is set to be 3 mm or less. According to such a configuration, it is easy to prevent the portion of the magnetic sheet 100 where the nanocrystalline alloy ribbon 20 is not arranged from becoming larger. In addition, when the magnetic sheets 100 are arranged in parallel, it is easy to prevent the interval (magnetic gap) between the nanocrystalline alloy ribbons from becoming larger.

[0228] The magnetic sheet 100 is set to satisfy the relationship of 0 mm < gap a and 0 mm < gap b. According to such a configuration, when the nanocrystalline alloy strip 20 is attached to the adhesive layer 10, it is easy to suppress the nanocrystalline alloy strip 20 from protruding from the area where the adhesive 12 is provided. Therefore, it is easy to suppress the generation of a portion on the nanocrystalline alloy strip 20 where the adhesive 12 is not provided.

[0229] According to the present disclosure, a nanocrystalline alloy ribbon with high saturation flux density and high magnetic permeability is obtained. In addition, according to the present disclosure, a nanocrystalline alloy ribbon with low magnetostriction, low loss and isotropy is obtained. In addition, according to the present disclosure, wrinkles, stripes, etc. can be suppressed, and a nanocrystalline alloy ribbon with a high space factor is obtained.

[0230] According to the present disclosure, a magnetic sheet using a nanocrystalline alloy ribbon having excellent magnetic properties is obtained.

Claims

1. A nanocrystalline alloy ribbon having a composition formula (Fe 1-x A x ) a Si b B c Cu d M e Indicates that A is at least one of Ni and Co, M is at least one element selected from Nb, Mo, V, Zr, Hf and W, and is composed of 75.0≤a≤81.0, 9.0≤b≤18.0, 5.0≤c≤10.0, 0.02≤d≤1.2, 0.1≤e≤1.5, 0≤x≤0.1 in atomic %, an αFe crystal phase with an average grain size of less than 50nm accounts for more than 40% by volume, a saturation magnetic flux density is more than 1.36T, and a residual magnetic flux density Br is equal to the magnetic flux density B of a magnetic field of 8000A / m 8000 Br / B 8000 The maximum magnetic permeability is above 0.20 and above 4000.

2. The nanocrystalline alloy ribbon according to claim 1, wherein: The magnetic flux density B80 when a magnetic field of 80A / m is applied along the length direction of the nanocrystalline alloy ribbon L The magnetic flux density B80 when a magnetic field of 80 A / m is applied along the width direction orthogonal to the length direction W The ratio of B80 L / B80 W 0.60~1.40, and B80 L 、B80 W All are above 0.4T.

3. The nanocrystalline alloy ribbon according to claim 1 or 2, wherein: The saturation magnetostriction is 7 ppm or less.

4. The nanocrystalline alloy ribbon according to any one of claims 1 to 3, wherein The thickness is 20 μm or less and the width is 5 mm or more.

5. The nanocrystalline alloy ribbon according to any one of claims 1 to 4, wherein: The wrinkle height of the nanocrystalline alloy ribbon is less than 0.15 mm, and the space factor is more than 68.0%.

6. A magnetic sheet comprising the nanocrystalline alloy thin strip according to any one of claims 1 to 5 and an adhesive layer, The adhesive layer includes a support body formed in a strip shape and an adhesive provided on at least one of a first surface and a second surface of the support body. The nanocrystalline alloy ribbon is bonded to the adhesive of the adhesive layer, The thickness of the adhesive layer is 1-10 μm.

7. A magnetic sheet comprising the nanocrystalline alloy thin strip according to any one of claims 1 to 5 and an adhesive layer, The adhesive layer includes a support body formed in a strip shape and an adhesive provided on a first surface and a second surface of the support body. The thickness of the adhesive layer is 1 to 10 μm. The plurality of nanocrystalline alloy thin strips are formed into a multilayer structure with the adhesive layer interposed therebetween.

8. The magnetic sheet according to claim 6 or 7, wherein The iron loss at 128kHz and 0.2T is 2000kW / m 3 Below, the real part of the complex permeability at 128kHz and 0.03V is greater than 1500.

9. The magnetic sheet according to any one of claims 6 to 8, wherein Cracks are formed in the nanocrystalline alloy ribbon.

10. The magnetic sheet according to claim 9, wherein The iron loss at 128kHz and 0.2T is 2000kW / m 3 Below, the real part of the complex permeability at 128kHz and 0.03V is 400 to 3000.

Citation Information

Cited By

  • High-squareness-ratio amorphous alloy and preparation method thereof

    CN121826554A