Method for producing nanocrystalline alloy ribbon and method for producing magnetic sheet
By contacting the amorphous alloy thin strip with the heating body for heat treatment, the problems of low productivity and poor magnetic characteristics of the nanocrystalline alloy thin strip in the prior art are solved, and efficient production of nanocrystalline alloy thin strips with excellent magnetic characteristics are achieved. .
Patent Information
- Application Number
- CN202380031853.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-30
- Filing Date
- 2023-03-30
- Publication Date
- 2024-11-15
AI Technical Summary
The prior art is difficult to efficiently produce thin nanocrystalline alloy strips with excellent magnetic properties and isotropy through continuous heat treatment methods, and the productivity is low, making it prone to wrinkles, stripes and fracture problems.
The amorphous alloy thin strip is used to contact the heating body for heating, and heat treatment is carried out through uniform pressure and the contact surface of the heating body to control the heating speed and temperature, ensuring uniform heating of the thin strip and suppressing wrinkles and stripes caused by crystallization.
The production of nanocrystalline alloy thin strips with high saturation flux density, low magnetostriction, low loss and isotropy is achieved, which improves productivity and suppresses the generation of wrinkles and fringes.
Smart Images

Figure CN118974288A_ABST
Abstract
Description
[0001] Cross-reference to related applications
[0002] The present international application claims the priority based on Japanese Patent Application Nos. 2022-055681 and 2022-055682 filed with the Japan Patent Office on March 30, 2022, the entire contents of which are hereby incorporated by reference into the present international application. Technical Field
[0003] The present disclosure relates to a method for manufacturing a nanocrystalline alloy ribbon having a nanocrystalline structure and a method for manufacturing a magnetic sheet using the nanocrystalline alloy ribbon. Background Art
[0004] Nanocrystalline alloy ribbons with low magnetostriction having a nanocrystalline structure are known. Nanocrystalline alloy ribbons have excellent magnetic properties such as high magnetic permeability and low loss, and these excellent magnetic properties are displayed in a wide band. Nanocrystalline alloy ribbons are used in magnetic components such as transformers, motors, choke coils, magnetic shields, and current sensors. Among these magnetic components, with the high frequency of semiconductors, there are also many components with higher operating frequencies. With this, the situation of replacing the soft magnetic materials used with nanocrystalline alloy ribbons is increasing. The reason is that the nanocrystalline alloy ribbon has the following excellent characteristics: the saturation flux density is as high as 1.2T or more and the saturation flux density required to achieve further miniaturization of the components, and further, the nanocrystalline alloy ribbon is low magnetostriction and low loss.
[0005] In addition, in recent years, non-contact charging is being adopted or studied for charging methods for mobile phones, small appliances, electronic devices, and electric vehicles. In non-contact charging devices, nanocrystalline alloy thin strips are sometimes used as soft magnetic materials for the magnetic core or magnetic shielding of the transceiver coil. The main properties required of soft magnetic materials for non-contact charging are high magnetic permeability, low loss, high saturation magnetic flux density, and thinness.
[0006] The frequency band currently used for power transmission for contactless charging is around 100kHz, and the main soft magnetic materials used are limited to ferrite and nanocrystalline alloy ribbons. The thickness of the nanocrystalline alloy ribbon is about 20μm or less, which is very thin, and the saturation flux density is about 3 times that of ferrite. Therefore, the nanocrystalline alloy ribbon is excellent in miniaturization and thinness, which greatly contributes to the miniaturization and thinness of the receiving / transmitting coil group. As a result, nanocrystalline alloy ribbons are being used or are being studied in the coils for contactless charging of various products.
[0007] In contactless charging, in order to shorten the charging time, there is a tendency to increase the charging output. In order to correspond to this, for example, the magnetic flux flowing through the soft magnetic body can be increased. As a method to supplement the increase in magnetic flux, it is considered to increase the amount of soft magnetic body used or replace it with a soft magnetic body with a higher saturation magnetic flux density. In particular, the latter is required, thereby expanding the use of nanocrystalline alloy strips. In addition, in contactless charging, since the magnetic flux flows from the coil to the thickness direction of the alloy strip, and then flows from the center to the inside and outside of the surface, the nanocrystalline alloy strip preferably has isotropic magnetic properties.
[0008] On the other hand, in the case of making a nanocrystalline alloy ribbon used in contactless charging, the nanocrystalline alloy ribbon is made by casting an amorphous alloy ribbon for the nanocrystalline alloy ribbon and temporarily winding it. Then, a certain amount of amorphous alloy ribbon is rolled out from the wound ribbon, rewound on a core wound into a ring shape, and placed in a heat treatment furnace to the allowable amount of multiple heat treatment furnaces, and heat treated at a temperature of 550°C to 580°C. The nanocrystalline alloy ribbon is made in this way. When the heat treatment process performed by the heat treatment furnace includes cooling, etc., it takes 5 to 8 hours. The nanocrystalline alloy ribbon nanocrystallized by heat treatment is rewound from the core wound into a ring shape while being laminated, stacked, etc., thereby making a magnetic sheet.
[0009] The above is a process in which a lamination and stacking process is added to the manufacturing process of the core product using the conventional nanocrystalline alloy thin strip. In the case of the manufacturing process of the annular core product formed by rewinding the thin strip, the core is made in a manner consistent with the size of the final product, heat treated, and transferred to the subsequent process, so there is no unnecessary process in the above manufacturing process. However, in the case of the magnetic sheet, the thin strip is rewound for heat treatment to make the annular core, but this process is not necessary. Since the magnetic sheet will not directly use the annular core made by rewinding the thin strip, it becomes an unnecessary process to rewind the cast and wound thin strip to make the annular core. Therefore, it is ideal that the magnetic sheet is preferably manufactured by directly rolling out the cast thin strip and continuously performing heat treatment, winding or direct lamination and stacking processes.
[0010] Japanese Patent Application No. 2014-516386 discloses a process of heat treating an amorphous alloy ribbon under a continuous furnace tensile stress at a temperature Ta of 450°C ≤ Ta ≤ 750°C. The composition of the amorphous alloy ribbon is Fe 100-a-b-c-d-x-y-z Cu a Nb b M c T d Si x B y Z zand consists of impurities of up to 1 at%, M is one or more of the elements Mo, Ta or Zr, T is one or more of the elements V, Mn, Cr, Co or Ni, Z is one or more of the elements C, P or Ge, 0 at% ≤ a < 1.5 at%, 0 at% ≤ b < 2 at%, 0 at% ≤ (b + c) < 2 at%, 0 at% ≤ d < 5 at%, 10 at% < x < 18 at%, 5 at% < y < 11 at% and 0 at% ≤ z < 2 at%.
[0011] A method for manufacturing a soft magnetic material that takes into account high saturation magnetization and low coercive force is disclosed in Patent Document 2. The soft magnetic material has a composition formula Fe 100-a-b-c B a Cu b M’ c , where M’ is at least one element selected from Nb, Mo, Ta, W, Ni and Co, and satisfies the composition of 10 ≤ a ≤ 16, 0 < b ≤ 2 and 0 ≤ c ≤ 8. Moreover, the soft magnetic material is manufactured by heating an alloy having an amorphous phase at a heating rate of 10 °C / second or more, and holding it for 0 to 80 seconds at a temperature above the crystallization start temperature and below the generation start temperature of the Fe-B compound.
[0012] A nanocrystalline alloy ribbon is disclosed in Patent Document 3. The nanocrystalline alloy ribbon is represented by the composition formula Fe 100-a-b-c-d B a Si b Cu c M d , where a, b, c and d are all atomic%, and respectively satisfy 0 < a, 0 < b, 0 < c, 0 ≤ d and 78 ≤ 100 - a - b - c - d, and M represents at least one element selected from the group consisting of Ti, Zr, Hf, V, Nb, Ta, Cr, Mo and W. The nanocrystalline alloy ribbon is manufactured by continuously advancing the amorphous alloy ribbon in a state where a tension F is applied to the amorphous alloy ribbon, and bringing a part of the region of the amorphous alloy ribbon into contact with a heat transfer medium maintained at a temperature of 450 °C or more. At this time, the temperature of the amorphous alloy ribbon is raised to a reaching temperature of 450 °C or more in such a manner that the average heating rate in the temperature range from 350 °C to 450 °C becomes 10 °C / second or more.
[0013] A method for treating an amorphous alloy ribbon is disclosed in Patent Document 4. In this method, the amorphous alloy ribbon is conveyed forward along a traveling path at a set conveying speed and guided in a non-relaxed manner. Then, the amorphous alloy ribbon is heated to a temperature for starting heat treatment at a speed exceeding 10 3 °C / second, and the amorphous alloy ribbon is heated at a speed exceeding 10 3During the heat treatment, mechanical constraints are applied to the amorphous alloy ribbon before it takes a specific shape in a static state after the heat treatment, and then after the heat treatment, the amorphous alloy ribbon is cooled at a speed to preserve the specific shape.
[0014] Prior art literature
[0015] Patent Literature
[0016] Patent Document 1: Japanese Patent Application No. 2014-516386
[0017] Patent Document 2: International Publication No. 2018 / 025931
[0018] Patent Document 3: International Publication No. 2017 / 150440
[0019] Patent Document 4: Japanese Patent No. 6254757 Summary of the invention
[0020] Problems to be solved by the invention
[0021] In order to continuously heat treat the nanocrystalline alloy ribbon, it is necessary to continuously heat treat the thin ribbon taken up after casting at a high temperature after unwinding, and in order to improve productivity, it is required to be as fast as possible and not to break. In addition, in order to make the nanocrystalline alloy ribbon have excellent magnetic properties, it is necessary to have a fine nanocrystalline structure with an average particle size of less than 50nm and low magnetostriction. In order to maintain low magnetostriction, a certain amount of Si needs to be added.
[0022] Furthermore, in the use of magnetic sheets for contactless charging, it is required that the magnetic properties be isotropic, wrinkles and striae that are easily generated during nanocrystallization during heat treatment be as small as possible, and the space factor be high.
[0023] Patent document 1 discloses nanocrystalline alloy ribbons of 1.4T or more, but since tension is applied and heat treatment is performed, anisotropy may be imparted. Furthermore, the magnetic permeability is also below 3000, and the residual magnetic susceptibility Jr / Js (Br / Bs) is as low as below 0.1. Therefore, the alloy of Patent document 1 is difficult to use except for some products that require low magnetic permeability. In addition, since the alloy ribbon is not constrained during heat treatment, wrinkles, stripes, etc. are easily generated in the ribbon during nanocrystalline, and the plate thickness deviation, space factor, etc. may deteriorate. In addition, the portion where wrinkles or stripes are generated becomes very brittle, and problems such as breakage due to tension may occur.
[0024] Patent document 2 discloses a method of heating an amorphous alloy by sandwiching an amorphous alloy between heated blocks. A series of heat treatment operations such as sandwiching an amorphous thin strip between blocks and removing the amorphous alloy after heating takes time. Moreover, the amount of treatment at one time is limited, so it is not suitable as a method for heat treating a large number of thin strips during mass production. In addition, since it is impossible to continuously heat treat the thin strip, it is not suitable as a heat treatment method for magnetic sheets.
[0025] In addition, the soft magnetic material described in Patent Document 2 does not contain Si, so no SiO2 film that contributes to the corrosion resistance of the soft magnetic material is formed on the surface of the material. Therefore, it may be difficult to prevent rust and the like.
[0026] According to the method described in Patent Document 3, a method for bringing a thin strip into contact with a heated plate is disclosed. Since the thin strip can be heat treated while being transported, mass production is high. In addition, good magnetic properties can be obtained. However, although tension is applied to the thin strip so that the thin strip is in uniform contact with the heating plate, it takes time and effort to make the moving thin strip in uniform and continuous contact with the heating plate. In addition, only one side of the thin strip is in contact with the heating plate and is transported, and the surface on the opposite side of the surface in contact with the heating plate is not constrained, so it may not be possible to suppress the generation of wrinkles and stripes caused by crystallization when in contact with the heating plate or the local floating of the thin strip.
[0027] According to the method described in patent document 4, a method for making a thin strip contact with a heated roller is disclosed. Since the thin strip can be heat-treated while being transported, mass production is high. However, since a stable heat treatment is achieved by pressing the thin strip against the roller with a large tension of more than 25MPa, anisotropy may be imparted during the heat treatment as in patent document 1. Therefore, it is not suitable for applications requiring isotropy. In addition, only one side of the thin strip is in contact with the heated roller and transported, and the surface on the opposite side of the surface in contact with the heated roller is not constrained, so it is impossible to suppress the generation of wrinkles and stripes caused by crystallization when in contact with the heated roller, or the thin strip may float locally. In addition, there is a problem of fracture due to tension.
[0028] In addition, the nanocrystalline alloy strip is manufactured by the following method: the alloy melt adjusted to a specified alloy composition is ejected onto a rotating cooling roller, and the alloy strip is manufactured by rapid solidification, and then the alloy strip is heat treated. The thickness of the nanocrystalline alloy strip is thin, and it can be manufactured into a long strip with a specified width. According to this manufacturing method, it is easy to introduce anisotropy in the casting direction (length direction), and even after heat treatment, there is a tendency that the magnetic properties are different in the length direction of the long strip and the width direction orthogonal to the length direction.
[0029] For example, nanocrystalline alloy ribbons used in stators of electric motors, magnetic sheets of contactless charging coils, etc. are required to be as isotropic as possible. However, as described above, it is difficult to obtain nanocrystalline alloy ribbons having excellent magnetic properties (high saturation magnetic flux density, low iron loss) and isotropic properties by a continuous heat treatment method with high productivity.
[0030] The present disclosure provides a method for manufacturing a nanocrystalline alloy ribbon by continuously heat treating a ribbon and a method for manufacturing a magnetic sheet using the method. The method for manufacturing a nanocrystalline alloy ribbon includes: a method for manufacturing a nanocrystalline alloy ribbon having excellent magnetic properties such as high saturation flux density and high magnetic permeability; a method for manufacturing a nanocrystalline alloy ribbon having low magnetostriction, low loss, and isotropy; or a method for manufacturing a nanocrystalline alloy ribbon having high space factor and capable of suppressing wrinkles, stripes, etc.
[0031] Methods for solving problems
[0032] A method for manufacturing a nanocrystalline alloy ribbon according to a first embodiment of the present invention is to heat an amorphous alloy ribbon by contacting the amorphous alloy ribbon with a heating body, thereby manufacturing a nanocrystalline alloy ribbon having a structure in which grains with an average crystal grain size of 50 nm or less exist in an amorphous phase.
[0033] The nanocrystalline alloy ribbon is composed of the formula A a Si b B c Cu d M e It represents that A is at least one of Ni and Co, M is at least one element selected from Nb, Mo, V, Zr, Hf and W, and in terms of atomic %, 72.0≤a≤81.0, 9.0≤b≤17.0, 5.0≤c≤10.0, 0.02≤d≤1.2, 0.1≤e≤3.5, 0≤x≤0.1,
[0034] When the amorphous alloy thin strip contacts the heating body and is heated, the amorphous alloy thin strip is conveyed, and a thin strip pressing member contacts the surface of the amorphous alloy thin strip opposite to the surface in contact with the heating body, and the amorphous alloy thin strip is heated while being pressed against the heating body.
[0035] When the bccFe crystallization start temperature of the amorphous alloy ribbon measured at a heating rate of 20 K / min is defined as Tx1°C, the heater is heated to a heating temperature Ta of Tx1+80°C or higher and Tx1+230°C or lower.
[0036] In the method for producing a magnetic sheet according to the second aspect of the present disclosure, a nanocrystalline alloy thin strip obtained by the method for producing a nanocrystalline alloy thin strip according to the first aspect and an adhesive layer having a support body formed in a strip shape and an adhesive provided on at least one of a first surface and a second surface of the support body are prepared.
[0037] The nanocrystalline alloy ribbon and the adhesive layer are continuously guided to an attaching roller, and the nanocrystalline alloy ribbon and the adhesive layer are bonded to each other by the attaching roller.
[0038] Effects of the Invention
[0039] According to the present disclosure, a nanocrystalline alloy ribbon having excellent magnetic properties of high saturation magnetic flux density and high magnetic permeability can be obtained by continuously heat treating the ribbon. In addition, a nanocrystalline alloy ribbon having low magnetostriction, low loss and isotropy can be obtained. In addition, a nanocrystalline alloy ribbon having high space factor and suppressing wrinkles and stripes can be obtained. In addition, a soft magnetic sheet using the same can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 This is a conceptual diagram showing one embodiment of the heat treatment method disclosed in the present invention.
[0041] Figure 2 This is a conceptual diagram showing another embodiment of the heat treatment method disclosed in the present invention.
[0042] Figure 3 This is a conceptual diagram showing another embodiment of the heat treatment method disclosed in the present invention.
[0043] Figure 4 This is a laser microscope photograph of the wrinkle height of Sample No. 10 of the present disclosure evaluated.
[0044] Figure 5 This is a laser microscope photograph of the wrinkle height of Sample No. 16 of the present disclosure evaluated.
[0045] Figure 6 This is a laser microscope photograph of the wrinkle height of Sample No. 17 of the present disclosure evaluated.
[0046] Figure 7 This is a laser microscope photograph of the wrinkle height of Sample No. 18 of the present disclosure evaluated.
[0047] Figure 8 This is an example of a temperature profile during heat treatment of the present disclosure.
[0048] Fig. 9 This is an example of a temperature profile during heat treatment of the present disclosure.
[0049] Fig.10It is a schematic diagram explaining the manufacturing method of the magnetic sheet of this disclosure.
[0050] Fig.11 It is a cross-sectional view explaining the structure of the laminated body supplied from the first delivery roll.
[0051] Fig.12 This is a cross-sectional view for explaining the structure of the laminated body from which the resin sheet is fed and peeled off from the first delivery roll.
[0052] Fig.13 It is a cross-sectional view illustrating the structure of the nanocrystalline alloy ribbon supplied from the second unwinding roll.
[0053] Fig.14 It is a cross-sectional view explaining a state where a nanocrystalline alloy thin strip is bonded to an adhesive layer by a bonding roller.
[0054] Fig.15 This is a cross-sectional view illustrating a state in which cracks are formed in a nanocrystalline alloy ribbon by a cracking roller.
[0055] Fig.16 is a cross-sectional view illustrating the magnetic sheet of the present disclosure. DETAILED DESCRIPTION
[0056] Hereinafter, embodiments of the present disclosure will be described in detail. The present disclosure is not limited to the following embodiments at all, and can be implemented by appropriately adding modifications within the scope of the present disclosure.
[0057] In the present disclosure, the numerical range represented by "to" represents a range including the numerical values recorded before and after "to" as the lower limit and upper limit, respectively. In the numerical range recorded in stages in the present disclosure, the upper limit or lower limit recorded in a certain numerical range may also be replaced by the upper limit or lower limit of the numerical range recorded in other stages. In addition, in the numerical range recorded in the present disclosure, the upper limit or lower limit recorded in a certain numerical range may also be replaced by the value shown in the embodiment.
[0058] In the present disclosure, a combination of two or more preferred aspects is a more preferred aspect.
[0059] The nanocrystalline alloy ribbon disclosed in the present invention is composed of a composition formula (Fe 1-x A x ) a Si b B c Cu d M eIt means that A is at least one of Ni and Co, M is at least one element selected from Nb, Mo, V, Zr, Hf and W, and in atomic % 72.0≤a≤81.0, 9.0≤b≤17.0, 5.0≤c≤10.0, 0.02≤d≤1.2, 0.1≤e≤3.5, and 0≤x≤0.1.
[0060] The composition of the nanocrystalline alloy ribbon disclosed in the present invention is described in detail below.
[0061] The content of Fe (iron) is 72.0% or more and 81.0% or less in atomic %.
[0062] A high saturation magnetic flux density can be obtained by making the Fe content 72.0% or more. It is preferably 73% or more, more preferably 75.0% or more, more preferably 76% or more, and more preferably 77% or more. It should be noted that when it is desired to obtain a saturation magnetic flux density of 1.36T or more, the Fe content is preferably 75.0% or more.
[0063] When the Fe content exceeds 81.0%, it becomes difficult to reduce magnetostriction, so the Fe content is made 81.0% or less, preferably 80% or less, and more preferably 78% or less.
[0064] In addition, part of Fe may be replaced by at least one element selected from Ni and Co. 1-x A x ), A is at least one of Ni and Co, and x is 0.1 or less. When part of Fe is replaced by at least one of Ni and Co, (Fe 1-x A x ) a The a represented by the formula is in the range of 72.0%≤a≤81.0%. (Fe 1-x A x The content a of ) is preferably 73% or more, more preferably 75.0% or more, more preferably 76% or more, and more preferably 77% or more. It is preferably 80% or less, and more preferably 78% or less.
[0065] The Si (silicon) content is 9.0% or more and 17.0% or less in atomic %.
[0066] By making the Si content 9.0% or more, low magnetostriction can be achieved. The Si content is preferably 10% or more, more preferably 13% or more, and more preferably 15% or more. When it exceeds 17.0%, the amorphous forming ability decreases, crystallization occurs during casting, and the soft magnetic properties are significantly reduced. It is preferably 16.5% or less.
[0067] The content of B (boron) is 5.0% or more and 10.0% or less in atomic %.
[0068] When the content of B is less than 5.0%, it becomes difficult to form an amorphous state, so the content of B is made 5.0% or more, preferably 5.5% or more, and more preferably 6.0% or more.
[0069] If the B content exceeds 10.0%, the Fe content and the Si content decrease, so the saturation magnetic flux density decreases and the magnetostriction increases. Therefore, the B content is set to 10.0% or less, preferably 8.5% or less, more preferably 7.5% or less, and even more preferably 7.0% or less.
[0070] The content of Cu (copper) is 0.02% or more and 1.2% or less in atomic %.
[0071] By containing Cu, it is easy to obtain a uniform and fine nanocrystalline structure. When the Cu content is less than 0.02%, it is difficult to make the average particle size less than 50nm. Therefore, the Cu content is set to 0.02% or more. Preferably, it is 0.05% or more, preferably 0.2% or more, preferably 0.3% or more, and more preferably 0.5% or more.
[0072] If the Cu content exceeds 1.2%, the steel tends to become brittle and the saturation magnetic flux density decreases. Therefore, the Cu content is 1.2% or less, preferably 1.0% or less, more preferably 0.75% or less, and further preferably 0.65% or less.
[0073] The M element is at least one selected from the group consisting of Nb, Mo, V, Zr, Hf, and W, and the content of the M element is 0.1% to 3.5% in atomic %.
[0074] Nanocrystalline alloy ribbons contain M elements, which can shift the precipitation start temperature of FeB compounds with significantly degraded soft magnetic properties to the high temperature side. As a result, the difference between the crystallization start temperature of bccFe (αFe) and the precipitation start temperature of FeB can be expanded, and the range of the optimal heat treatment temperature can be expanded, and the heat treatment conditions can be relaxed. The content of M elements is preferably 0.3% or more, and more preferably 0.4% or more.
[0075] The M element is expensive, so if the content of the M element increases, the price of the nanocrystalline alloy ribbon will increase. Therefore, it is preferred that the content is small. Therefore, the content of the M element is set to 3.5% or less. It is preferably 1.5% or less, more preferably 1.0% or less, more preferably 0.9% or less, more preferably 0.8% or less, and more preferably 0.7% or less.
[0076] The nanocrystalline alloy ribbon disclosed in the present invention may also contain C (carbon). C has the effect of improving the melt fluidity of the melt, and improves castability by containing a trace amount. On the other hand, when added in large quantities, the ribbon becomes brittle, so the C content is preferably less than 1% by mass. In addition, C can be contained as an impurity of the raw material. The lower the amount of C, the higher the price of the raw material, so it is preferably allowed to be more than 0.01% by mass. It should be noted that in order to improve the effect of C, the C content is preferably more than 0.1% by mass.
[0077] Furthermore, the nanocrystalline alloy ribbon disclosed herein may contain impurities other than the above-mentioned elements.
[0078] As impurities, for example, S (sulfur), O (oxygen), N (nitrogen), Cr, Mn, P, Ti, Al, etc. can be listed. For example, the content of S is preferably 200 mass ppm or less, the content of O is preferably 5000 mass ppm or less, and the content of N is preferably 1000 mass ppm or less. The content of P is preferably 2000 mass ppm or less. The total content of these impurities is preferably 0.5 mass % or less. In addition, if it is within the above range, an element equivalent to the impurity can be added.
[0079] The method for producing the nanocrystalline alloy ribbon disclosed in the present invention will be described.
[0080] For the nanocrystalline alloy ribbon disclosed in the present invention, the alloy melt having the above-mentioned alloy composition is sprayed onto a rotating cooling roller, and rapidly solidified on the cooling roller to obtain an alloy ribbon. Then, by heat treating the alloy ribbon, the nanocrystalline alloy ribbon disclosed in the present invention can be obtained. The alloy ribbon obtained by rapidly solidifying the alloy melt becomes an alloy structure in an amorphous state, becoming an amorphous alloy ribbon. By heat treating the amorphous alloy ribbon, a nanocrystalline alloy ribbon can be obtained. It should be noted that the amorphous alloy ribbon obtained by rapidly solidifying the alloy melt may also have a crystalline phase composed of fine crystals.
[0081] In order to obtain a molten alloy, various materials, i.e., various element sources (pure iron, ferroboron, ferrosilicon, etc.) for making a target alloy composition can be combined. In addition, the various materials are heated in an induction heating furnace to a temperature above the melting point, thereby melting to form a molten alloy.
[0082] The alloy strip can be obtained by ejecting the alloy melt from a slit-shaped nozzle of a predetermined shape onto a rotating cooling roller, and rapidly solidifying the alloy melt on the cooling roller. It should be noted that the outer diameter of the cooling roller can be 350 to 1000 mm, the width can be 100 to 400 mm, and the circumferential speed of rotation can be 20 to 35 m / s. The cooling roller is internally provided with a cooling mechanism (water cooling, etc.) for suppressing the temperature rise of the outer periphery.
[0083] In addition, the outer periphery of the cooling roller is preferably composed of a Cu alloy having a thermal conductivity of 120 W / (m·K) or more. By setting the thermal conductivity of the outer periphery to 120 W / (m·K) or more, the cooling rate of the alloy melt when casting the alloy strip can be increased. As a result, the embrittlement of the alloy strip can be suppressed, the thickness of the alloy strip can be increased (the thickness can be increased), and the surface crystallization during casting can be suppressed. Therefore, the coarsening of grains during heat treatment can be suppressed, and the iron loss can be reduced.
[0084] The thermal conductivity of the outer peripheral portion of the cooling roller is preferably 150 W / (m·K) or more, and more preferably 180 W / (m·K) or more.
[0085] It should be noted that the outer peripheral portion of the cooling roll refers to the portion that can be in contact with the molten alloy, and the thickness thereof may be about 5 to 15 mm, and a structural material that maintains the roll structure may be used inside the outer peripheral portion.
[0086] The amorphous alloy ribbon produced by the above-mentioned rapid cooling method (a method of rapidly cooling an alloy melt to produce an alloy ribbon) is subjected to heat treatment to produce a nanocrystalline alloy ribbon. The method for producing a nanocrystalline alloy ribbon disclosed in the present invention is characterized in that the heat treatment method is used.
[0087] The heat treatment method disclosed in the present invention is a method for heating an amorphous alloy thin strip by contacting it with a heating body. When the amorphous alloy thin strip is heated by contacting it with a heating body, the amorphous alloy thin strip is conveyed, and the amorphous alloy thin strip is heated by being pressed against the heating body by a thin strip pressing member that contacts the opposite surface of the amorphous alloy thin strip that contacts the heating body.
[0088] In the present disclosure, when the heating rate of the amorphous alloy ribbon is set to 20K / min and the measured bccFe crystallization start temperature is set to Tx1°C, the above-mentioned heating body is heated to a heating temperature Ta of Tx1+80°C or more and Tx1+230°C or less. Preferably, the heating body is heated to Tx1+100°C or more. Moreover, when the amorphous alloy ribbon is heated, the heating rate of the amorphous alloy ribbon is preferably 15000°C / min. or more.
[0089] In the heat treatment of the present disclosure, the contact time (holding time) between the amorphous alloy thin strip and the heating body is preferably 0.1 seconds to 30 seconds.
[0090] During the heat treatment, the magnetic permeability, B80 and L / B80 W and other characteristics.
[0091] In the present disclosure, a soft member may be used as the ribbon pressing member to form a state in which the amorphous alloy ribbon is pressed against the heating body.
[0092] As the soft member, a metal member is preferred. It should be noted that the soft member refers to a member that can be deformed along the roller. In addition, the thin strip pressing member can also be a belt or a roller.
[0093] An example of the heat treatment method of the present disclosure will be described.
[0094] Figure 1 This is a conceptual diagram showing one embodiment of the heat treatment method disclosed in the present invention.
[0095] exist Figure 1 The structure used in the heat treatment method shown in the figure includes: a heating roller 2 serving as a heating body, a thin strip pressing metal belt 3 (thin strip pressing member), a roller 4 supporting the thin strip pressing metal belt 3, and a roller 5. The thin strip pressing metal belt 3 is an example of a structure in a state where an amorphous alloy thin strip (hereinafter also referred to as a thin strip) 1 is pressed against the heating roller 2 serving as a heating body.
[0096] In the heat treatment method, the amorphous alloy thin strip 1 is passed between the heating roller 2 (heating body) and the thin strip pressing metal belt 3, and the thin strip 1 is heated while being pressed against the heating body (heating roller 2). Figure 1 The arrows in show the operation of each part. The heating roller 2, the roller 4, and the roller 5 are cylindrical and rotate. Thus, the amorphous alloy thin strip 1 is conveyed and heated while being pressed against the heating roller 2.
[0097] Here, the ribbon 1 heated by the heating roller 2 becomes a nanocrystalline alloy ribbon.
[0098] In addition, it is preferable to use a heating roller that can also heat the rollers 4 and 5. Therefore, it is preferable to preheat the metal belt 3 pressing the thin strip before contacting the thin strip 1. In the case where the rollers 4 and 5 are used as heating rollers, it is preferable to set the temperature of the metal belt 3 pressing the thin strip (the temperature when in contact with the thin strip 1) to be equal to or slightly lower than the heating temperature of the thin strip 1. The temperature of the rollers 4 and 5 can be set to a temperature appropriate for the temperature of the metal belt 3 pressing the thin strip. For example, it is also preferable to set the temperature of the rollers 4 and 5 to be about 50°C higher than the temperature of the heating body. The temperature of the metal belt 3 pressing the thin strip, the rollers 4 and 5 can be selected to be a temperature suitable for the heat treatment of the thin strip 1.
[0099] The thin strip pressing metal belt 3 is an example of a soft member, and from the viewpoint of flexibility and strength, the soft member is preferably a metal member. For example, it is more preferable to use a material having excellent heat resistance, such as heat-resistant stainless steel and nickel-based super heat-resistant alloy.
[0100] According to the above heat treatment method, a structure is formed in which a soft member (strip pressing metal belt 3) is pressed against the opposite surface of the surface of the amorphous alloy strip 1 that contacts the heating body, thereby the amorphous alloy strip 1 is pressed against the heating body (heating roller 2). It should be noted that it is preferred that the amorphous alloy strip 1 is in close contact with the heating roller 2 through the strip pressing metal belt 3, and the amorphous alloy strip 1, the strip pressing metal belt 3 and the heating roller 2 perform an integrated operation.
[0101] Here, the heating roller 2 is a heating body (heating body disclosed in the present invention) for directly contacting and heating the amorphous alloy thin strip 1. The amorphous alloy thin strip 1 is in contact with a portion of the outer peripheral surface (a portion of the circumferential area) of the cylindrical heating roller 2 and is heated. The heating roller 2 can also have a conveying driving force for the amorphous alloy thin strip. The roller used to drive the thin strip to press the metal strip 3 can be both roller 4 and roller 5, or either one. It can also be configured so that roller 5 has a driving force and roller 4 is mechanically subordinate. In this way, complex control such as the electrical synchronous operation of rollers 4 and 5 can be avoided, and there is no need to correct the synchronization deviation caused by the thermal expansion difference between rollers 4 and 5.
[0102] It should be noted that the heating roller 2 is an example of a heating body having a convex surface for contacting and heating the amorphous alloy thin strip 1. In addition, the "convex surface" refers to a surface that is raised on the side of the amorphous alloy thin strip 1. For example, the heating roller 2 may also be as follows: Figure 1 As long as the amorphous alloy ribbon follows and ensures sufficient contact, the heating body of the present disclosure may be a non-rotating structure or a structure in which the ribbon moves (slides) on the heating body.
[0103] Figure 2 This is a conceptual diagram showing another embodiment of the heat treatment method disclosed in the present invention.
[0104] exist Figure 2 The structure used in the heat treatment method shown in the figure includes a heating roller 2 as a heating body and thin strip pressing rollers 6, 7, and 8. The thin strip pressing rollers 6, 7, and 8 function as thin strip pressing members that press the amorphous alloy thin strip 1 against the heating roller 2. Figure 2 In the heat treatment method shown, the ribbon 1 is passed between the heating roller 2 (heating body) and the ribbon pressing rollers 6, 7, 8, so that the ribbon 1 is pressed against the heating body (heating roller 2), and the ribbon 1 is heated. Figure 2The arrows in the figure indicate the actions of each part, and the heating roller 2 and the ribbon pressing rollers 6, 7, and 8 are cylindrical and rotate. Thus, the amorphous alloy ribbon 1 is conveyed and heated while being pressed against the heating roller 2. It should be noted that the ribbon pressing rollers 6, 7, and 8 are preferably heated rollers that can be heated.
[0105] Figure 3 This is a conceptual diagram showing another embodiment of the heat treatment method disclosed in the present invention.
[0106] exist Figure 3 In the heat treatment method shown in the figure, instead of Figure 1 The heating roller 2 is provided with a substantially D-shaped heating body 32, and as a structure in which the amorphous alloy thin strip 1 is pressed against the heating body 32, a thin strip pressing metal belt 33 and rollers 34 and 35 supporting the thin strip pressing metal belt 33 are provided. Figure 3 In the heat treatment method shown, the thin strip 1 is passed between the heating body 32 and the thin strip pressing metal belt 33 (thin strip pressing member), and the thin strip 1 is heated while being pressed against the heating body 32 . Figure 3 The arrows in the figure indicate the actions of each part, and the rollers 34 and 35 are cylindrical and rotate. Thus, the amorphous alloy thin strip 1 is conveyed and heated while being pressed against the heating body 32. Here, the amorphous alloy thin strip 1 slides on the heating body 32. It should be noted that it is preferable to use a heating roller that can also heat the rollers 34 and 35. Therefore, it is preferable to preheat the thin strip to press the metal strip 33.
[0107] like Figure 1 , Figure 2 , Figure 3 As shown, when the amorphous alloy strip 1 is brought into contact with the heating body for heating, the amorphous alloy strip 1 can be heated while being conveyed and pressed against the heating body by the strip pressing member.
[0108] At this time, the heating rate of the amorphous alloy ribbon 1 is preferably 15000° C. / min. or higher. In addition, it is more preferable to set the heating rate of the amorphous alloy ribbon 1 to 30000° C. / min. or higher.
[0109] In the case of obtaining a nanocrystalline alloy ribbon by heat treatment, in order to achieve a fine nanocrystalline structure, the appropriate heating rate varies according to the composition. For example, the composition of the amorphous alloy ribbon 1 is low Cu (less Cu content), low M element (less M element content), and high Fe (more Fe content) composition that can obtain a high saturation magnetic flux density, the faster the heating rate is required. In the case of the composition disclosed in the present invention, the lower limit of the heating rate is 15000℃ / min., and the upper limit can be determined according to the equipment capacity of the heat treatment device, the temperature of the heating body and the ribbon pressing member, the contact state between the heating body and the ribbon pressing member and the ribbon, etc. However, the actual upper limit of the heating rate is about 240000℃ / min. It is preferably 100000℃ / min.
[0110] The heating body preferably has a width wider than the width of the amorphous alloy strip 1. Thus, when the amorphous alloy strip 1 is pressed against the heating body, the entire width of the strip 1 is in close contact with the heating body. In addition, the strip pressing member also preferably has a width wider than the width of the amorphous alloy strip 1. Thus, when the amorphous alloy strip 1 is pressed against the heating body, the entire width of the strip 1 is easily in close contact with the heating body. It should be noted that the direction in which the amorphous alloy strip 1 is conveyed is referred to as the length direction, and the length in the length direction is referred to as the length. In addition, the direction orthogonal to the length direction is referred to as the width direction, and the length in the width direction is referred to as the width.
[0111] In addition, when the amorphous alloy thin strip 1 is heated while being pressed against the heating body, the distance from the contact of the amorphous alloy thin strip 1 with the heating body to the separation is preferably 50 mm or more in the length of the heating body surface. In addition, the distance from the contact of the amorphous alloy thin strip with the heating body to the separation is more preferably 150 mm or more in the length of the heating body surface.
[0112] The conveying speed of the amorphous alloy ribbon 1 is preferably 1 m / min or more. When mass-producing nanocrystalline alloy ribbons, the higher the conveying speed, the higher the production volume, so the conveying speed is more preferably 10 m / min or more.
[0113] The contact time between the amorphous alloy thin strip 1 and the heating body is preferably 0.1 to 30 seconds. The lower limit of the contact time is more preferably 0.2 seconds, the upper limit of the contact time is more preferably 10 seconds, further more preferably 5 seconds, and most preferably 2 seconds. In order to improve mass production, in the case of high speed and stabilization, the contact time is preferably set within the range of 0.2 to 2 seconds.
[0114] According to the heat treatment method disclosed in the present invention, by forming a state where the amorphous alloy strip 1 is pressed against a heating body, the heating body and the strip 1 are in good contact, the heat transfer from the heating body to the strip 1 is improved, and the heating rate of the strip 1 becomes faster. In addition, the heat generated by crystallization can be released more to the heating body and the strip pressing member (belt, roller). Therefore, the maximum temperature of the strip 1 can be suppressed (the temperature rise caused by self-heating can be suppressed). Furthermore, a state where the strip 1 is pressed by the strip pressing member (belt, roller) can be formed, so the generation of wrinkles or stripes that are easy to occur during crystallization can be suppressed. Thus, heat treatment at a higher temperature can be performed, and heat treatment using a fast heating rate and short contact time can be performed. Therefore, productivity can be improved and a uniform nanocrystalline structure can be obtained, and a nanocrystalline alloy strip with a higher saturation magnetic flux density and excellent magnetic properties can be obtained.
[0115] [Temperature increase rate of amorphous alloy ribbon during heat treatment]
[0116] The inventors confirmed the temperature increase rate of the amorphous alloy ribbon during heat treatment by the following method.
[0117] The surface temperature of the amorphous alloy thin strip was measured using a radiation thermometer FLHX-TNE0090 manufactured by Nippon Sensor Co., Ltd. This radiation thermometer can only perform fixed-point measurement, so the temperature measurement of the amorphous alloy thin strip 1 during heat treatment was carried out without conveying the thin strip 1. Figure 3 The method shown is configured as follows: the thin strip pressing metal belt 33 is not driven, the thin strip 1 is arranged between the thin strip pressing metal belt 33 and the heating body 32, and tension is applied to the thin strip pressing metal belt 33 to press the thin strip 1 against the heating body 32. In addition, the heating body 32 is a mechanism that rises and falls, and the heating body 32 is lowered to heat the thin strip 1 without contacting the thin strip 1. Then, after the heating body 32 reaches the specified heat treatment temperature, the heating body 32 is raised, and the thin strip 1 is pressed toward the heating body 32 side by the metal belt 33, and the temperature of the thin strip 1 is measured. In this way, the temperature change of the thin strip 1 after being pressed against the heating body is confirmed.
[0118] Figure 8 The temperature curve of an example measured when the temperature of the heating body 32 is set to 620° C. is shown. Fig. 9 The temperature curve of an example measured with the temperature of the heating body 32 set to 640°C is shown. The X-axis is time (seconds), and the Y-axis is the measured temperature of the thin strip 1. The thin strip 1 is pressed against the heating body 32 heated to the set temperature (620°C, 640°C) by the above method for measurement. Figure 8 , Fig. 9The contact time indicated by the arrow parallel to the X axis in FIG. 1 is the time when the thin strip 1 is pressed against the heating body 32. According to this measurement method, the temperature of the thin strip 1 rises to about 450°C before contacting the heating body 32. Therefore, the heating rate is determined by Figure 8 , Fig. 9 The arrow parallel to the Y axis in the figure indicates the heating rate. The heating rate is calculated as the temperature change from the moment when the thin strip 1 contacts the heating body 32 to the moment when the set temperature is reached divided by the time. It should be noted that the temperature of the thin strip 1 is measured by opening a hole for measurement on the metal strip 33 where the thin strip is pressed. In fact, since the metal strip 33 presses the thin strip 1 during the heat treatment, it can be inferred that the temperature of the thin strip 1 is higher than that of the metal strip 33. Figure 8 , Fig. 9 The heating rate of the temperature rise is fast, but it cannot be measured, so the heating rate of each condition is not determined. Figure 8 , Fig. 9 Since the heating rate at the set temperature of 620°C was 1240°C / sec. (74400°C / min.), and the heating rate at 640°C was 1280°C / sec. (76800°C / min.), it can be confirmed that it is above 15000°C / min.
[0119] Next, the pressure with which the amorphous alloy thin strip 1 is pressed against the heating body is preferably 0.03 MPa or more, more preferably 0.05 MPa or more, and even more preferably 0.07 MPa or more.
[0120] In order to further optimize the contact state between the amorphous alloy thin strip 1 and the heater, it is also effective to provide the heater with a curvature. The curvature of the heater preferably has a radius of curvature of 25 mm or more.
[0121] In order to speed up the heating rate of the amorphous alloy thin strip 1, it is effective to heat the thin strip pressing member (belt, roller) to the same temperature as the heating body. Figure 1 , Figure 2 , Figure 3 In the embodiment, heated rollers are used as rollers 4, 5, 6, 7, 8, 34 and 35. In order to suppress heat generation due to crystallization of bccFe of the ribbon, it is effective to set the temperature of the ribbon and rollers lower than the heating plate temperature Ta°C.
[0122] According to the present disclosure, a nanocrystalline alloy ribbon having excellent magnetic properties and isotropy can be obtained. In addition, a nanocrystalline alloy ribbon having high space factor and suppressing wrinkles and streaks can be obtained.
[0123] The saturation magnetic flux density Bs of the nanocrystalline alloy ribbon disclosed herein is 1.15 T or more, more preferably 1.20 T or more, more preferably 1.35 T or more, more preferably 1.36 T or more, more preferably 1.37 T or more, and more preferably 1.40 T or more.
[0124] In addition, the nanocrystalline alloy ribbon disclosed in the present invention preferably has a residual magnetic flux density Br and a magnetic flux density B of 8000A / m magnetic field. 8000 The ratio of Br / B 8000 It is 0.20 or more. In addition, the maximum magnetic permeability is preferably 4000 or more. In addition, the maximum magnetic permeability is preferably 5000 or more.
[0125] In addition, the nanocrystalline alloy ribbon of the present invention preferably has a magnetic flux density B80 when a magnetic field of 80 A / m is applied along the length direction of the nanocrystalline alloy ribbon. L The magnetic flux density B80 when a magnetic field of 80A / m is applied in the width direction perpendicular to the length direction W The ratio (B80 L / B80 W ) is 0.60~1.40, and B80 L 、B80 W All are above 0.4T. L / B80 W ) is more preferably 0.70 to 1.30. L 、B80 W Both are more preferably 0.5T or more.
[0126] The space factor of the nanocrystalline alloy ribbon disclosed in the present invention is preferably 68.0% or more, preferably 70% or more, and more preferably 75% or more.
[0127] In addition, the space factor can be measured by the following method based on JIS C 2534:2017.
[0128] 20 nanocrystalline alloy ribbons cut into lengths of 120 mm were stacked and placed on a flat sample table. A flat anvil with a diameter of 16 mm was placed on the stacked ribbons at a pressure of 50 kPa, and the height was measured at intervals of 10 mm along the width direction. The maximum height at this time was set as hmax (μm), and the duty cycle LF was calculated according to the following calculation formula.
[0129] LF(%)=sample weight(g) / density(g / cm 3 ) / hmax(μm) / sample length(240cm) / strip width(cm)×10000
[0130] At this time, the density (g / cm3 ) is the density of the alloy strip after heat treatment. The density can be 7.4 g / cm 3 .
[0131] When the amorphous alloy strip 1 is made into a nanocrystalline alloy strip by making it contact with a heating body and heating, if there are local differences in the heating rate and temperature of the amorphous alloy strip 1 due to the contact deviation between the amorphous alloy strip 1 and the heating body, the progress of crystallization will also be different. As a result, local strain is generated, and there is a problem that a part of the strip 1 floats from the heating body. In the floating part, it is difficult to release the self-heating caused by crystallization to the heating body, and the temperature of the strip 1 rises sharply to reach the FeB precipitation temperature, which is easy to form wrinkles or stripes. As a result, the duty cycle is reduced. In addition, the wrinkles or stripes become very brittle, which may cause problems in handling such as the breakage of the nanocrystalline alloy strip during transportation and stacking, and deterioration of magnetic properties.
[0132] According to the present disclosure, the amorphous alloy strip 1 is pressed against the heating body by a strip pressing member that contacts the opposite surface of the amorphous alloy strip 1 that contacts the heating body. Therefore, the amorphous alloy strip 1 can be heated evenly, and the floating of the alloy strip can be suppressed, and the generation of wrinkles or streaks can be suppressed. Moreover, in the present disclosure, there is also an effect of correcting wrinkles and the like generated by cooling deviation during the casting of the amorphous alloy strip 1. According to the present disclosure, wrinkles or streaks can be suppressed, and a nanocrystalline alloy strip with good flatness can be obtained.
[0133] The wrinkle height of the nanocrystalline alloy ribbon disclosed herein is preferably 0.15 mm or less, more preferably 0.10 mm or less, and further preferably 0.08 mm or less. The wrinkle height is the height of wrinkles or stripes, and can be evaluated by the method described in the following examples.
[0134] The thickness of the nanocrystalline alloy ribbon disclosed in the present invention is preferably 25 μm or less, more preferably 20 μm or less. In addition, the thickness is preferably 5 μm or more, more preferably 10 μm or more. The width is preferably 5 mm or more, more preferably 20 mm or more, and more preferably 30 mm or more.
[0135] In addition, if the width of the nanocrystalline alloy ribbon of the present disclosure is too wide, it is difficult to achieve stable production, so the width is preferably 500 mm or less, and more preferably 400 mm or less.
[0136] The nanocrystalline alloy ribbon disclosed in the present invention can be used for magnetic cores, magnetic shielding materials, and the like used in electronic components, motors, and the like, thereby obtaining magnetic cores and magnetic shielding materials having excellent characteristics.
[0137] The nanocrystalline alloy ribbon disclosed in the present invention can constitute a magnetic sheet that can be used as a magnetic sheet for contactless charging, for example.
[0138] [Example 1]
[0139] In Example 1, the alloy composition is Fe 76.4 Si 16 B 6.5 Cu 0.6 Nb 0.5 The element source is combined in a manner, heated to 1350°C to produce an alloy melt, and the alloy melt is ejected onto a cooling roller with an outer diameter of 400mm and a width of 200mm rotating at a peripheral speed of 30m / sec, and rapidly solidified on the cooling roller to produce an amorphous alloy thin strip. It should be noted that the outer periphery of the cooling roller is composed of a Cu alloy with a thermal conductivity of 150W / (m·K), and a cooling mechanism for controlling the temperature of the outer periphery is provided inside.
[0140] A sample (Comparative Example 1) was prepared by heat treating the amorphous alloy thin strip at a heating rate of 6°C / min., a heat treatment temperature of 470°C, and a holding time of 1 hour, and a sample (Example 1) was prepared by heat treating the amorphous alloy thin strip at a heating rate of 79200°C / min., a heat treatment temperature of 660°C, and a holding time of 1.2 seconds. It should be noted that the heat treatment in Example 1 was performed using Figure 1 The heat treatment method shown. It should be noted that the samples of Example 1 and Comparative Example 1 after heat treatment are nanocrystalline alloy strips. It should be noted that the heat treatment temperature of Example 1 is the heating temperature of the heating body. In addition, Tx1 of the alloy composition (the same as No. 10 in Table 2) is 468.5°C. The heating temperature Ta of the heating body of Example 1 is Tx1+191.5°C.
[0141] In addition, the nanocrystalline alloy ribbons of Example 1 and Comparative Example 1 had a width of 50 mm and a thickness of 16.4 μm.
[0142] For Example 1 and Comparative Example 1, the average grain size, iron loss at 20 kHz and 0.2 T, Br / B 8000 The maximum magnetic permeability is shown in Table 1. 8000 (Bs) is equivalent to 1.41T. In Example 1, by setting the heating rate to 15000°C / min. or more, the average crystal grain size can be made 50nm or less. In addition, the iron loss at 20kHz and 0.2T is also excellent, being 10W / kg or less. In addition, Br / B 8000 The value is 0.20 or more, and the maximum magnetic permeability is 4000 or more. In Example 1, a nanocrystalline alloy ribbon having high saturation magnetic flux density, low loss, and high magnetic permeability can be realized. It should be noted that the measurement method is described in Example 2.
[0143] [Table 1]
[0144]
[0145] [Example 2]
[0146] In Example 2, the element sources were mixed in such a manner as to form the compositions shown in Table 2, and the alloy melt was prepared by heating to 1350°C. The alloy melt was ejected onto a cooling roller having an outer diameter of 400 mm and a width of 200 mm rotating at a peripheral speed of 30 m / sec, and rapidly solidified on the cooling roller to prepare an amorphous alloy ribbon. The width and thickness of the amorphous alloy ribbon are shown in Table 3. In addition, the outer periphery of the cooling roller is composed of a Cu alloy having a thermal conductivity of 150 W / (m·K), and a cooling mechanism for controlling the temperature of the outer periphery is provided inside.
[0147] The amorphous alloy ribbons of various materials shown in Table 2 were heat treated under the conditions of Table 3 (heating rate, heating temperature of the heating body, pressure of pressing the amorphous alloy ribbon on the heating body: pressing pressure, holding time). The evaluation results are shown in Tables 3 and 4. In addition, blank columns in the table are not measured.
[0148] [Table 2]
[0149]
[0150] [Table 3]
[0151]
[0152] [Table 4]
[0153]
[0154] [Average grain size]
[0155] The average crystal grain size is obtained by using the integrated width of the diffraction peak from the (110) plane in the X-ray diffraction pattern obtained by the X-ray diffraction experiment, and is obtained by the Scherrer formula. The integrated width of the diffraction peak from the (110) plane is obtained by peak decomposition using the pseudo-Voigt function for the diffraction pattern. If the average grain size is set to D, the integrated width is set to β, the diffraction angle is set to θ, the Scherrer constant is set to K, and the wavelength of the X-ray is set to λ, D is obtained according to the Scherrer formula (Formula 1) given below. However, in this case, it is assumed that the wavelength of the X-ray is λ = 0.154050nm and the Scherrer constant K = 1.333.
[0156] In addition, as the integral width, a value corrected so that the integral width becomes narrower by the amount of spread of the diffraction line width from the device is used.
[0157] [Number 1]
[0158]
[0159] [Volume rate]
[0160] The volume ratio is the volume ratio of the nanocrystals, and the portion other than the nanocrystals is an amorphous portion.
[0161] The volume fraction is obtained by the ratio of the integrated intensity of the diffraction peak from the (110) plane of Fe to the integrated intensity of the halo pattern. The integrated intensity of the halo pattern is the integrated intensity of the diffraction peak from the (110) plane of Fe + the integrated intensity near 2θ=44°. The integrated intensity of the peak shown by the nanocrystal and the halo pattern shown by the amorphous are obtained by peak decomposition using the pseudo-Voigt function for the X-ray diffraction pattern. If the integrated intensity of the (110) peak of the nanocrystal is set to Ic and the integrated intensity of the halo pattern near 2θ=44° is set to Ia, the volume fraction V is calculated according to the formula (number 2) given below. However, in the case of the composition in this embodiment, the peaks of the integrated intensities of Fe and Fe2B overlap and are difficult to distinguish, so Ic and Ia may also include the integrated intensity of trace precipitated Fe2B.
[0162] [Number 2]
[0163]
[0164] [Saturation magnetic flux density Bs]
[0165] The saturation magnetic flux density Bs is obtained by applying a 8000A / m magnetic field to the nanocrystalline alloy ribbon (single plate sample) after heat treatment using a DC magnetization characteristic test device manufactured by Metron Technology Co., Ltd. and measuring the maximum magnetic flux density at this time. The nanocrystalline alloy ribbon disclosed in the present invention has the characteristic of being easy to saturate, so it will reach saturation when the 8000A / m magnetic field is applied. 8000 Since it is approximately the same value as the saturation magnetic flux density Bs, B is used 8000 Indicates the saturation magnetic flux density Bs.
[0166] [Maximum magnetic permeability]
[0167] Regarding the maximum magnetic permeability, a DC magnetization characteristic testing device manufactured by Metron Giken Co., Ltd. was used to apply a magnetic field of 800 A / m to the nanocrystalline alloy strip (single plate sample) after heat treatment, and the magnetic permeability relative to the magnetic field H at this time was measured. The maximum magnetic permeability was applied at this time.
[0168] [Magnetic flux density B80]
[0169] In a DC magnetization characteristic test device manufactured by Metron Technology Co., Ltd., a magnetic field of 80 A / m was applied in the length direction (casting direction) and the width direction orthogonal to the length direction of the nanocrystalline alloy thin strip, and the maximum magnetic flux density at this time was set as B80 L 、B80 W Then, calculate the ratio B80 L / B80 W , for isotropic evaluation.
[0170] [Saturation magnetostriction]
[0171] A 5 kOe magnetic field was applied to a sample (nanocrystalline alloy ribbon) with a strain gauge made by Kyowa Electric Co., Ltd. attached by an electromagnet. Then, the electromagnet was rotated 360°, and the maximum change in the elongation and contraction of the sample when the direction of the magnetic field applied to the sample was changed by 360° was measured based on the change in the resistance value of the strain gauge. Saturation magnetostriction = 2 / 3 × maximum change.
[0172] [Wrinkle height]
[0173] The wrinkle height is the height of the stripes and wrinkles formed on the surface of the thin strip. The height of the thin strip surface was measured by a KEYENCE laser microscope VR3200 when the nanocrystalline alloy thin strip was sandwiched between glass plates, and the difference between the maximum and minimum values was calculated as the wrinkle height. The reason for sandwiching the nanocrystalline alloy thin strip between the glass plates is that if the thin strip is very thin and is only placed on the measuring table, the thin strip will partially float due to undulations, etc., affecting the measurement of the height, so the purpose is to minimize their influence.
[0174] [Magnetic flux density Br]
[0175] A magnetic field of 8000 A / m was applied to the nanocrystalline alloy ribbon (single plate sample) after the heat treatment using a DC magnetization characteristics tester manufactured by Metron Giken Co., Ltd., and the value of the magnetic flux density B when the magnetic field was 0 was defined as Br.
[0176] [Iron loss]
[0177] In the BH analyzer SY8218 manufactured by Iwasaki Communication Equipment Co., Ltd., a toroidal core with an inner diameter of 8.8 mm and an outer diameter of 19.9 mm was punched out from a 15-layer nanocrystalline alloy ribbon, placed in a housing, and the iron loss was measured. The measurement conditions were 15 turns of primary and secondary windings, a frequency of 20 kHz, and a magnetic flux density of 0.2 T.
[0178] [Example 3]
[0179] The evaluation results of the nanocrystalline alloy ribbon produced in Example 3 are shown in Table 5. In Example 3, when the amorphous alloy ribbon of the composition No. 10 of Example 2 was heat treated, the pressure of pressing the ribbon was changed to 0.019, 0.038, 0.058, and 0.086 MPa to produce a nanocrystalline alloy ribbon. In Example 3, by setting the pressure of pressing the ribbon to 0.03 MPa or more, a duty cycle of 68.0% or more was obtained. Laser microscope photographs of the wrinkle heights of No. 10, 16, 17, and 18 are respectively shown in Figure 4 , Figure 5 , Figure 6 , Figure 7 .
[0180] [Table 5]
[0181]
[0182] As described above, according to the present disclosure, a nanocrystalline alloy ribbon having a saturation magnetic flux density of 1.15 T or more and a maximum magnetic permeability of 4000 or more is obtained. In addition, the residual magnetic flux density Br and the magnetic flux density B at a magnetic field of 8000 A / m are obtained. 8000 The ratio of Br / B 8000 In addition, the ratio of the magnetic flux density B80L when a 80A / m magnetic field is applied along the length direction of the nanocrystalline alloy thin strip to the magnetic flux density B80W when a 80A / m magnetic field is applied along the width direction orthogonal to the length direction (B80L / B80W) is 0.60 to 1.40, and a nanocrystalline alloy thin strip showing isotropic properties is obtained.
[0183] In addition, according to the present disclosure, a nanocrystalline alloy ribbon with a wrinkle height of 0.15 mm or less is obtained. In addition, by setting the pressure of pressing the ribbon to 0.03 MPa or more, a nanocrystalline alloy ribbon with a wrinkle height of 0.10 mm or less and a space factor of 68.0% or more is obtained.
[0184] Therefore, according to the present disclosure, a nanocrystalline alloy ribbon having excellent magnetic properties of high saturation magnetic flux density and high magnetic permeability can be obtained. In addition, a nanocrystalline alloy ribbon having low magnetostriction, low loss and isotropy can be obtained. In addition, a nanocrystalline alloy ribbon having high space factor and suppressing wrinkles and stripes can be obtained.
[0185] [Example 4]
[0186] In Example 4, a 3 μm thick adhesive layer was attached to one surface of the nanocrystalline alloy ribbons of Example 1 and Example 2 to produce a magnetic sheet.
[0187] Fig.14It is a cross-sectional view cut along the width direction for explaining the structure of the magnetic sheet.
[0188] like Fig.14 As shown, the magnetic sheet has a structure in which one adhesive layer 10 , one resin sheet 15 ( 15B) and one nanocrystalline alloy thin strip 20 are stacked.
[0189] The adhesive layer 10 is mainly provided with a support 11 and a plurality of adhesives 12. It should be noted that the support 11 is a film member formed in a long strip shape, for example, a film member formed in a rectangular shape. The support 11 is formed using a flexible resin material. As the resin material, polyethylene terephthalate (PET: Polyethyleneterephthalate) can be used. The adhesive 12 can use, for example, a pressure-sensitive adhesive. For example, known adhesives such as acrylic adhesives, silicone adhesives, polyurethane adhesives, synthetic rubber, and natural rubber can be used as the adhesive 12. Acrylic adhesives have excellent heat resistance and moisture resistance, and can also be bonded to a wide range of materials, so they are preferably used as the adhesive 12.
[0190] The adhesive 12 is provided in a film or layer form on the first surface 11A and the second surface 11B of the support 11. Here, the total thickness of the adhesive 12 on the first surface 11A side of the adhesive layer 10 and the adhesive 12 on the support 11 and the second surface 11B side is 3 μm.
[0191] Moreover, by removing the resin sheet 15 , the magnetic sheet can be attached to another member using the adhesive 12 on the second surface 11B side.
[0192] In addition, a plurality of the magnetic sheets are prepared to produce a magnetic sheet in which a plurality of nanocrystalline alloy thin strips are stacked. The plurality of magnetic sheets are used to stack the nanocrystalline alloy thin strips via an adhesive layer.
[0193] Specifically, first, the resin sheet 15 (15B) is peeled off on the side of the adhesive layer 10 of the first magnetic sheet where the nanocrystalline alloy thin strip 20 is not attached. Next, the nanocrystalline alloy thin strip 20 of another magnetic sheet is attached to the portion of the adhesive layer 10 where the adhesive 12 is exposed. By repeating this operation, a magnetic sheet having 15 layers of nanocrystalline alloy thin strips stacked is formed.
[0194] A magnetic sheet having 15 layers of nanocrystalline alloy thin strips was used and punched into a ring shape having an inner diameter of 8.8 mm and an outer diameter of 19.9 mm. The iron loss at 128 kHz and 0.2 T and the real part of the complex permeability at 128 kHz and 0.03 V were evaluated using the ring-shaped magnetic sheet. The results are shown in Table 6.
[0195] According to the present disclosure, the iron loss at 128kHz and 0.2T is 2000kW / m3 The following are magnetic sheets having a real part of complex permeability of 1500 or more.
[0196] According to the present disclosure, a magnetic sheet having excellent magnetic properties can be configured.
[0197] [Table 6]
[0198]
[0199] [Example 5]
[0200] In Example 5, a 3 μm thick adhesive layer 10 is attached to one side of the nanocrystalline alloy ribbon of Example 1, and then cracks 21 are formed in the nanocrystalline alloy ribbon to produce a magnetic sheet.
[0201] Fig.15 It is a cross-sectional view cut along the width direction for explaining the structure of the magnetic sheet 100 .
[0202] like Fig.15 As shown, the magnetic sheet 100 has a structure in which one adhesive layer 10, one resin sheet 15 (15B) and one nanocrystalline alloy ribbon 20 are stacked. Here, cracks 21 are formed in the nanocrystalline alloy ribbon 20, and the nanocrystalline alloy ribbon 20 is divided into small pieces 22 by the cracks 21.
[0203] In addition, a plurality of the magnetic sheets are prepared to produce a magnetic sheet in which a plurality of nanocrystalline alloy thin strips are stacked. The plurality of magnetic sheets are used to stack the nanocrystalline alloy thin strips 20 via the adhesive layer 10 .
[0204] Specifically, first, the resin sheet 15 (15B) is peeled off on the side of the adhesive layer 10 of the first magnetic sheet 100 where the nanocrystalline alloy ribbon 20 is not attached. Next, the nanocrystalline alloy ribbon 20 of another magnetic sheet 100 is attached to the portion of the adhesive layer 10 where the adhesive 12 is exposed. By repeating this operation, a magnetic sheet having 15 layers of nanocrystalline alloy ribbons stacked is formed.
[0205] A magnetic sheet having 15 layers of nanocrystalline alloy thin strips was used and punched into a ring shape having an inner diameter of 8.8 mm and an outer diameter of 19.9 mm. The iron loss at 128 kHz and 0.2 T and the real part of the complex permeability at 128 kHz and 0.03 V were evaluated using the ring-shaped magnetic sheet. The results are shown in Table 7.
[0206] Similarly, a 15-layer magnetic sheet was prepared for No. 4 of Example 2, and the iron loss at 128 kHz and 0.2 T and the real part of the complex permeability at 128 kHz and 0.03 V were evaluated. The results are shown in Table 7.
[0207] According to the present disclosure, the iron loss at 128kHz and 0.2T is 2000kW / m 3 The following are magnetic sheets having a real part of complex permeability of 400 to 3000.
[0208] [Table 7]
[0209]
[0210] In Examples 4 and 5, the methods for measuring the iron loss and the real part of the complex permeability are as follows.
[0211] [Iron loss]
[0212] In the BH analyzer SY8218 manufactured by Iwasaki Communication Equipment Co., Ltd., a toroidal core with an inner diameter of 8.8 mm and an outer diameter of 19.9 mm was punched out from a 15-layer magnetic sheet and placed in a housing to measure the iron loss. The measurement conditions were 15 turns of primary and secondary windings, 128 kHz, and a magnetic flux density of 0.2 T.
[0213] [Complex permeability]
[0214] Using the BH analyzer SY8218 manufactured by Iwasaki Communication Equipment Co., Ltd., a toroidal core with an inner diameter of 8.8 mm and an outer diameter of 19.9 mm was punched out from a 15-layer magnetic sheet and placed in a housing to measure the real part of the complex permeability. The measurement conditions were 15 turns of primary and secondary windings, a frequency of 128 kHz, and a voltage of 0.03 V.
[0215] Fig.10 1 is a schematic diagram for explaining a method for manufacturing a magnetic sheet 100 having a single layer of nanocrystalline alloy thin strip according to the present disclosure. Fig.10 2 shows a method of continuously attaching the adhesive layer 10 to the nanocrystalline alloy ribbon 20 .
[0216] Magnetic sheet 100 use Fig.10 The manufacturing device 500 is shown in the figure. In the manufacturing device 500, from the upstream to the downstream of the manufacturing process, the first unwinding roller 510, the first winding roller 520, the second unwinding roller 530, the plurality of attaching rollers 540, the crack section 550, the plurality of flattening rollers 560 and the third winding roller 570 are mainly provided. A plurality of guide rollers 580 may also be provided in the manufacturing device 500. In addition, the guide roller 580 may be arranged at a position not shown in the figure as required.
[0217] Fig.11 It is a cross-sectional view for explaining the structure of the stacked body supplied from the first delivery roll 510 .
[0218] like Fig.11As shown, a laminated body in which resin sheets 15A and 15B are laminated on the first surface 11A and the second surface 11B of the adhesive layer 10 is wound on the first unwinding roll 510. The resin sheet 15A disposed on the first surface 11A is a protective sheet. The resin sheet 15B disposed on the second surface 11B is also marked as a liner. The resin sheet 15A is a sheet thinner than the resin sheet 15B.
[0219] Fig.12 This is a cross-sectional view for explaining the structure of the laminated body in which the resin sheet 15A is supplied from the first unwinding roll 510 and peeled off.
[0220] like Fig.12 As shown, the resin sheet 15A is peeled off from the laminate unwound from the first unwinding roll 510. Fig.10 As shown, the peeled resin sheet 15A is wound up on the first winding roll 520 .
[0221] Fig.13 It is a cross-sectional view illustrating the structure of the nanocrystalline alloy strip 20 supplied from the second unwinding roll 530 .
[0222] The laminated body from which the resin sheet 15A is peeled off is guided to the attaching roller 540 by a plurality of guide rollers 580. The nanocrystalline alloy thin strip 20 unwound from the second unwinding roller 530 is further guided to the attaching roller 540. Fig.13 As shown, cracks 21 are not formed in the nanocrystalline alloy strip 20 guided to the attachment roller 540 .
[0223] Fig.14 It is a cross-sectional view illustrating a state where the nanocrystalline alloy thin strip 20 is bonded to the adhesive layer 10 by the bonding roller 540 .
[0224] As the attachment roller 540, Fig.10 As shown, there are two cylindrical rollers arranged opposite to each other. The two rollers each have a smooth circumferential surface without protrusions. The two rollers press and adhere the nanocrystalline alloy thin strip 20 to the laminated body from which the resin sheet 15A is peeled off. Specifically, the laminated body and the nanocrystalline alloy thin strip 20 are introduced between the two rollers arranged opposite to each other, and the two rollers are used, such as Fig.14 As shown, the nanocrystalline alloy thin strip 20 is pressed and bonded to the first surface 11A of the adhesive layer 10. Fig.10 As shown, the stacked body to which the nanocrystalline alloy strips 20 are bonded is guided from the attachment roller 540 to the crack portion 550 .
[0225] It should be noted that, when the crack 21 is not formed, the strand may be wound up on the third winding roller 570 without being guided to the crack portion 550 , or may be cut into a desired length.
[0226] Fig.151 is a cross-sectional view illustrating a state in which a crack 21 is formed in the nanocrystalline alloy strip 20 through a crack portion 550 .
[0227] The crack portion 550 forms cracks 21 in the nanocrystalline alloy strip 20 bonded to the adhesive layer 10. Specifically, the crack portion 550 includes two rollers arranged opposite to each other. That is, the crack portion 550 includes a crack roller 550A and a support roller 550B. The manufacturing device 500 guides the stacked body bonded with the nanocrystalline alloy strip 20 between the two rollers. The crack roller 550A is a cylindrical roller with protrusions on the circumferential surface. The support roller 550B is a cylindrical roller without protrusions on the circumferential surface. The manufacturing device 500 presses the protrusion of the crack roller 550A against the nanocrystalline alloy strip 20, as shown in FIG. Fig.15 As shown, cracks 21 are formed.
[0228] The support roll 550B is disposed on the laminated body side from which the resin sheet 15 has been peeled. The nanocrystalline alloy ribbon 20 having the cracks 21 formed therein includes a plurality of small pieces 22. The plurality of small pieces 22 are bonded to the adhesive layer 10.
[0229] Here, the structure of the crack roller 550A is described. A plurality of convex members are arranged on the circumferential surface of the crack roller 550A as the above-mentioned protrusions. The shape of the end of the convex member of the crack roller 550A can be flat, conical, inverted conical with a central depression, or cylindrical. The plurality of convex members can be arranged regularly or irregularly.
[0230] The laminated body guided from the crack portion 550 to the flattening roller 560 is flattened by the flattening roller 560. In addition, the flattening roller 560 is also referred to as a reforming roller.
[0231] Specifically, the laminate is introduced between two rollers of the flattening rollers 560 that are arranged opposite to each other, and the laminate is sandwiched and pressed between the two rollers. As a result, the surface of the nanocrystalline alloy ribbon 20 having the cracks 21 formed therein is flattened.
[0232] The flattened laminated body becomes the magnetic sheet 100. The magnetic sheet 100 is guided to the third winding roller 570 via the guide roller 580. The magnetic sheet 100 is wound on the third winding roller 570. The magnetic sheet 100 wound on the third winding roller 570 into a ring or spiral shape is the wound magnetic sheet 200.
[0233] The magnetic sheet 100 may be wound up, or may be cut into a predetermined length without being wound up.
[0234] Here, the width B of the nanocrystalline alloy ribbon 20 and the width A of the adhesive layer 10 preferably have a shape satisfying the following relationship (see Fig.16 ).
[0235] 0.2mm≤(width A-width B)≤3mm
[0236] Width A is a dimension related to the adhesive layer 10, and more preferably a dimension related to the region of the adhesive layer 10 where the adhesive 12 for bonding the nanocrystalline alloy strip 20 is provided. Width B is a dimension related to the nanocrystalline alloy strip 20. It should be noted that, when the adhesive 12 is provided on the entire surface of the support 11 of the adhesive layer 10, width A is a dimension related to the adhesive layer 10 or the support 11.
[0237] Here, the lower limit of (width A-width B) is preferably 0.5 mm, and more preferably 1.0 mm. In addition, the upper limit of (width A-width B) is preferably 2.5 mm, and more preferably 2.0 mm.
[0238] The nanocrystalline alloy thin strip 20 may be arranged with the adhesive layer 10 aligned with the center in the width direction, or may be arranged with the center separated. In this case, the relationship of 0 mm < gap a and 0 mm < gap b is satisfied (see Fig.16 ) method.
[0239] The gap a and the gap b are the distances from the end of the adhesive layer 10 to the end of the nanocrystalline alloy thin strip 20. Specifically, the gap a is the distance from the first adhesive layer end 10X of the adhesive layer 10 to the first thin strip end 20X of the nanocrystalline alloy thin strip 20. The gap b is the distance from the second adhesive layer end 10Y of the adhesive layer 10 to the second thin strip end 20Y of the nanocrystalline alloy thin strip 20.
[0240] The first thin strip end 20X is the end on the same side as the first adhesive layer end 10X in the nanocrystalline alloy thin strip 20. The second adhesive layer end 10Y is the end on the opposite side of the first adhesive layer end 10X of the adhesive layer 10. The second thin strip end 20Y is the end on the same side as the second adhesive layer end 10Y in the nanocrystalline alloy thin strip 20.
[0241] The width A, the width B, the gap a, and the gap b are dimensions in a direction intersecting, more preferably orthogonal to, the length direction of the magnetic sheet 100. The length direction of the magnetic sheet 100 is the same as the length direction of the adhesive layer 10. In addition, the length direction of the magnetic sheet 100 is the same as the length direction of the nanocrystalline alloy ribbon 20.
[0242] The width A of the region where the adhesive 12 is provided in the adhesive layer 10 of the magnetic sheet 100 is set wider than the width B of the nanocrystalline alloy ribbon 20. According to such a configuration, when the nanocrystalline alloy ribbon 20 is attached to the adhesive layer 10, even if the adhesive layer 10 and the nanocrystalline alloy ribbon 20 meander, the adhesive 12 of the adhesive layer 10 can be easily arranged on the entire surface of the nanocrystalline alloy ribbon 20. In addition, by arranging the adhesive layer 10 on the entire surface of the nanocrystalline alloy ribbon 20, after the cracks 21 are formed in the nanocrystalline alloy ribbon 20 to form the small pieces 22, it is possible to suppress the small pieces 22 from falling off.
[0243] The value obtained by subtracting the width B from the width A of the magnetic sheet 100 is set to be 0.2 mm or more. With such a configuration, when the nanocrystalline alloy ribbon 20 is attached to the adhesive layer 10 , it is easy to suppress the occurrence of a portion where the adhesive 12 is not disposed in the nanocrystalline alloy ribbon 20 .
[0244] The value obtained by subtracting the width B from the width A of the magnetic sheet 100 is set to be 3 mm or less. According to such a configuration, it is easy to prevent the portion of the magnetic sheet 100 where the nanocrystalline alloy ribbons 20 are not arranged from becoming larger. In addition, when the magnetic sheets 100 are arranged in parallel, it is easy to prevent the intervals (magnetic gaps) between the nanocrystalline alloy ribbons from becoming larger.
[0245] The magnetic sheet 100 is set to satisfy the relationship of 0 mm < gap a and 0 mm < gap b. According to such a configuration, when the nanocrystalline alloy strip 20 is attached to the adhesive layer 10, it is easy to suppress the nanocrystalline alloy strip 20 from protruding from the area where the adhesive 12 is provided. Therefore, it is easy to suppress the generation of a portion in the nanocrystalline alloy strip 20 where the adhesive 12 is not provided.
[0246] According to the present disclosure, a nanocrystalline alloy ribbon with high magnetic permeability is obtained with high saturation magnetic flux density. In addition, according to the present disclosure, a nanocrystalline alloy ribbon with low magnetostriction, low loss and isotropy is obtained. In addition, according to the present disclosure, a nanocrystalline alloy ribbon with high space factor and wrinkles and streaks suppressed is obtained.
[0247] According to the present disclosure, a magnetic sheet using a nanocrystalline alloy ribbon having excellent characteristics is obtained.
Claims
1. A method for producing a nanocrystalline alloy ribbon, comprising: bringing an amorphous alloy ribbon into contact with a heating body to heat the amorphous alloy ribbon, producing a nanocrystalline alloy ribbon having a structure in which grains with an average grain size of 50 nm or less exist in an amorphous phase, The nanocrystalline alloy ribbon has a composition formula (Fe 1-x A x ) a Si b B c Cu d M e It represents that A is at least one of Ni and Co, M is at least one element selected from Nb, Mo, V, Zr, Hf and W, and in terms of atomic %, 72.0≤a≤81.0, 9.0≤b≤17.0, 5.0≤c≤10.0, 0.02≤d≤1.2, 0.1≤e≤3.5, 0≤x≤0.1, When the amorphous alloy thin strip contacts the heating body and is heated, the amorphous alloy thin strip is conveyed, and a thin strip pressing member contacts the surface of the amorphous alloy thin strip opposite to the surface in contact with the heating body, and the amorphous alloy thin strip is heated while being pressed against the heating body. When the bccFe crystallization start temperature of the amorphous alloy ribbon measured at a heating rate of 20 K / min is defined as Tx1°C, the heater is heated to a heating temperature Ta of Tx1+80°C or higher and Tx1+230°C or lower.
2. The method for producing a nanocrystalline alloy ribbon according to claim 1, wherein: The thin strip pressing member is a soft member.
3. The method for producing a nanocrystalline alloy ribbon according to claim 1 or 2, wherein: The conveying speed of the amorphous alloy ribbon is 1 m / min or more.
4. The method for producing a nanocrystalline alloy ribbon according to any one of claims 1 to 3, wherein: The contact time between the amorphous alloy ribbon and the heating body is 0.1 second to 30 seconds.
5. The method for producing a nanocrystalline alloy ribbon according to any one of claims 1 to 4, wherein: The pressure at which the amorphous alloy ribbon is pressed against the heating body is 0.03 MPa or more.
6. The method for producing a nanocrystalline alloy ribbon according to any one of claims 1 to 5, wherein: The wrinkle height of the nanocrystalline alloy ribbon is less than 0.15 mm, and the space factor is more than 68.0%.
7. The method for producing a nanocrystalline alloy ribbon according to any one of claims 1 to 6, wherein: The saturation magnetic flux density Bs of the nanocrystalline alloy ribbon is greater than 1.15 T, and the maximum magnetic permeability is greater than 4000.
8. The method for producing a nanocrystalline alloy ribbon according to any one of claims 1 to 7, wherein: The residual magnetic flux density Br of the nanocrystalline alloy ribbon and the magnetic flux density B of the 8000A / m magnetic field 8000 The ratio of Br / B 8000 It is above 0.
20.
9. The method for producing a nanocrystalline alloy ribbon according to any one of claims 1 to 8, wherein: The magnetic flux density B80 when a magnetic field of 80A / m is applied along the length direction of the nanocrystalline alloy ribbon L The magnetic flux density B80 when a magnetic field of 80 A / m is applied along the width direction orthogonal to the length direction W ratio, i.e. B80 L / B80 W 0.60~1.40, and B80 L 、B80 W All are above 0.4T.
10. The method for producing a nanocrystalline alloy ribbon according to any one of claims 1 to 9, wherein: The saturation magnetostriction is 7 ppm or less.
11. A method for manufacturing a magnetic sheet, comprising: The nanocrystalline alloy ribbon obtained by the manufacturing method according to claim 1, and A support body formed in a strip shape and an adhesive layer of an adhesive provided on at least one of a first surface and a second surface of the support body, The nanocrystalline alloy ribbon and the adhesive layer are continuously guided to an attaching roller, and the nanocrystalline alloy ribbon and the adhesive layer are bonded to each other by the attaching roller.
12. The method for producing a magnetic sheet according to claim 11, wherein: After the adhesive layer is attached to one side of the nanocrystalline alloy ribbon, a cracking roller is pressed against the opposite side of the nanocrystalline alloy ribbon to the side to which the adhesive layer is attached, so as to form cracks in the nanocrystalline alloy ribbon.
13. The method for producing a magnetic sheet according to claim 11 or 12, wherein: When the dimension related to the adhesive layer and the dimension in the direction intersecting the length direction of the adhesive layer is set as width A, and the dimension related to the nanocrystalline alloy strip and the dimension in the direction intersecting the length direction of the nanocrystalline alloy strip is set as width B, the relationship of 0.2mm≤(width A-width B)≤3mm is satisfied.
14. The method for producing a magnetic sheet according to any one of claims 11 to 13, wherein: In a cross-sectional view taken along a direction intersecting the longitudinal direction of the adhesive layer, When the distance from the first adhesion layer end of the adhesion layer to the end of the nanocrystalline alloy strip on the same side as the first adhesion layer end, i.e., the first strip end, is set as gap a, and the distance from the second adhesion layer end of the adhesion layer on the opposite side of the first adhesion layer end to the end of the nanocrystalline alloy strip on the same side as the second adhesion layer end, i.e., the second strip end, is set as gap b, the relationship of 0mm<gap a and 0mm<gap b is satisfied.