Carbon-coated cerium oxide material with excellent electro-catalytic oxygen reduction performance
The ceria material is coated through amorphous carbon coating technology, and the problem of insufficient stability and active sites in electrocatalytic oxygen reduction reactions is solved, and efficient and stable oxygen reduction reactions and hydrogen peroxide generation are achieved.
Patent Information
- Application Number
- CN202411061126.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-05
AI Technical Summary
The existing carbon-based materials have insufficient stability and service life in electrocatalytic redox reactions, and lack effective mechanical strength and active sites, which affect catalytic performance.
Amorphous carbon coating technology is used to coat cerium oxide materials, and the cerium oxide core is protected by introducing a high electron density carbon layer, promoting the generation of oxygen vacancies and defects, optimizing the charge distribution and mechanical strength of the catalyst surface, and reducing the activation of oxygen reduction reaction able.
It significantly improves the stability and service life of the catalyst, increases the mechanical strength and active sites, improves the selectivity and reaction efficiency for hydrogen peroxide generation, and extends the durability time of the catalyst.
Smart Images

Figure CN118976479A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the fields of materials, chemistry and electrocatalysis technology, and in particular to a carbon-coated cerium oxide material with excellent electrocatalytic oxygen reduction performance. Background Art
[0002] In recent years, the massive consumption of fossil energy has caused a series of problems such as energy shortage. The electrocatalytic oxygen reduction reaction is an important step in fuel cells and metal-air batteries, and has attracted increasing attention. In recent years, hybrid electrocatalysts of transition metal oxides and carbon materials have been widely used in the study of electrocatalytic oxygen reduction reactions, in which carbon materials play the role of promoters most of the time. Carbon-based materials have received widespread attention for their applications in the electrocatalytic reduction of oxygen to hydrogen peroxide due to their good conductivity, low cost, and high stability. The ability of carbon-based materials to electrochemically generate hydrogen peroxide can be improved by doping non-metallic heteroatoms or creating structural defects and modifying the surface. The electrocatalytic activity of carbon-based materials can be optimized by strategies such as the construction of porous structures and the manufacture of special functional groups, which can accelerate mass transfer and expose more active sites. For example, samples rich in C=O functional groups show more positive potentials than samples containing COC functional groups. More noteworthy is that cerium oxide, as a rare earth metal oxide, has been widely used in various catalytic fields. The electrocatalytic activity of cerium oxide originates from Ce. 3+ / Ce 4+ Redox couple, this is due to the Ce of cerium oxide in the catalytic system 3+ and Ce 4+ The redox couple can undergo rapid transformation and generate abundant oxygen vacancies. When the catalytic reaction occurs, cerium oxide can act as a reaction site to promote the activation of reactants, and can also improve the specific surface area, exposing more active sites in the catalytic boundary to increase the electrocatalytic activity. In addition, cerium oxide has excellent oxygen storage and release capacity and electronic / ionic conductivity.
[0003] Therefore, the present invention proposes a carbon-coated cerium oxide material with excellent electrocatalytic oxygen reduction performance, which exhibits excellent performance in the cathode oxygen reduction reaction of a fuel cell. Summary of the invention
[0004] The purpose of the present invention is to make up for the shortcomings of the prior art and provide a carbon-coated cerium oxide material with excellent electrocatalytic oxygen reduction performance. The amorphous carbon coating technology is used to introduce a carbon layer with a high electron density to effectively protect the cerium oxide core and prevent it from being corroded or decomposed during the reaction, thereby significantly improving the stability and service life of the catalyst. The presence of the carbon layer also improves the mechanical strength of the catalyst, reduces agglomeration and wear between particles, and further extends the durability of the catalyst. The interaction between the amorphous carbon coating and the cerium oxide promotes the generation of more oxygen vacancies and defects. These vacancies and defects serve as active sites, accelerate the oxygen reduction reaction, and improve the selectivity for the formation of hydrogen peroxide. The electronic structure of the carbon layer optimizes the charge distribution on the catalyst surface, making it easier for electrons to be transferred to the reactant molecules, reducing the activation energy of the oxygen reduction reaction and improving the reaction efficiency.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: On the one hand, a carbon-coated cerium oxide material with excellent electrocatalytic oxygen reduction performance is provided, and the preparation method comprises: step S100 of preparing a cerium oxide precursor and step S200 of preparing a carbon-coated cerium oxide, wherein the specific steps of preparing the cerium oxide precursor in step S100 are:
[0006] S101, material preparation: weigh an appropriate amount of cerium nitrate hexahydrate (Ce(NO3)3·6H2O) to ensure the required molar amount,
[0007] Prepare deionized water for dissolving cerium nitrate and for subsequent cleaning steps, and prepare sodium hydroxide (NaOH) solution, the concentration of which is adjusted according to the reaction requirements;
[0008] S102, mixing: in a suitable container, slowly add cerium nitrate hexahydrate powder into deionized water, stirring while adding, until it is completely dissolved to form a uniform solution, slowly dropwise add sodium hydroxide solution into the cerium nitrate solution, stirring continuously, and ensure that the two are fully mixed and uniform. This process will produce a white precipitate, i.e., the initial formation of cerium hydroxide (Ce(OH)4);
[0009] S103, heating: placing the mixed solution in a heating device, heating it to a certain temperature, and maintaining it for a period of time to promote the complete formation and aging of cerium hydroxide;
[0010] S104, centrifugation and drying: centrifuging the heated solution to separate a solid precipitate, washing the precipitate with deionized water for multiple times to remove residual ions and impurities, centrifuging the washed precipitate in a centrifuge to remove excess water, and placing the centrifuged solid in an oven to dry overnight at an appropriate temperature (e.g., 80-120° C.) to obtain a cerium oxide precursor;
[0011] The specific steps of preparing the carbon-coated cerium oxide in step S200 are:
[0012] S201, preparation of glucose solution: weigh an appropriate amount of glucose (C6H 12 O6), add it into deionized water, heat and stir until it is completely dissolved to form a glucose solution;
[0013] S202, mixing and heating: adding the cerium oxide precursor powder obtained in step S100 to the glucose solution, stirring evenly to ensure that the precursor particles are fully coated by the glucose solution, placing the mixed solution in a heating device, heating to a certain temperature, and maintaining it for a period of time, so that the glucose is carbonized at high temperature and coated on the surface of the cerium oxide;
[0014] S203, centrifugation and dialysis: centrifuging the heated solution to separate the solid product, washing the solid product with deionized water to remove the unreacted substances attached to the surface, placing the washed solid product in a dialysis membrane, and dialyzing it with deionized water to remove the residual glucose and other small molecules. The dialysis time is determined according to actual needs until no glucose is detected in the dialysate;
[0015] S204, freeze drying and crushing: the dialyzed sample is placed in a freeze dryer for freeze drying to remove moisture from the sample and retain its porous structure. After the freeze dried sample is taken out, an appropriate amount of deionized water is added and crushed in a cell crusher to refine the particles and increase the specific surface area. Centrifugal drying is performed again to remove excess moisture to obtain the final carbon-coated cerium oxide electrocatalyst.
[0016] Furthermore, during the heating process in step S103, an inert gas (such as nitrogen or argon) is introduced into the heating device for protection to prevent the cerium oxide precursor from being oxidized at high temperature, thereby improving the purity and catalytic performance of the product.
[0017] Furthermore, during the mixing and heating process in step S202, the heating rate is further controlled to not exceed 5°C per minute to ensure that the glucose is evenly and slowly carbonized and coated on the surface of the cerium oxide precursor to form a uniform carbon layer, thereby improving the stability and durability of the catalyst.
[0018] Furthermore, after the centrifugation and dialysis in step S203, the dialyzed solid product is also subjected to an acid wash treatment to further remove impurities attached to the surface and incompletely reacted organic matter. The acid wash treatment uses a dilute acid solution (such as dilute nitric acid, dilute hydrochloric acid), and after soaking at room temperature for a certain period of time, it is washed with deionized water until neutral, thereby obtaining a purer carbon-coated cerium oxide material.
[0019] Furthermore, before the freeze-drying step S204, the dialyzed and acid-washed sample is subjected to ultrasonic treatment to further break up the agglomeration between the particles and increase the specific surface area and active sites of the catalyst. The ultrasonic treatment is carried out in a suitable solvent including but not limited to ethanol and acetone, and the ultrasonic time and power are controlled to avoid particle damage.
[0020] Furthermore, the concentration of the prepared sodium hydroxide in step S101 is 1-10 mol / L, the volume ratio of water to sodium hydroxide in step S102 is 1:(1-20), the reaction time is 1-100 min, and the heating temperature in step S103 is 50-150° C., and the heating time is 12-36 h.
[0021] Furthermore, in step S201, the mass ratio of cerium oxide precursor powder to glucose is 1:(1-10), the heating temperature in step S202 is 100-200° C., the heating time is 1-10 h, and the cell crushing time in step S204 is 1-5 h.
[0022] Furthermore, the drying temperature in steps S104 and S204 is 50-100° C., and the drying time is 10-24 hours.
[0023] On the other hand, a carbon-coated rare earth metal oxide electrocatalyst for producing hydrogen peroxide by electrocatalytic oxygen reduction is provided, characterized in that it is prepared according to the method according to any one of claims 1 to 8.
[0024] Compared with the prior art, the carbon-coated cerium oxide material with excellent electrocatalytic oxygen reduction performance has the following beneficial effects:
[0025] 1. The present invention uses amorphous carbon coating technology to introduce a carbon layer with a high electron density, which can effectively protect the cerium oxide core and prevent it from being corroded or decomposed during the reaction, thereby significantly improving the stability and service life of the catalyst. The slow heating carbonization process (such as a temperature increase of no more than 5°C per minute) ensures that the carbon layer can be evenly and densely covered on the surface of cerium oxide, reducing the performance degradation of the catalyst caused by the shedding or breakage of the carbon layer during use. The presence of the carbon layer also improves the mechanical strength of the catalyst, reduces the agglomeration and wear between particles, and further extends the durability of the catalyst.
[0026] 2. The present invention utilizes the interaction between amorphous carbon coating and cerium oxide to promote the generation of more oxygen vacancies and defects. These vacancies and defects serve as active sites, which can accelerate the oxygen reduction reaction and improve the selectivity of hydrogen peroxide production. The electronic structure of the carbon layer optimizes the charge distribution on the catalyst surface, making it easier for electrons to be transferred to the reactant molecules, reducing the activation energy of the oxygen reduction reaction, thereby improving the reaction efficiency. Freeze-drying and pulverization treatments further refine the catalyst particles, increase the specific surface area and the number of active sites, provide more reaction sites for the oxygen reduction reaction, and further improve the catalytic performance.
[0027] 3. In the preparation process of the present invention, impurities on the catalyst surface and incompletely reacted organic matter are effectively removed through multiple purification steps such as centrifugation, dialysis, acid washing and ultrasonic treatment, thereby improving the purity and quality of the product. The heating process under the protection of inert gas prevents the oxidation of the cerium oxide precursor at high temperature, avoids the formation of harmful oxides, and improves the safety and environmental friendliness of the product. The finally obtained carbon-coated cerium oxide electrocatalyst has excellent catalytic performance and stability, and can efficiently and stably generate hydrogen peroxide in the electrocatalytic oxygen reduction reaction, providing reliable technical support for industrial production in related fields.
[0028] Other advantages, objectives and features of the present invention will be set forth in part in the following description and, in part, will be apparent to those skilled in the art based on an examination of the following or may be taught from the practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the prior art descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0030] Figure 1 is an X-ray diffraction pattern of carbon-coated cerium oxide and cerium oxide materials prepared by the method of the present invention;
[0031] Figure 2 is a scanning electron microscope image of a carbon-coated cerium oxide material prepared by the method of the present invention;
[0032] Figure 3 is a projection electron microscope image of a carbon-coated cerium oxide material prepared by the method of the present invention;
[0033] Figure 4 It is a graph of hydrogen peroxide selectivity of carbon-coated cerium oxide and cerium oxide materials prepared by the method of the present invention. DETAILED DESCRIPTION
[0034] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] Embodiment 1
[0036] Preparation of CeO2 / C
[0037] Step 1: Preparation of CeO2 precursor
[0038] Solution preparation: First, weigh 0.8 g of cerium nitrate hexahydrate (Ce(NO3)3·6H2O) and add it to 5 mL of deionized water. Stir it thoroughly with a magnetic stirrer or a glass rod until it is completely dissolved to form a uniform cerium nitrate solution. Then, quickly pour 35 mL of 6 mol / L sodium hydroxide (NaOH) solution into the above cerium nitrate solution and immediately stir vigorously for 30 minutes. The purpose of this step is to make Ce 3+ Ions and OH - The ions react to form Ce(OH)3 precipitate;
[0039] Hydrothermal reaction: The mixed solution was carefully transferred to a 100 mL autoclave (lined with polytetrafluoroethylene for corrosion prevention), ensuring good sealing. Then, the autoclave was placed in an oven and reacted at 100 °C for 24 hours. The hydrothermal reaction was helpful for the crystallization and morphology control of Ce(OH)3 precipitation.
[0040] Washing and drying: After the reaction is completed, wait for the reactor to cool naturally to room temperature, take out the precipitate, and wash the precipitate three times with deionized water and anhydrous ethanol alternately to remove excess ions and impurities. Then, place the yellow solid in a constant temperature oven at 65°C and dry overnight until it is completely dry. Finally, grind the dried solid into powder to obtain the CeO2 precursor.
[0041] Step 2: Preparation of CeO2 / C composite materials
[0042] Mixing of glucose solution: Weigh 0.1 g of CeO2 precursor powder and add it to 4 mL of 0.1 g / mL glucose solution. Stir vigorously to ensure that the CeO2 powder is evenly dispersed in the glucose solution.
[0043] Secondary hydrothermal reaction: The mixed solution was transferred to a 10 mL high pressure reactor (also lined with polytetrafluoroethylene), sealed and placed in an oven for 3 hours at 160 °C. This step was to carbonize glucose at high temperature and coat it on the surface of CeO2 particles.
[0044] Purification and drying: After the reaction is completed, the reactor is cooled naturally to room temperature, the reaction product is taken out, and the product is dialyzed using a dialysis membrane (molecular weight cutoff is about 2000Da) for 2 days to remove unreacted glucose and other small molecule impurities. After dialysis, the solution is freeze-dried to remove moisture to obtain a CeO2 / C composite material;
[0045] Crushing and post-processing: Add an appropriate amount of deionized water to the freeze-dried CeO2 / C composite material and crush it for 1.5 hours using a cell crusher or ball mill to improve the dispersibility and particle size distribution of the material. After crushing, centrifuge the suspension to remove larger particles or undispersed agglomerates. Finally, dry the solid obtained by centrifugation in a constant temperature oven to obtain the final CeO2 / C composite material sample.
[0046] Embodiment 2
[0047] Preparation of CeO2
[0048] Step 1: Solution preparation: First, accurately weigh 0.8 g of cerium nitrate hexahydrate (Ce(NO3)3·6H2O) and add it to 4 mL of deionized water. Use a magnetic stirrer or a glass rod to stir thoroughly until the cerium nitrate hexahydrate is completely dissolved to form a uniform solution. Then, quickly and evenly pour 35 mL of 6 mol / L sodium hydroxide (NaOH) solution into the above cerium nitrate solution. Stir vigorously during the addition process to ensure that the two solutions are fully mixed and the reaction is uniform. Stir for about 30 minutes to allow Ce to 3+ Ions and OH - The ions react fully to form Ce(OH)3 precipitate;
[0049] Step 2: Hydrothermal reaction: Carefully transfer the mixed solution containing Ce(OH)3 precipitate to a 100mL high-pressure reactor, which should be equipped with a polytetrafluoroethylene liner to prevent corrosion. After ensuring that the reactor is well sealed, place it in an oven and react at a constant temperature of 100°C for 24 hours. The hydrothermal reaction helps the crystallization of Ce(OH)3 precipitate to form a more stable CeO2 precursor.
[0050] Washing and centrifugation: After the reaction is completed, let the reactor cool naturally to room temperature, open the reactor, take out the precipitate, and use deionized water and anhydrous ethanol to wash and centrifuge the precipitate alternately. Centrifugal separation is required after each washing to remove residual ions and impurities. This process is repeated three times to ensure that the precipitate is fully washed;
[0051] Drying and grinding: Place the washed yellow solid in a constant temperature oven at 65°C and dry overnight until the solid is completely dry with no water residue. Then, take out the dried solid and grind it in a mortar or ball mill until fine CeO2 powder is obtained.
[0052] Product collection: Collect the ground CeO2 powder to get the final CeO2 product.
[0053] Embodiment 3
[0054] Electrocatalytic oxygen reduction testing and series characterization of carbon-coated cerium oxide materials:
[0055] Weigh 3 mg of catalyst and disperse it in a mixed solution of isopropanol, water and Nafion. After ultrasonic treatment, a uniformly dispersed solution is obtained. Then, an appropriate amount is dropped on a glassy carbon electrode and dried. The test system is a three-electrode system, namely Ag / AgCl (reference electrode), a platinum mesh (counter electrode) and a glassy carbon electrode with a catalyst added (working electrode). The test electrolyte is an oxygen-saturated 0.1M KOH solution. The potential scanning range is 0.2-1.0V relative to the reversible hydrogen electrode. The scanning speed is 5mV / s, the rotation speed of the rotating disk is 1600rpm, and the carbon-coated cerium oxide material is structurally characterized by XRD, SEM and TEM.
[0056] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A carbon-coated cerium oxide material having excellent electrocatalytic oxygen reduction performance, including a preparation method, It is characterized in that The preparation method comprises: step S100 of preparing a cerium oxide precursor and step S200 of preparing carbon-coated cerium oxide, wherein the specific steps of preparing the cerium oxide precursor in step S100 are: S101, material preparation: weigh an appropriate amount of cerium nitrate hexahydrate (Ce(NO 3 ) 3 6H 2 O), ensuring the required molar amount, Prepare deionized water and sodium hydroxide (NaOH) solution; S102, mixing: In an appropriate container, slowly add cerium nitrate hexahydrate powder into deionized water, stirring while adding, until it is completely dissolved to form a uniform solution, slowly add sodium hydroxide solution dropwise into the cerium nitrate solution, stirring continuously, and ensure that the two are fully mixed. This process will produce a white precipitate, namely cerium hydroxide (Ce(OH) 4 )’s initial formation; S103, heating: placing the mixed solution in a heating device, heating it to a certain temperature, and maintaining it for a period of time to promote the complete formation and aging of cerium hydroxide; S104, centrifugation and drying: centrifuging the heated solution to separate a solid precipitate, washing the precipitate with deionized water for multiple times to remove residual ions and impurities, centrifuging the washed precipitate in a centrifuge to remove excess water, and placing the centrifuged solid in an oven to dry overnight at an appropriate temperature (e.g., 80-120° C.) to obtain a cerium oxide precursor; The specific steps of preparing the carbon-coated cerium oxide in step S200 are: S201, preparation of glucose solution: weigh an appropriate amount of glucose (C 6 H 12 O 6 ), add to deionized water, heat and stir until completely dissolved to form a glucose solution; S202, mixing and heating: adding the cerium oxide precursor powder obtained in step S100 to the glucose solution, stirring evenly to ensure that the precursor particles are fully coated by the glucose solution, placing the mixed solution in a heating device, heating to a certain temperature, and maintaining it for a period of time, so that the glucose is carbonized at high temperature and coated on the surface of the cerium oxide; S203, centrifugation and dialysis: centrifuging the heated solution to separate the solid product, washing the solid product with deionized water to remove the unreacted substances attached to the surface, placing the washed solid product in a dialysis membrane, and dialyzing it with deionized water to remove the residual glucose and other small molecules. The dialysis time is determined according to actual needs until no glucose is detected in the dialysate; S204, freeze drying and crushing: the dialyzed sample is placed in a freeze dryer for freeze drying to remove moisture from the sample and retain its porous structure. After the freeze dried sample is taken out, an appropriate amount of deionized water is added and crushed in a cell crusher to refine the particles and increase the specific surface area. Centrifugal drying is performed again to remove excess moisture to obtain the final carbon-coated cerium oxide electrocatalyst.
2. A carbon-coated cerium oxide material having excellent electrocatalytic oxygen reduction performance according to claim 1, It is characterized in that During the heating process in step S103, an inert gas is introduced into the heating device for protection to prevent the cerium oxide precursor from being oxidized at high temperature, thereby improving the purity and catalytic performance of the product.
3. The carbon-coated cerium oxide material having excellent electrocatalytic oxygen reduction performance according to claim 1, It is characterized in that During the mixing and heating process in step S202, the heating rate is further controlled to not exceed 5°C per minute to ensure that the glucose is evenly and slowly carbonized and coated on the surface of the cerium oxide precursor to form a uniform carbon layer, thereby improving the stability and durability of the catalyst.
4. The carbon-coated cerium oxide material having excellent electrocatalytic oxygen reduction performance according to claim 1, It is characterized in that After the centrifugation and dialysis in step S203, the dialyzed solid product is further subjected to an acid wash treatment to further remove impurities attached to the surface and incompletely reacted organic matter. The acid wash treatment uses a dilute acid solution, and after soaking at room temperature for a certain period of time, it is washed with deionized water until it is neutral, thereby obtaining a purer carbon-coated cerium oxide material.
5. The carbon-coated cerium oxide material having excellent electrocatalytic oxygen reduction performance according to claim 1, It is characterized in that Before the freeze-drying step S204, the dialyzed and acid-washed sample is subjected to ultrasonic treatment to further break up the agglomeration between the particles and increase the specific surface area and active sites of the catalyst. The ultrasonic treatment is carried out in a suitable solvent including but not limited to ethanol and acetone, and the ultrasonic time and power are controlled to avoid particle damage.
6. The carbon-coated cerium oxide material having excellent electrocatalytic oxygen reduction performance according to claim 1, It is characterized in that The concentration of the prepared sodium hydroxide in step S101 is 1-10 mol / L, the volume ratio of water to sodium hydroxide in step S102 is 1:(1-20), the reaction time is 1-100 min, and the heating temperature in step S103 is 50-150° C., and the heating time is 12-36 h.
7. The carbon-coated cerium oxide material having excellent electrocatalytic oxygen reduction performance according to claim 1, It is characterized in that In step S201, the mass ratio of cerium oxide precursor powder to glucose is 1:(1-10), the heating temperature in step S202 is 100-200° C., the heating time is 1-10 h, and the cell crushing time in step S204 is 1-5 h.
8. The carbon-coated cerium oxide material having excellent electrocatalytic oxygen reduction performance according to claim 1, It is characterized in that The drying temperature in steps S104 and S204 is 50-100° C., and the drying time is 10-24 hours.
9. A carbon-coated cerium oxide material with excellent electrocatalytic oxygen reduction performance, It is characterized in that Prepared according to any one of claims 1 to 8.
Citation Information
Patent Citations
Compound catalyst with nanometer core-shell structure and preparing method of compound catalyst
CN107890863A
Carbon-coated cerium dioxide hollow sphere and preparation method thereof
CN108022758A
Membrane electrode of fuel cell and preparation method of membrane electrode
CN117810462A
Carbon-coated metal-doped cerium oxide lithium air battery catalyst and preparation method thereof
CN118299595A
Cited By
Method for manufacturing ink for forming electrolyte layer of fuel cell
JP2025111021A
Method for manufacturing ink for forming electrolyte layer of fuel cell
JP7745019B2