Ti2AlNb-based alloy wire, preparation method of Ti2AlNb-based alloy wire and application of Ti2AlNb-based alloy wire in electric arc additive manufacturing
By optimizing the chemical element composition and process flow of Ti2AlNb-based alloy, high-performance Ti2AlNb-based alloy wire was prepared, which solved the problems of poor material performance and complex operation in the existing technology, and achieved the improvement of high-temperature mechanical properties and simplification of operation .
Patent Information
- Application Number
- CN202411053450.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-19
AI Technical Summary
The existing Ti2AlNb-based alloys have unoptimized raw material composition ratios in arc additive manufacturing, resulting in poor microstructure and performance of the material, complex operation and difficult to control.
By optimizing the chemical element composition ratio of Ti2AlNb-based alloy, using vacuum suspension smelting and upsetting cycles, 10-11% Al, 41-43% Nb, 0.02-0.06% B, 0.01-0.03% Ta were prepared Alloy wire material, and annealing heat treatment and surface treatment, improve the uniformity and mechanical properties of the material.
The uniform structure and high-temperature mechanical properties of Ti2AlNb-based alloy wire are realized, the mechanical properties of arc additive manufacturing are improved, the operation process is simplified, and it is suitable for high-temperature applications.
Smart Images

Figure CN118977013A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of additive manufacturing, and in particular to a Ti2AlNb-based alloy wire, a preparation method thereof, and an application thereof in arc additive manufacturing. Background Art
[0002] Ti2AlNb alloy is a metal material with excellent mechanical properties and high temperature resistance, composed of titanium (Ti), aluminum (Al) and niobium (Nb) elements. Due to its advantages of low density, high strength and high hardness, Ti2AlNb alloy is widely used in aerospace, automobile manufacturing, electronic equipment and chemical industry.
[0003] In the past few decades, metal additive manufacturing technology has become a manufacturing method with great potential. By stacking metal materials layer by layer on the surface of a workpiece with a certain shape, using energy such as laser or arc to melt the material and form a new layer, the metal component is finally manufactured. This technology can not only greatly shorten the manufacturing cycle, but also realize the manufacture of complex structures, providing new possibilities for functions that cannot be achieved by traditional manufacturing methods.
[0004] Chinese patent document CN110977108A discloses an arc additive manufacturing method for Ti2AlNb-based alloy structural parts and a device used therefor. The invention first constructs a three-dimensional solid model, then slices it, generates a processing program, and imports it into a control system; titanium wire, aluminum wire and niobium wire are simultaneously fed under the welding gun for arc additive manufacturing, wherein the titanium wire and the niobium wire are auxiliary heated. The invention overcomes the segregation problem and aluminum burnout problem existing in the traditional preparation method, but the method requires auxiliary heating of the titanium wire and the niobium wire at the same time, which is more complicated to operate and difficult to control. In addition, directly using titanium wire, aluminum wire and niobium wire for arc additive manufacturing without optimizing the ratio of the raw material components will affect the microstructure and performance of the material. Summary of the invention
[0005] In view of the above-mentioned defects of the prior art, the technical problem to be solved by the present invention is to provide a Ti2AlNb-based alloy wire with optimized raw material formula and good performance, and further provide a preparation method and application of the wire.
[0006] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:
[0007] In a first aspect, the present invention provides a Ti2AlNb-based alloy wire comprising the following components in percentage by mass: 10-11% Al, 41-43% Nb, 0.02%-0.06% B, 0.01%-0.03% Ta, and the remainder being Ti and unavoidable impurities.
[0008] In a second aspect, the present invention also provides a method for preparing the above-mentioned Ti2AlNb-based alloy wire, comprising the following steps:
[0009] S1. preparing raw materials according to the composition ratio of each chemical element of the Ti2AlNb-based alloy wire, smelting and casting to obtain an ingot;
[0010] S2: processing the ingot obtained in step S1 into a cylindrical ingot and then performing upsetting and drawing cycles at 1050-1100° C. and 920-960° C. to obtain a forging blank;
[0011] S3 annealing the forged blank after upsetting in step S2;
[0012] S4 extrudes the forging blank after the heat treatment in step S3 to obtain a wire;
[0013] S5: performing surface treatment on the wire obtained in step S4 to remove oxides on the surface of the wire, thereby obtaining a Ti2AlNb-based alloy wire.
[0014] Preferably, the raw materials in step S1 are aluminum bars with a purity of 99.7% to 99.9%; niobium chips with a purity of 99.7% to 99.9%; boron powder with a purity of 99.7% to 99.9%; tantalum powder with a purity of 99.7% to 99.9%; and titanium blocks with a purity of 99.7% to 99.9%. Those skilled in the art can calculate the input amount of each component required for the Ti2AlNb-based alloy wire of the present invention through the content of each metal element in the aluminum bars, niobium chips, boron powder, tantalum powder, and titanium blocks.
[0015] Preferably, in step S1, the smelting step is carried out in a vacuum suspension smelting furnace, the preheating power of the vacuum suspension smelting furnace is 150-250KW, the smelting power is 320KW-400KW, and argon is filled after the vacuum degree reaches 0.5-0.8Pa; an electromagnetic stirring device is placed in the vacuum suspension smelting furnace, and the parameters of the electromagnetic stirring device are: voltage 350-400V, current 280-320A, frequency 3-6Hz, and stirring time 30S-60S. The present invention melts the alloy raw material in a vacuum electromagnetic induction melting furnace. During the smelting process, the content of gas, inclusions and harmful elements can be reduced by electromagnetic stirring technology, and then casting can obtain a high-purity and high-homogeneity ingot for preparing Ti2AlNb alloy wire for arc additive manufacturing.
[0016] Preferably, in step S2, the cylindrical ingot has a specification of 90 mm to 110 mm × 390 mm to 410 mm; processing the ingot into a round ingot can make the internal structure more uniform, and the structural defects and grain segregation generated during the casting process can be improved through processing, thereby improving the uniformity and stability of the material.
[0017] Preferably, in step S2, the number of upsetting cycles is 2-3 times for each temperature range, and the deformation is 30% to 50%; on the one hand, the forging cycle helps to eliminate defects and pores that may exist in the ingot, improve the organizational structure of the material, and improve its uniformity and strength; on the other hand, it can also eliminate residual stress in the material, improve its thermal stability, and reduce the risk of deformation and fracture in a high temperature environment; it is conducive to subsequent extrusion into wire; wherein too high a variable may cause excessive plastic deformation of the material, causing the grain to grow and reversely coarsen, thereby reducing the strength and toughness of the material, and may also cause quality problems such as cracks and uneven deformation of the material; if the deformation is too low, the expected grain refinement effect may not be achieved, and the performance improvement effect of the material is not obvious. At the same time, problems such as organizational non-uniformity and internal stress may occur, so the deformation is controlled at 30% to 50%.
[0018] Preferably, in step S2, after the upsetting and drawing cycle, the blank needs to be rounded and 100% polished and repaired; by rounding and polishing, the surface of the blank can be made smoother and flatter, surface defects and oxide layers can be removed, the surface quality and the roundness and diameter accuracy of the blank can be improved, the size can be made more precise and meet the required dimensional tolerance, which is beneficial to optimize the internal structure of the blank, further reduce internal stress and improve the uniformity of the structure.
[0019] Preferably, in the step S3, the annealing heat treatment step is to keep the temperature at 960-970°C for 2 hours and then air-cool to room temperature; the annealing heat treatment is performed on the forging billet after upsetting to eliminate the stress and grain boundary degradation generated during the processing and improve the mechanical properties and stability of the alloy.
[0020] Preferably, in the step S4, the diameter of the wire obtained by extrusion is 0.8 to 1.5 mm.
[0021] Preferably, in the step S4, the surface treatment step is to pass the wire through a sizing machine at a uniform speed, and to remove the oxide on the surface of the wire by mechanical means under the condition of a diameter reduction rate of less than 10%; surface treatment of the wire can effectively remove surface oxides, improve the surface quality of the wire, and facilitate subsequent processing and application.
[0022] In a third aspect, the present invention further provides an application of the above-mentioned Ti2AlNb-based alloy wire in arc additive manufacturing, which specifically comprises the following steps:
[0023] A1: Fix the pure titanium substrate, preheat it, install the Ti2AlNb-based alloy wire, and then place it in an inert gas atmosphere;
[0024] A2: Write a scanning path program in the additive manufacturing process, arc melt the Ti2AlNb-based alloy wire and deposit it on a pure titanium substrate to complete the additive manufacturing of a pre-set workpiece shape to obtain an arc additively manufactured workpiece.
[0025] Preferably, the process parameters of the additive manufacturing in the step A2 are: the current of the additive manufacturing machine is 70A to 75A, the wire feeding speed is 700 to 800 mm / min, the scanning speed is 10 to 15 mm / s, the scanning spacing is 1.5 to 2 mm, and the layer thickness is 1.5 to 2 mm.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] 1) The Ti2AlNb-based alloy wire provided by the present invention has been studied in depth on the alloy element content, manufacturing process control and heat treatment process optimization, and the microstructure and high-temperature mechanical properties of the alloy have been systematically tested, and the optimal element composition and preparation process of the alloy have been finally determined. In the casting process, the steps of smelting, ingot casting, round casting, upsetting and drawing cycle, annealing heat treatment, extrusion and surface treatment are optimized, so that the obtained wire structure is uniform, which effectively improves the mechanical properties of the Ti2AlNb alloy welding wire for arc additive manufacturing, and further improves the mechanical properties of the additive manufacturing workpiece;
[0028] 2) In the composition design of the Ti2AlNb-based alloy, the present invention focuses on adding B element and Ta element. The addition of B element may form a strengthening phase at the grain boundary, such as titanium boride, aluminum boride, and niobium boride, which can effectively enhance the strength of the grain boundary and improve the heat resistance and oxidation resistance of the alloy. The addition of Ta element can promote grain boundary migration and grain refinement, which is beneficial to improving the forming quality, plasticity and toughness of the Ti2AlNb-based alloy specimen, thereby improving the tensile resistance of the alloy at high temperature.
[0029] 3) In the additive manufacturing process of the present invention, Ti2AlNb-based alloy wire is directly used for arc melting deposition, which is simple to operate. The room temperature tensile strength of the obtained additive manufacturing sample is 1168MPa, the yield strength is 1078MPa, and the elongation is 7.5%; the high temperature tensile strength at 650°C is 946MPa, the yield strength is 883MPa, and the elongation is 20%. It has good room temperature and high temperature tensile properties and can be applied to the field of aerospace technology with high temperature requirements. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is an optical microscope micrograph of the Ti2AlNb-based alloy wire prepared in Example 1;
[0031] Figure 2 It is a schematic diagram of the preparation process flow of the Ti2AlNb-based alloy wire of the present invention. DETAILED DESCRIPTION
[0032] To make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be described clearly and completely below. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] Example 1
[0034] A method for preparing a Ti2AlNb-based alloy wire comprises the following steps:
[0035] S1: Take 99.7% pure aluminum bars, 99.7% pure niobium chips, 99.7% pure boron powder, 99.7% pure tantalum powder, 99.7% pure titanium blocks, and prepare the raw materials according to the chemical element composition ratio of Ti2AlNb-based alloy wire: Al: 10%, Nb: 43%, B: 0.02%, Ta: 0.01%, and the balance is Ti. Then, place the raw materials in a vacuum suspension melting furnace for melting and casting. The vacuum suspension melting furnace has a preheating power of 200KW and a melting power of 340KW. After the vacuum degree reaches 0.68Pa, argon is filled in. An electromagnetic Stirring device, the parameters of the electromagnetic stirring device are: voltage 380V, current 300A, frequency 5Hz, stirring time 40S, turn on the electromagnetic stirring device after the raw materials are completely melted, and cool in the crucible after stirring to obtain a first-melting ingot; then turn the ingot in the crucible 180 degrees and melt again, turn on the electromagnetic stirring device again after the ingot is completely melted, and cast after stirring to obtain a second-melting ingot; repeat the above process and cast into a final ingot after melting once, and the impurity element content of the ingot after melting is N=0.04%, C=0.08%, H=0.008%, O=0.09%;
[0036] S2: Remove the riser and peel the ingot to obtain a cylindrical ingot of 90mm×400mm, apply an anti-oxidation coating on the surface of the ingot, and then heat and keep it at 1080℃ for 2h. After it comes out of the furnace, it is upsetting and deformed on a forging machine with a deformation of 30%, and then the bar blank is drawn from the middle to the original size, and the upsetting and drawing cycle is repeated three times to obtain a primary forging blank, and after the bar blank is cooled, 100% grinding and repairing is performed; apply an anti-oxidation coating on the surface of the primary forging blank, and then heat and keep it at 950℃ for 2h. After it comes out of the furnace, it is upsetting and deformed on a forging machine with a deformation of 40%, and then the bar blank is drawn from the middle to the original size, and the upsetting and drawing cycle is repeated three times to obtain a final forging blank, and the forging blank is rounded and 100% grinding and repairing is performed after the bar blank is cooled;
[0037] S3: placing the final forging billet in a vacuum heat treatment furnace, heating it to 960°C, keeping it at that temperature for 2 hours, and then air cooling it to room temperature;
[0038] S4: The die used for extrusion is preheated in advance, and the obtained rod blank is extruded into a wire with a diameter of 1.2 mm;
[0039] S5: Surface treatment of the wire, passing the wire through the sizing machine at a uniform speed, and mechanically removing the surface oxides under the condition of a diameter reduction rate of less than 10%, to further improve the dimensional accuracy and roundness of the wire.
[0040] An arc additive manufacturing method using a Ti2AlNb-based alloy wire comprises the following steps:
[0041] A1: Fix the pure titanium substrate, preheat the substrate at 450°C, install the Ti2AlNb-based alloy wire, and perform additive manufacturing in a nitrogen atmosphere;
[0042] A2: Write a scanning path program during the additive manufacturing process, move the welding gun to a height of 10 mm from the substrate, and arc melt the Ti2AlNb-based alloy wire and deposit it on the pure titanium substrate to complete the additive manufacturing of the pre-set workpiece shape to obtain an additively manufactured workpiece; the process parameters of the additive manufacturing method are: the current of the additive manufacturing machine is 70A, the wire feeding speed is 700mm / min, the scanning speed is 10mm / s, the scanning spacing is 1.5mm, and the layer thickness is 1.5mm.
[0043] The additive manufacturing specimens were sampled and tested, and the room temperature tensile strength of the test rods was 1098MPa, the yield strength was 1006MPa, and the elongation was 8%; the high temperature tensile strength at 650°C was 903MPa, the yield strength was 823MPa, and the elongation was 16%.
[0044] Example 2
[0045] A method for preparing a Ti2AlNb-based alloy wire comprises the following steps:
[0046] S1: Take 99.9% pure aluminum bars, 99.9% pure niobium chips, 99.9% pure boron powder, 99.9% pure tantalum powder, 99.9% pure titanium blocks, and prepare the raw materials according to the chemical element composition ratio of Ti2AlNb-based alloy wire: Al: 11%, Nb: 42%, B: 0.05%, Ta: 0.02%, and the balance is Ti. Then, place the raw materials in a vacuum suspension melting furnace for melting and casting. The vacuum suspension melting furnace has a preheating power of 150KW and a melting power of 320KW. After the vacuum degree reaches 0.68Pa, argon is filled in; electromagnetic stirring The parameters of the device are: voltage 380V, current 300A, frequency 5Hz, stirring time 60S, after the raw materials are smelted to be completely melted, the electromagnetic stirring device is turned on, and after stirring, the raw materials are cooled in the crucible to obtain a first-melting ingot; the ingot in the crucible is turned over 180 degrees and smelted again, and the electromagnetic stirring device is turned on again after the ingot is completely melted, and the ingot is cast after stirring to obtain a second-melting ingot; the above process is repeated and the final ingot is cast after one smelting. The impurity element content of the ingot after smelting is N=0.03%, C=0.06%, H=0.006%, and O=0.08%;
[0047] S2: Remove the riser and peel the ingot to obtain a cylindrical ingot of Ф100mm×390mm, apply anti-oxidation coating on the surface of the ingot, then heat and keep it at 1100℃ for 2h, perform upsetting deformation on a forging machine after it comes out of the furnace, and the deformation amount is 35%, then the bar blank is drawn from the middle to the original size, and the upsetting cycle is repeated three times to obtain a primary forging blank, and after the bar blank is cooled, 100% grinding and repairing is performed; apply anti-oxidation coating on the surface of the primary forging blank, then heat and keep it at 960℃ for 2h, and after it comes out of the furnace, perform upsetting deformation on a forging machine, and the deformation amount is 45%, then the bar blank is drawn from the middle to the original size, and the upsetting cycle is repeated three times to obtain a final forging blank, and the forging blank is rounded and 100% grinding and repairing is performed after the bar blank is cooled.
[0048] S3: placing the final forging billet in a vacuum heat treatment furnace, heating it to 970°C, keeping it at that temperature for 1 hour, and then air cooling it to room temperature;
[0049] S4: The die used for extrusion is preheated in advance, and the obtained rod blank is extruded into a wire with a diameter of 0.8 mm;
[0050] S5: Surface treatment of the wire, passing the wire through the sizing machine at a uniform speed, and mechanically removing the surface oxides under the condition of a diameter reduction rate of less than 10%, to further improve the dimensional accuracy and roundness of the wire.
[0051] An arc additive manufacturing method using a Ti2AlNb-based alloy wire comprises the following steps:
[0052] A1: Fix the pure titanium substrate, preheat the substrate at 460°C, install the Ti2AlNb-based alloy wire, and perform additive manufacturing in a nitrogen atmosphere;
[0053] A2: Write a scanning path program during the additive manufacturing process, move the welding gun to a height of 15mm from the substrate, and arc melt the Ti2AlNb-based alloy wire and deposit it on the pure titanium substrate to complete the additive manufacturing of the pre-set workpiece shape to obtain an additively manufactured workpiece; the process parameters of the additive manufacturing method are: the current of the additive manufacturing machine is 75A, the wire feeding speed is 800mm / min, the scanning speed is 15mm / s, the scanning spacing is 2mm, and the layer thickness is 2mm.
[0054] The additive manufacturing specimens were sampled and tested, and the room temperature tensile strength of the test rods was 1168MPa, the yield strength was 1078MPa, and the elongation was 7.5%; the high temperature tensile strength at 650°C was 946MPa, the yield strength was 883MPa, and the elongation was 20%.
[0055] Example 3
[0056] A method for preparing a Ti2AlNb-based alloy wire comprises the following steps:
[0057] S1: Take 99.8% pure aluminum bars, 99.8% pure niobium chips, 99.8% pure boron powder, 99.8% pure tantalum powder, 99.8% pure titanium blocks, and prepare the raw materials according to the chemical element composition ratio of Ti2AlNb-based alloy wire: Al: 10.5%, Nb: 41.5%, B: 0.06%, Ta: 0.03%, and the balance is Ti. Then place the raw materials in a vacuum suspension melting furnace for melting and casting. The preheating power of the vacuum suspension melting furnace is 250KW and the melting power is 400K W, after the vacuum degree reaches 0.68Pa, argon gas is filled; the parameters of the electromagnetic stirring device are: voltage 380V, current 300A, frequency 5Hz, stirring time 30S, the electromagnetic stirring device is turned on after the raw materials are smelted to complete melting, and after stirring, it is cooled in the crucible to obtain a smelting primary ingot; then the ingot in the crucible is turned 180 degrees, and smelted again, and the electromagnetic stirring device is turned on again after the ingot is completely melted, and after stirring, it is cast to obtain a smelting secondary ingot; repeat the above process and then cast it into a final ingot after one smelting;
[0058] S2: Remove the riser and peel the ingot to obtain a cylindrical ingot of Ф110mm×410mm, apply anti-oxidation coating on the surface of the ingot, then heat and keep it at 1050℃ for 2h, perform upsetting deformation on a forging machine after it comes out of the furnace, and the deformation amount is 40%, then the bar blank is drawn from the middle to the original size, and the upsetting cycle is repeated three times to obtain a primary forging blank, and after the bar blank is cooled, 100% grinding and repairing is performed; apply anti-oxidation coating on the surface of the primary forging blank, then heat and keep it at 920℃ for 2h, and after it comes out of the furnace, perform upsetting deformation on a forging machine, and the deformation amount is 50%, then the bar blank is drawn from the middle to the original size, and the upsetting cycle is repeated three times to obtain a final forging blank, and the forging blank is rounded and 100% grinding and repairing is performed after the bar blank is cooled.
[0059] S3: The final forging billet is placed in a vacuum heat treatment furnace, heated to 965°C, kept at this temperature for 3 hours, and then air-cooled to room temperature;
[0060] S4: The die used for extrusion is preheated in advance, and the obtained rod blank is extruded into a wire with a diameter of 1.5 mm;
[0061] S5: Surface treatment of the wire, passing the wire through the sizing machine at a uniform speed, and mechanically removing the surface oxides under the condition of a diameter reduction rate of less than 10%, to further improve the dimensional accuracy and roundness of the wire.
[0062] An arc additive manufacturing method using a Ti2AlNb-based alloy wire comprises the following steps:
[0063] A1: Fix the pure titanium substrate, preheat the substrate at 455°C, install the Ti2AlNb-based alloy wire, and perform additive manufacturing in a nitrogen atmosphere;
[0064] A2: Write a scanning path program in the additive manufacturing process, move the welding gun to a height of 13mm from the substrate, and the Ti2AlNb-based alloy wire is arc-melted and deposited on the pure titanium substrate to complete the additive manufacturing of the pre-set workpiece shape to obtain an additively manufactured workpiece; the process parameters of the additive manufacturing method are: the current of the additive manufacturing machine is 72A, the wire feeding speed is 750mm / min, the scanning speed is 12mm / s, the scanning spacing is 1.8mm, and the layer thickness is 1.8mm.
[0065] The additive manufacturing specimens were sampled and tested. The room temperature tensile strength of the test rods was 1105MPa, the yield strength was 1018MPa, and the elongation was 7.7%; the high temperature tensile strength at 650°C was 923MPa, the yield strength was 852MPa, and the elongation was 18%.
[0066] Comparative Example 1
[0067] A method for preparing a Ti2AlNb-based alloy wire is similar to that of Example 1, except that no Ta element is added to the raw material, and specifically comprises the following steps:
[0068] S1: Take 99.9% pure aluminum bars, 99.9% pure niobium chips, 99.9% pure boron powder, 99.9% pure tantalum powder, 99.9% pure titanium block, and prepare the raw materials according to the chemical element composition ratio of Ti2AlNb-based alloy wire: Al: 11%, Nb: 42%, B: 0.05%, and the balance is Ti. Then put the raw materials into a vacuum suspension melting furnace for melting and casting. The vacuum suspension melting furnace has a preheating power of 200KW, a melting power of 380KW, and a vacuum degree of 1000KW. After reaching 0.68Pa, argon gas is filled; the parameters of the electromagnetic stirring device are: voltage 380V, current 300A, frequency 5Hz, stirring time 60S, the electromagnetic stirring device is turned on after the raw materials are completely melted, and after stirring, the raw materials are cooled in the crucible to obtain a first-melting ingot; the ingot in the crucible is turned 180 degrees and melted again, and the electromagnetic stirring device is turned on again after the ingot is completely melted, and the ingot is cast after stirring to obtain a second-melting ingot; the above process is repeated and then cast into a final ingot after one more melting;
[0069] S2: Remove the riser and peel the ingot to obtain a cylindrical ingot of Ф100mm×390mm, apply anti-oxidation coating on the surface of the ingot, then heat and keep it at 1100℃ for 2h, perform upsetting deformation on a forging machine after it comes out of the furnace, and the deformation amount is 35%, then the bar blank is drawn from the middle to the original size, and the upsetting cycle is repeated three times to obtain a primary forging blank, and after the bar blank is cooled, 100% grinding and repairing is performed; apply anti-oxidation coating on the surface of the primary forging blank, then heat and keep it at 960℃ for 2h, and after it comes out of the furnace, perform upsetting deformation on a forging machine, and the deformation amount is 45%, then the bar blank is drawn from the middle to the original size, and the upsetting cycle is repeated three times to obtain a final forging blank, and the forging blank is rounded and 100% grinding and repairing is performed after the bar blank is cooled.
[0070] S3: placing the final forging billet in a vacuum heat treatment furnace, heating it to 970°C, keeping it at that temperature for 2 hours, and then air cooling it to room temperature;
[0071] S4: The die used for extrusion is preheated in advance, and the obtained rod blank is extruded into a wire with a diameter of 1.2 mm;
[0072] S5: Surface treatment of the wire, passing the wire through the sizing machine at a uniform speed, and mechanically removing the surface oxides under the condition of a diameter reduction rate of less than 10%, to further improve the dimensional accuracy and roundness of the wire.
[0073] An arc additive manufacturing method using a Ti2AlNb-based alloy wire comprises the following steps:
[0074] A1: Fix the pure titanium substrate, preheat the substrate at 455°C, install the Ti2AlNb-based alloy wire, and perform additive manufacturing in a nitrogen atmosphere;
[0075] A2: Write a scanning path program during the additive manufacturing process, move the welding gun to a height of 15mm from the substrate, and arc melt the Ti2AlNb-based alloy wire and deposit it on the pure titanium substrate to complete the additive manufacturing of the pre-set workpiece shape to obtain an additively manufactured workpiece; the process parameters of the additive manufacturing method are: the current of the additive manufacturing machine is 75A, the wire feeding speed is 800mm / min, the scanning speed is 15mm / s, the scanning spacing is 2mm, and the layer thickness is 2mm.
[0076] The additive manufacturing specimens were sampled and tested, and the room temperature tensile strength of the test rods was 852MPa, the yield strength was 741MPa, and the elongation was 6.5%; the high temperature tensile strength at 650℃ was 696MPa, the yield strength was 615MPa, and the elongation was 13%.
[0077] Comparative Example 2
[0078] A method for preparing a Ti2AlNb-based alloy wire is similar to that of Example 1, except that no B element is added to the raw material, and specifically comprises the following steps:
[0079] S1 takes 99.9% pure aluminum bars, 99.9% pure niobium chips, 99.9% pure boron powder, 99.9% pure tantalum powder, 99.9% pure titanium block, and prepares each raw material according to the chemical element composition ratio of Ti2AlNb-based alloy wire: Al: 11%, Nb: 42%, Ta: 0.02%, and the balance is Ti. Then, each raw material is placed in a vacuum suspension melting furnace for melting and casting. The vacuum suspension melting furnace has a preheating power of 200KW, a melting power of 380KW, and a vacuum degree of 1000KW. After reaching 0.68Pa, argon gas is filled; the parameters of the electromagnetic stirring device are: voltage 380V, current 300A, frequency 5Hz, stirring time 60S, the electromagnetic stirring device is turned on after the raw materials are completely melted, and after stirring, the raw materials are cooled in the crucible to obtain a first-melting ingot; the ingot in the crucible is turned 180 degrees and melted again, and the electromagnetic stirring device is turned on again after the ingot is completely melted, and the ingot is cast after stirring to obtain a second-melting ingot; the above process is repeated and then cast into a final ingot after one more melting;
[0080] S2: Remove the riser and peel the ingot to obtain a cylindrical ingot of Ф100mm×390mm, apply anti-oxidation coating on the surface of the ingot, then heat and keep it at 1100℃ for 2h, perform upsetting deformation on a forging machine after it comes out of the furnace, and the deformation amount is 35%, then the bar blank is drawn from the middle to the original size, and the upsetting cycle is repeated three times to obtain a primary forging blank, and after the bar blank is cooled, 100% grinding and repairing is performed; apply anti-oxidation coating on the surface of the primary forging blank, then heat and keep it at 960℃ for 2h, and after it comes out of the furnace, perform upsetting deformation on a forging machine, and the deformation amount is 45%, then the bar blank is drawn from the middle to the original size, and the upsetting cycle is repeated three times to obtain a final forging blank, and the forging blank is rounded and 100% grinding and repairing is performed after the bar blank is cooled.
[0081] S3: placing the final forging billet in a vacuum heat treatment furnace, heating it to 970°C, keeping it at that temperature for 2 hours, and then air cooling it to room temperature;
[0082] S4: The die used for extrusion is preheated in advance, and the obtained rod blank is extruded into a wire with a diameter of 1.2 mm;
[0083] S5: Surface treatment of the wire, passing the wire through the sizing machine at a uniform speed, and mechanically removing the surface oxides under the condition of a diameter reduction rate of less than 10%, to further improve the dimensional accuracy and roundness of the wire.
[0084] An arc additive manufacturing method using a Ti2AlNb-based alloy wire comprises the following steps:
[0085] A1: Fix the pure titanium substrate, preheat the substrate at 460°C, install the Ti2AlNb-based alloy wire, and perform additive manufacturing in a nitrogen atmosphere;
[0086] A2: Write a scanning path program during the additive manufacturing process, move the welding gun to a height of 15mm from the substrate, and arc melt the Ti2AlNb-based alloy wire and deposit it on the pure titanium substrate to complete the additive manufacturing of the pre-set workpiece shape to obtain an additively manufactured workpiece; the process parameters of the additive manufacturing method are: the current of the additive manufacturing machine is 75A, the wire feeding speed is 800mm / min, the scanning speed is 15mm / s, the scanning spacing is 2mm, and the layer thickness is 2mm.
[0087] The additive manufacturing specimens were sampled and tested, and the room temperature tensile strength of the test rods was 808MPa, the yield strength was 726MPa, and the elongation was 6.3%; the high temperature tensile strength at 650°C was 602MPa, the yield strength was 556MPa, and the elongation was 11%.
[0088] Comparative Example 3
[0089] A method for preparing a Ti2AlNb-based alloy wire comprises the following steps:
[0090] S1 takes 99.7% pure aluminum bars, 99.7% pure niobium chips, 99.7% pure boron powder, 99.7% pure tantalum powder, 99.7% pure titanium blocks, and configures each raw material according to the chemical element composition ratio of Ti2AlNb-based alloy wire: Al: 10%, Nb: 43%, B: 0.02%, Ta: 0.01%, and the balance is Ti, and then places each raw material in a vacuum consumable shell furnace for smelting and casting, wherein the vacuum consumable shell furnace has an arc voltage of 50V, an arc current of 2400A, a smelting voltage of 40V, and a smelting current of 10000A. After smelting, the impurity element content of the ingot is N = 0.04%, C = 0.09%, H = 0.012%, and O = 0.13%.
[0091] S2: Remove the riser and peel the ingot to obtain a cylindrical ingot of 90mm×400mm in diameter, apply an anti-oxidation coating on the surface of the ingot, and then heat and keep it at 1080℃ for 2h. After it comes out of the furnace, it is upsetting and deformed on a forging machine with a deformation of 30%. Then, the bar blank is drawn from the middle to the original size. The upsetting and drawing cycle is repeated three times to obtain a primary forging blank. After the bar blank is cooled, 100% grinding and repairing are performed; Anti-oxidation coating is applied on the surface of the primary forging blank, and then it is heated and kept at 950℃ for 2h. After it comes out of the furnace, it is upsetting and deformed on a forging machine with a deformation of 40%. Then, the bar blank is drawn from the middle to the original size. The upsetting and drawing cycle is repeated three times to obtain a final forging blank. The forging blank is rounded and 100% grinding and repairing is performed after the bar blank is cooled;
[0092] S3: The final forging blank is placed in a vacuum heat treatment furnace, heated to 960°C, kept at this temperature for 2 hours, and then air-cooled to room temperature;
[0093] The die used for S4 extrusion is preheated in advance, and the obtained rod blank is extruded into a wire with a diameter of 1.2 mm;
[0094] S5 treats the surface of the wire, allowing the wire to pass through the sizing machine at a uniform speed. Under the condition of a diameter reduction rate of less than 10%, the surface oxide is mechanically removed to further improve the wire size accuracy and roundness.
[0095] An arc additive manufacturing method using a Ti2AlNb-based alloy wire comprises the following steps:
[0096] A1: Fix the pure titanium substrate, preheat the substrate at 450°C, install the Ti2AlNb-based alloy wire, and perform additive manufacturing in a nitrogen atmosphere;
[0097] A2: Write a scanning path program during the additive manufacturing process, move the welding gun to a height of 10 mm from the substrate, and arc melt the Ti2AlNb-based alloy wire and deposit it on the pure titanium substrate to complete the additive manufacturing of the pre-set workpiece shape to obtain an additively manufactured workpiece; the process parameters of the additive manufacturing method are: the current of the additive manufacturing machine is 70A, the wire feeding speed is 700mm / min, the scanning speed is 10mm / s, the scanning spacing is 1.5mm, and the layer thickness is 1.5mm.
[0098] The additive manufacturing specimens were sampled and tested. The room temperature tensile strength of the test rods was 968MPa, the yield strength was 887MPa, and the elongation was 8%; the high temperature tensile strength at 650°C was 789MPa, the yield strength was 721MPa, and the elongation was 15%.
[0099] Comparative Example 4
[0100] A method for preparing a Ti2AlNb-based alloy wire comprises the following steps:
[0101] S1 takes 99.7% pure aluminum bars, 99.7% pure niobium chips, 99.7% pure boron powder, 99.7% pure tantalum powder, 99.7% pure titanium blocks, and configures the raw materials according to the chemical element composition ratio of Ti2AlNb-based alloy wire: Al: 8%, Nb: 50%, B: 0.08%, Ta: 0.05%, and the balance is Ti. Then, the raw materials are placed in a vacuum suspension melting furnace for melting and casting. The vacuum suspension melting furnace has a preheating power of 200KW, a melting power of 200KW, and a vacuum degree of 0.58P a, and then filled with argon gas; an electromagnetic stirring device is placed in the vacuum suspension melting furnace, and the parameters of the electromagnetic stirring device are: voltage 380V, current 300A, frequency 5Hz, stirring time 80S, and the electromagnetic stirring device is turned on after the raw materials are completely melted, and after stirring, the raw materials are cooled in the crucible to obtain a first-melting ingot; the ingot in the crucible is turned 180 degrees and melted again, and the electromagnetic stirring device is turned on again after the ingot is completely melted, and the ingot is cast after stirring to obtain a second-melting ingot; the above process is repeated and then cast into a final ingot after one more melting;
[0102] S2: Remove the riser and peel the ingot to obtain a cylindrical ingot of 90 mm × 400 mm, apply an anti-oxidation coating on the surface of the ingot, and then heat and keep it at 1200 ° C for 2 hours. After it comes out of the furnace, it is upsetting and deformed on a forging machine with a deformation of 20%, and then the bar blank is drawn from the middle to the original size, and the upsetting and drawing cycle is repeated three times to obtain a primary forging blank, and after the bar blank is cooled, 100% grinding and repairing is performed; Anti-oxidation coating is applied to the surface of the primary forging blank, and then it is heated and kept at 800 ° C for 2 hours. After it comes out of the furnace, it is upsetting and deformed on a forging machine with a deformation of 60%, and then the bar blank is drawn from the middle to the original size, and the upsetting and drawing cycle is repeated three times to obtain a final forging blank, and the forging blank is rounded and 100% grinding and repairing is performed after the bar blank is cooled;
[0103] S3: placing the final forging billet in a vacuum heat treatment furnace, heating it to 1100°C, keeping it at that temperature for 2 hours, and then air cooling it to room temperature;
[0104] S4: The die used for extrusion is preheated in advance, and the obtained rod blank is extruded into a wire with a diameter of 1.2 mm;
[0105] S5: Surface treatment of the wire, passing the wire through the sizing machine at a uniform speed, and mechanically removing the surface oxides under the condition of a diameter reduction rate of less than 10%, to further improve the dimensional accuracy and roundness of the wire.
[0106] An arc additive manufacturing method using a Ti2AlNb-based alloy wire comprises the following steps:
[0107] A1: Fix the pure titanium substrate, preheat the substrate at 450°C, install the Ti2AlNb-based alloy wire, and perform additive manufacturing in a nitrogen atmosphere;
[0108] A2: Write a scanning path program during the additive manufacturing process, move the welding gun to a height of 10mm from the substrate, and the Ti2AlNb-based alloy wire is arc-melted and deposited on the pure titanium substrate to complete the additive manufacturing of the pre-set workpiece shape to obtain an additively manufactured workpiece; the process parameters of the additive manufacturing method are: the current of the additive manufacturing machine is 66A, the wire feeding speed is 650mm / min, the scanning speed is 10mm / s, the scanning spacing is 1.5mm, and the layer thickness is 1.5mm.
[0109] The additive manufacturing specimens were sampled and tested. The room temperature tensile strength of the test rods was 621MPa, the yield strength was 503MPa, and the elongation was 5.2%; the high temperature tensile strength at 650°C was 584MPa, the yield strength was 538MPa, and the elongation was 9%.
[0110] In the above embodiments, the chemical composition contents of each alloy are summarized in Table 1:
[0111] Table 1 Chemical composition of the alloy of the present invention (mass fraction, %)
[0112] Al Nb B Ta Ti Example 1 10 43 0.02 0.01 margin Example 2 11 42 0.05 0.02 margin Example 3 10.5 41.5 0.06 0.03 margin Comparative Example 1 11 42 0.05 0 margin Comparative Example 2 11 42 0 0.02 margin Comparative Example 3 10 43 0.02 0.01 margin Comparative Example 4 8 50 0.08 0.05 margin
[0113] The processing parameters of each wire material are summarized in Table 2-4:
[0114] Table 2 Wire smelting process of the present invention
[0115]
[0116]
[0117] Table 3 Wire upsetting and drawing cycle treatment process of the present invention
[0118]
[0119] Table 4 Wire annealing heat treatment process of the present invention
[0120]
[0121]
[0122] The performance tests were carried out on the alloy workpieces obtained in the above embodiments and comparative examples, and the results are shown in Table 5.
[0123] Table 5 Performance test results of alloy workpieces of the present invention
[0124]
[0125] It can be seen from the experimental data in Table 5 that the alloy workpiece prepared by the present invention has mechanical properties both at room temperature and at high temperature.
[0126] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only used to explain the present invention and are not used to limit the present invention.
[0127] The above embodiments are only preferred technical solutions of the present invention and should not be regarded as limiting the present invention. The protection scope of the present invention shall be the technical solutions recorded in the claims, including equivalent replacement solutions of the technical features in the technical solutions recorded in the claims. That is, equivalent replacement improvements within this scope are also within the protection scope of the present invention.
Claims
1. A Ti 2 AlNb based alloy wire, It is characterized in that The invention comprises the following components in percentage by mass: 10-11% Al, 41-43% Nb, 0.02%-0.06% B, 0.01%-0.03% Ta, and the balance is Ti and unavoidable impurities.
2. A Ti as claimed in claim 1 2 Preparation method of AlNb-based alloy wire, It is characterized in that The steps include: S1 according to Ti 2 The AlNb-based alloy wire material is smelted and cast to obtain an ingot according to the composition ratio of each chemical element; S2: processing the ingot obtained in step S1 into a cylindrical ingot and then performing upsetting and drawing cycles at 1050-1100° C. and 920-960° C. to obtain a forging blank; S3 annealing the forged blank after upsetting in step S2; S4 extrudes the forging blank after the heat treatment in step S3 to obtain a wire; S5: The wire obtained in step S4 is subjected to surface treatment to remove oxides on the wire surface, thereby obtaining Ti 2 AlNb based alloy wire.
3. The preparation method according to claim 2, Features: The raw materials in step S1 are aluminum bars with a purity of 99.7% to 99.9%; niobium chips with a purity of 99.7% to 99.9%; boron powder with a purity of 99.7% to 99.9%; tantalum powder with a purity of 99.7% to 99.9%; and titanium blocks with a purity of 99.7% to 99.9%.
4. The preparation method according to claim 2, Features: In the step S1, the smelting step is performed in a vacuum suspension smelting furnace; an electromagnetic stirring device is placed in the vacuum suspension smelting furnace.
5. The preparation method according to claim 2, Features: The specifications of cylindrical ingots are Ф90mm~110mm×390mm~410mm.
6. The preparation method according to claim 2, Features: The number of upsetting and drawing cycles is 2-3 times in each temperature range, and the deformation amount is 30% to 50%.
7. The preparation method according to claim 2 or 6, Features: After the upsetting and drawing cycle, the blank needs to be rounded and 100% polished and repaired.
8. The preparation method according to claim 2, Features: In the step S3, the annealing heat treatment step is to keep the temperature at 960-970°C for 1-3 hours and then air-cool to room temperature.
9. Ti according to claim 1 2 Application of AlNb-based alloy wire in arc additive manufacturing, It is characterized in that The steps include: A1: Fix the pure titanium substrate and preheat it, then install the Ti 2 The AlNb-based alloy wire is then placed in an inert gas atmosphere; A2: Write the scanning path program in the additive manufacturing process and 2 The AlNb-based alloy wire is arc-melted and deposited on a pure titanium substrate to complete additive manufacturing of a pre-set workpiece shape, thereby obtaining an arc additively manufactured workpiece.
10. The use according to claim 9, Features: The process parameters of the additive manufacturing in step A2 are: the current of the additive manufacturing machine is 70A-75A, and the wire feeding speed is 700-800mm / min.
Citation Information
Cited By
Intermediate alloy and preparation method and application thereof
CN119501488A
Additive preparation method of Ti2AlNb alloy with high strength and high plasticity
CN121017569A
A method for additive manufacturing of a Ti2AlNb alloy with high strength and high plasticity
CN121017569B
Welding wire for refining Ti2AlNb alloy weld grains and preparation method
CN121373912A