Polypropylene / polyethylene glycol terephthalate composite dielectric film as well as preparation method and application thereof
Through the melt blending, melt stretching and solid-state stretching processes of polypropylene and polyethylene terephthalate, the phase morphology and crystal structure are optimized, and the low breakdown field strength of polypropylene-based dielectric film is solved. and the problem of high charge and discharge loss, the performance of composite dielectric films with high energy storage and low loss is achieved, and is suitable for polymer film capacitors.
Patent Information
- Application Number
- CN202410934583.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-19
AI Technical Summary
The existing polypropylene-based dielectric film has low breakdown field strength, low energy density and high charge and discharge losses, which limits its miniaturization and integration development in electrical devices and power equipment.
The melt blending, melt stretching and solid-state stretching processes of polypropylene and polyethylene terephthalate are used to optimize their phase morphology and crystal structure to prepare composite media with high breakdown field strength and low loss Electric film.
The breakdown field strength and energy release density of the polypropylene-based composite dielectric film are significantly improved, the leakage current density is reduced, and the performance of high energy storage and low loss is achieved. It is suitable for polymer film capacitors.
Smart Images

Figure CN118977444A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer film capacitors, and in particular to a polypropylene / polyethylene terephthalate composite dielectric film and a preparation method and application thereof. Background Art
[0002] Film capacitors have the advantages of small size, light weight, low loss, stability and reliability, and are widely used in electric vehicles, power distribution systems, renewable energy and various electronic instruments. Typical polymer-based dielectric materials include polypropylene, polyethylene terephthalate, polyvinylidene fluoride, etc. Among them, biaxially stretched polypropylene has the advantages of excellent self-healing properties, ultra-low dielectric loss and extremely high breakdown field strength, and has become the most widely used capacitor dielectric in the market. However, the inherent defect of low energy density has become the main factor hindering its further development. The energy density of polypropylene-based dielectric films can be improved by grafting polar functional groups or incorporating high dielectric constant nanofillers, but these modification methods have the disadvantages of low film production efficiency and high preparation cost, and cannot meet the needs of industrialization. In addition, compared with linear dielectrics such as polypropylene, the charge and discharge loss of composite dielectrics is still high, and the organic-inorganic interface defects are not conducive to the improvement of breakdown field strength. In comparison, the all-organic blend system has natural advantages in the large-scale preparation of thin films and the quality control of ultra-thin films, and the phase morphology and crystal structure regulation can well achieve the customization of dielectric properties. Therefore, how to design the phase morphology and crystal structure of the all-organic blend system to maximize its performance advantages becomes the key to improving the performance upper limit of all-organic composite dielectrics and preparing high-energy storage, low-loss polymer dielectric materials. Summary of the invention
[0003] The present invention provides a polypropylene / polyethylene terephthalate composite dielectric film and a preparation method and application thereof, aiming to solve the problems of low breakdown field strength, low energy density and high charge and discharge loss in the existing composite dielectric film.
[0004] In order to achieve the above object, the present invention adopts the following technical solutions to achieve it.
[0005] A first aspect of the present invention provides a method for preparing a polypropylene / polyethylene terephthalate composite dielectric film, comprising:
[0006] (1) preparing polypropylene / polyethylene terephthalate composite pellets: melt-blending polypropylene and polyethylene terephthalate, and pelletizing to obtain polypropylene / polyethylene terephthalate composite pellets;
[0007] Wherein, the content of polyethylene terephthalate is 1 to 30 wt%.
[0008] (2) preparing a primary composite film: extruding and casting the polypropylene / polyethylene terephthalate composite pellets, and then melt stretching the composite pellets at a melt stretching ratio of 5 to 60, and then cooling and winding the composite pellets to obtain a primary composite film;
[0009] The melt stretch ratio is the ratio of the cross-sectional area of the free cast film to the cross-sectional area of the extrusion cast film.
[0010] (3) solid-state stretching the primary composite film under heating conditions, with a solid-state stretching ratio of 1 to 5, to obtain a polypropylene / polyethylene terephthalate composite dielectric film;
[0011] The solid-state stretching ratio is the ratio of the linear speed of the stretching roller to the linear speed of the preheating roller.
[0012] In some embodiments, the melt blending temperature is 140-280°C.
[0013] In some embodiments, the extrusion casting temperature is 140-280°C.
[0014] In some embodiments, the primary composite film is heated to a temperature of 80-150°C.
[0015] In some embodiments, the polypropylene includes any one or more of homopolypropylene, copolymer polypropylene, and polypropylene derivatives.
[0016] In some embodiments, the polypropylene has a melt index of 1 to 5 g / 10 min at 230° C.×2.16 kg load.
[0017] In some embodiments, the polyethylene terephthalate has an intrinsic viscosity of 0.5 to 1 dL / g as measured according to GB / T14190.
[0018] The second aspect of the present invention provides a polypropylene / polyethylene terephthalate composite dielectric film prepared by the above preparation method.
[0019] The third aspect of the present invention provides the use of the above-mentioned polypropylene / polyethylene terephthalate composite dielectric film in a polymer film capacitor.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] The preparation method of the present invention adopts melt blending, melt stretching and solid-state stretching processes, and has a simple process, low production cost and easy continuous production. After melt stretching treatment, the spherical polyethylene terephthalate particles undergo a phase morphology transformation from spherical to micron fibers; after further solid-state stretching treatment, the fiber morphology is optimized and the polypropylene crystal structure is further improved. This preparation method can greatly reduce the leakage current density, thereby improving the breakdown field strength and charge and discharge efficiency, so that the film has excellent energy storage performance.
[0022] The polypropylene / polyethylene terephthalate composite dielectric film prepared by the present invention has the characteristics of good insulation performance, high energy density, and low charge and discharge loss. Its breakdown field strength can reach 672.2MV / m, and its energy release density can reach 4.11J / cm 3 , the energy release efficiency is as high as 92.8%, and it has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. The drawings described below are only some embodiments recorded in the present invention, which are used to provide a further understanding of the embodiments of the present invention, constitute a part of the present invention, and do not constitute a limitation of the embodiments of the present invention. In the drawings:
[0024] Figure 1 This is a scanning electron micrograph of a cross section of a polypropylene / polyethylene terephthalate composite dielectric film prepared in Comparative Example 1 of the present invention after low temperature quenching;
[0025] Figure 2 A scanning electron micrograph of a cross section of a polypropylene / polyethylene terephthalate composite dielectric film prepared in Example 1 of the present invention after low temperature quenching;
[0026] Figure 3 This is a scanning electron micrograph of fibers of the polypropylene / polyethylene terephthalate composite film prepared in Example 1 of the present invention after being etched with xylene;
[0027] Figure 4 The wide-angle X-ray diffraction patterns of the polypropylene / polyethylene terephthalate composite films prepared in Example 1 of the present invention and Comparative Example 1;
[0028] Figure 5 This is a performance comparison chart of the polypropylene / polyethylene terephthalate composite films prepared in Example 1 of the present invention and Comparative Example 1. DETAILED DESCRIPTION
[0029] The specific implementation of the present invention is described in detail below in conjunction with specific examples. It should be understood that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Non-essential improvements and adjustments made to the present invention by technicians in this field based on the above invention content still belong to the scope of protection of the present invention.
[0030] The low energy release density of polypropylene dielectric films limits the miniaturization and integration of electronic devices and power equipment. At present, adding high dielectric constant inorganic fillers is a conventional method to improve the energy release density of polypropylene-based dielectric films, but it has disadvantages such as low film production efficiency and high preparation cost, and cannot meet the needs of industrialization. In addition, compared with linear dielectrics such as polypropylene, the charge and discharge losses of composite dielectrics are still relatively high, and organic-inorganic interface defects are not conducive to the improvement of breakdown field strength. In comparison, all-organic blend systems have natural advantages in industrial applications and film quality control, and the regulation of phase morphology and crystal structure can well achieve customized dielectric properties.
[0031] Based on this, the first aspect of the present invention provides a method for preparing a polypropylene / polyethylene terephthalate composite dielectric film, comprising:
[0032] (1) preparing polypropylene / polyethylene terephthalate composite pellets: melt-blending polypropylene and polyethylene terephthalate, and pelletizing to obtain polypropylene / polyethylene terephthalate composite pellets;
[0033] Wherein, the content of polyethylene terephthalate is 1 to 30 wt%.
[0034] (2) preparing a primary composite film: extruding and casting the polypropylene / polyethylene terephthalate composite pellets, and then melt stretching the composite pellets at a melt stretching ratio of 5 to 60, and then cooling and winding the composite pellets to obtain a primary composite film;
[0035] The melt stretch ratio is the ratio of the cross-sectional area of the free cast film to the cross-sectional area of the extrusion cast film.
[0036] (3) solid-state stretching the primary composite film under heating conditions, with a solid-state stretching ratio of 1 to 5, to obtain a polypropylene / polyethylene terephthalate composite dielectric film;
[0037] The solid-state stretching ratio is the ratio of the linear speed of the stretching roller to the linear speed of the preheating roller.
[0038] The physicochemical properties and component content of the dispersed phase of the all-organic polypropylene-based composite dielectric are important reasons that affect its dielectric properties. Based on rich experience and a large number of experiments, the inventors of this application have found that using polypropylene in a specific melt index range as the matrix, polyethylene terephthalate in a specific characteristic viscosity range as the dispersed phase, and assisted by melt stretching and solid-state stretching under heating conditions, can achieve the coordinated optimization of polyethylene terephthalate phase morphology and film interface polarization, and significantly inhibit the carrier transport of the composite dielectric. In addition, the dispersed phase morphology and interface polarization strength can be well regulated by adjusting process parameters such as component content, melt stretching ratio, solid-state stretching temperature and solid-state stretching ratio, thereby achieving customization of the dielectric properties of the composite dielectric.
[0039] In summary, the present invention can optimize the dielectric properties of polypropylene and prepare a high-energy storage, low-loss polypropylene-based composite dielectric by selecting polypropylene as the matrix and polyethylene terephthalate as the dispersed phase, and by reasonably regulating process parameters such as component content, melt stretching ratio, solid-state stretching temperature and solid-state stretching ratio.
[0040] According to some specific embodiments of the present invention, the component content of the polyethylene terephthalate can be selected from any value between 1 and 30wt%. Specifically, the component content of the polyethylene terephthalate includes but is not limited to 1wt%, 1.5wt%, 2wt%, 3wt%, 4wt%, 5wt%, 7wt%, 8wt%, 10.8wt%, 13.7wt%, 16.3wt%, 18wt%, 22wt%, 25wt% or 30wt%.
[0041] According to some specific embodiments of the present invention, the temperature of the melt blending is 140 to 280° C. Specifically, the temperature for melt blending includes but is not limited to 140° C., 160° C., 180° C., 200° C., 220° C., 240° C., 260° C., 261° C., 262° C., 263° C., 264° C., 265° C., 266° C., 267° C., 268° C., 269° C., 270° C., 271° C., 272° C., 273° C., 274° C., 275° C., 276° C., 277° C., 278° C., 279° C. or 280° C.
[0042] According to some specific embodiments of the present invention, wherein the extrusion casting temperature is 140-280° C. Specifically, the temperature for extrusion casting includes but is not limited to 140° C., 160° C., 180° C., 200° C., 220° C., 240° C., 260° C., 261° C., 262° C., 263° C., 264° C., 265° C., 266° C., 267° C., 268° C., 269° C., 270° C., 271° C., 272° C., 273° C., 274° C., 275° C., 276° C., 277° C., 278° C., 279° C. or 280° C.
[0043] According to some specific embodiments of the present invention, the melt stretching ratio is 5 to 60. Specifically, the melt stretching ratio includes but is not limited to 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55 or 60.
[0044] According to some specific embodiments of the present invention, the temperature at which the primary film is heated is 80-150° C. Specifically, the temperature at which the primary film is heated includes but is not limited to 80° C., 85° C., 90° C., 95° C., 100° C., 105° C., 110° C., 115° C., 120° C., 125° C., 130° C., 135° C., 140° C., 145° C. or 150° C.
[0045] According to some specific embodiments of the present invention, the solid-state stretching ratio is 1 to 5. Specifically, the melt stretching ratio includes but is not limited to 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5 or 5.
[0046] According to some specific embodiments of the present invention, the polypropylene includes any one or more of homopolypropylene, copolymer polypropylene and polypropylene derivatives. It can be understood that any polymer prepared with propylene as a single polymerization monomer or one of the polymerization monomers can be used as the matrix of the composite dielectric in the present invention. Specifically, it includes but is not limited to one or more of homopolypropylene, random copolymer polypropylene, block copolymer polypropylene, polypropylene grafted with maleic anhydride, polypropylene grafted with styrene, and polypropylene grafted with methyl methacrylate.
[0047] According to some specific embodiments of the present invention, the melt index of the polypropylene at 230°C×2.16kg load is 1-5g / 10min. Specifically, the melt index of the polypropylene at 230°C×2.16kg load includes but is not limited to 1g / 10min, 2g / 10min, 3g / 10min, 4g / 10min or 5g / 10min.
[0048] According to some specific embodiments of the present invention, the intrinsic viscosity of the polyethylene terephthalate measured according to GB / T14190 is 0.5-1dL / g. Specifically, the intrinsic viscosity of the polyethylene terephthalate includes but is not limited to 0.5dL / g, 0.6dL / g, 0.7dL / g, 0.8dL / g, 0.9dL / g or 1dL / g.
[0049] The second aspect of the present invention provides a polypropylene / polyethylene terephthalate composite dielectric film prepared by the above preparation method.
[0050] The third aspect of the present invention provides the use of the above-mentioned polypropylene / polyethylene terephthalate composite dielectric film in a polymer film capacitor.
[0051] The polypropylene / polyethylene terephthalate composite dielectric film provided by the present invention has excellent breakdown field strength, energy release density and energy release efficiency, and can meet the performance requirements of high energy storage and low loss dielectric films.
[0052] Unless otherwise defined, the technical terms used in the following examples have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. The test reagents used in the following examples, unless otherwise specified, are all conventional biochemical reagents; the experimental methods, unless otherwise specified, are all conventional methods.
[0053] Example 1
[0054] Weigh 950g of polypropylene and 50g of polyethylene terephthalate and place them in a twin-screw extruder for melt blending. The melt index of polypropylene at 230℃×2.16kg load is 3.3g / 10min, and the intrinsic viscosity of polyethylene terephthalate measured according to GB / T14190 is 0.7dL / g. The melt blending process is: extrusion temperature 275℃, screw speed 200rpm, pelletizing and drying to obtain polypropylene / polyethylene terephthalate composite pellets. The composite pellets are placed in an extrusion casting machine with an extrusion temperature of 275℃, a screw speed of 50rpm, a melt stretch ratio of 30, and cooling and winding to obtain a polypropylene / polyethylene terephthalate primary composite film. Finally, the obtained polypropylene / polyethylene terephthalate primary composite film is heated to 130° C. and solid-state stretched with a solid-state stretching ratio of 2. After winding, the final composite film, namely, the polypropylene / polyethylene terephthalate composite dielectric film, is obtained.
[0055] Example 2
[0056] 990g of polypropylene and 10g of polyethylene terephthalate were weighed and placed in a twin-screw extruder for melt blending. The melt index of polypropylene at 230°C × 2.16kg load was 3.3g / 10min, and the intrinsic viscosity of polyethylene terephthalate measured according to GB / T14190 was 0.7dL / g. The melt blending process was as follows: extrusion temperature 275°C, screw speed 200rpm, pelletizing and drying to obtain polypropylene / polyethylene terephthalate composite pellets. The composite pellets were placed in an extrusion casting machine with an extrusion temperature of 275°C, a screw speed of 50rpm, a melt stretch ratio of 30, and cooling and winding to obtain a polypropylene / polyethylene terephthalate primary composite film. Finally, the obtained polypropylene / polyethylene terephthalate primary composite film is heated to 130° C. and solid-state stretched with a solid-state stretching ratio of 2. After winding, the final composite film, namely, the polypropylene / polyethylene terephthalate composite dielectric film, is obtained.
[0057] Example 3
[0058] 700g of polypropylene and 300g of polyethylene terephthalate were weighed and placed in a twin-screw extruder for melt blending. The melt index of polypropylene at 230°C × 2.16kg load was 3.3g / 10min, and the intrinsic viscosity of polyethylene terephthalate measured according to GB / T14190 was 0.7dL / g. The melt blending process was as follows: extrusion temperature 275°C, screw speed 200rpm, pelletizing and drying to obtain polypropylene / polyethylene terephthalate composite pellets. The composite pellets were placed in an extrusion casting machine with an extrusion temperature of 275°C, a screw speed of 50rpm, a melt stretch ratio of 30, and cooling and winding to obtain a polypropylene / polyethylene terephthalate primary composite film. Finally, the obtained polypropylene / polyethylene terephthalate primary composite film is heated to 130° C. and solid-state stretched with a solid-state stretching ratio of 2. After winding, the final composite film, namely, the polypropylene / polyethylene terephthalate composite dielectric film, is obtained.
[0059] Example 4
[0060] 950g of polypropylene and 50g of polyethylene terephthalate were weighed and placed in a twin-screw extruder for melt blending. The melt index of polypropylene at 230°C × 2.16kg load was 3.3g / 10min, and the intrinsic viscosity of polyethylene terephthalate measured according to GB / T14190 was 0.7dL / g. The melt blending process was as follows: extrusion temperature 275°C, screw speed 200rpm, pelletizing and drying to obtain polypropylene / polyethylene terephthalate composite pellets. The composite pellets were placed in an extrusion casting machine with an extrusion temperature of 275°C, a screw speed of 50rpm, a melt stretch ratio of 5, and cooling and winding to obtain a polypropylene / polyethylene terephthalate primary composite film. Finally, the obtained polypropylene / polyethylene terephthalate primary composite film is heated to 130° C. and solid-state stretched with a solid-state stretching ratio of 2. After winding, the final composite film, namely, the polypropylene / polyethylene terephthalate composite dielectric film, is obtained.
[0061] Example 5
[0062] Weigh 950g of polypropylene and 50g of polyethylene terephthalate and place them in a twin-screw extruder for melt blending. The melt index of polypropylene at 230℃×2.16kg load is 3.3g / 10min, and the intrinsic viscosity of polyethylene terephthalate measured according to GB / T14190 is 0.7dL / g. The melt blending process is: extrusion temperature 275℃, screw speed 200rpm, pelletizing and drying to obtain polypropylene / polyethylene terephthalate composite pellets. The composite pellets are placed in an extrusion casting machine with an extrusion temperature of 275℃, a screw speed of 50rpm, a melt stretch ratio of 60, and cooling and winding to obtain a polypropylene / polyethylene terephthalate primary composite film. Finally, the obtained polypropylene / polyethylene terephthalate primary composite film is heated to 130° C. and solid-state stretched with a solid-state stretching ratio of 2. After winding, the final composite film, namely, the polypropylene / polyethylene terephthalate composite dielectric film, is obtained.
[0063] Example 6
[0064] Weigh 950g of polypropylene and 50g of polyethylene terephthalate and place them in a twin-screw extruder for melt blending. The melt index of polypropylene at 230℃×2.16kg load is 3.3g / 10min, and the intrinsic viscosity of polyethylene terephthalate measured according to GB / T14190 is 0.7dL / g. The melt blending process is: extrusion temperature 275℃, screw speed 200rpm, pelletizing and drying to obtain polypropylene / polyethylene terephthalate composite pellets. The composite pellets are placed in an extrusion casting machine with an extrusion temperature of 275℃, a screw speed of 50rpm, a melt stretch ratio of 30, and cooling and winding to obtain a polypropylene / polyethylene terephthalate primary composite film. Finally, the obtained polypropylene / polyethylene terephthalate primary composite film is heated to 80° C. and solid-state stretched with a solid-state stretching ratio of 2. After winding, the final composite film, ie, the polypropylene / polyethylene terephthalate composite dielectric film, is obtained.
[0065] Example 7
[0066] Weigh 950g of polypropylene and 50g of polyethylene terephthalate and place them in a twin-screw extruder for melt blending. The melt index of polypropylene at 230℃×2.16kg load is 3.3g / 10min, and the intrinsic viscosity of polyethylene terephthalate measured according to GB / T14190 is 0.7dL / g. The melt blending process is: extrusion temperature 275℃, screw speed 200rpm, pelletizing and drying to obtain polypropylene / polyethylene terephthalate composite pellets. The composite pellets are placed in an extrusion casting machine with an extrusion temperature of 275℃, a screw speed of 50rpm, a melt stretch ratio of 30, and cooling and winding to obtain a polypropylene / polyethylene terephthalate primary composite film. Finally, the obtained polypropylene / polyethylene terephthalate primary composite film is heated to 150° C. and solid-state stretched with a solid-state stretching ratio of 2. After winding, the final composite film, ie, the polypropylene / polyethylene terephthalate composite dielectric film, is obtained.
[0067] Example 8
[0068] Weigh 950g of polypropylene and 50g of polyethylene terephthalate and place them in a twin-screw extruder for melt blending. The melt index of polypropylene at 230℃×2.16kg load is 3.3g / 10min, and the intrinsic viscosity of polyethylene terephthalate measured according to GB / T14190 is 0.7dL / g. The melt blending process is: extrusion temperature 275℃, screw speed 200rpm, pelletizing and drying to obtain polypropylene / polyethylene terephthalate composite pellets. The composite pellets are placed in an extrusion casting machine with an extrusion temperature of 275℃, a screw speed of 50rpm, a melt stretch ratio of 30, and cooling and winding to obtain a polypropylene / polyethylene terephthalate primary composite film. Finally, the obtained polypropylene / polyethylene terephthalate primary composite film is heated to 130° C. and solid-state stretched with a solid-state stretching ratio of 1. After winding, the final composite film, namely the polypropylene / polyethylene terephthalate composite dielectric film, is obtained.
[0069] Example 9
[0070] Weigh 950g of polypropylene and 50g of polyethylene terephthalate and place them in a twin-screw extruder for melt blending. The melt index of polypropylene at 230℃×2.16kg load is 3.3g / 10min, and the intrinsic viscosity of polyethylene terephthalate measured according to GB / T14190 is 0.7dL / g. The melt blending process is: extrusion temperature 275℃, screw speed 200rpm, pelletizing and drying to obtain polypropylene / polyethylene terephthalate composite pellets. The composite pellets are placed in an extrusion casting machine with an extrusion temperature of 275℃, a screw speed of 50rpm, a melt stretch ratio of 30, and cooling and winding to obtain a polypropylene / polyethylene terephthalate primary composite film. Finally, the obtained polypropylene / polyethylene terephthalate primary composite film is heated to 130° C. and solid-state stretched with a solid-state stretching ratio of 5. After winding, the final composite film, namely, the polypropylene / polyethylene terephthalate composite dielectric film, is obtained.
[0071] Comparative Example 1
[0072] 950g of polypropylene and 50g of polyethylene terephthalate were weighed and placed in a twin-screw extruder for melt blending. Among them, the melt index of polypropylene at 230℃×2.16kg load is 3.3g / 10min, and the intrinsic viscosity of polyethylene terephthalate measured according to GB / T14190 is 0.7dL / g. The melt blending process is: extrusion temperature 275℃, screw speed 200rpm, pelletizing and drying to obtain polypropylene / polyethylene terephthalate composite pellets. The polypropylene / polyethylene terephthalate composite pellets were preheated at 200℃ for 15min by hot pressing molding equipment, then hot pressed for 5min under the conditions of pressure of 15MPa and temperature of 200℃, and finally cold pressed for 5min under the conditions of pressure of 15MPa to obtain a polypropylene / polyethylene terephthalate composite dielectric film.
[0073] Comparative Example 2
[0074] Weigh 950g of polypropylene and 50g of polyethylene terephthalate and place them in a twin-screw extruder for melt blending. The melt index of polypropylene at 230℃×2.16kg load is 3.3g / 10min, and the intrinsic viscosity of polyethylene terephthalate measured according to GB / T14190 is 0.7dL / g. The melt blending process is: extrusion temperature 275℃, screw speed 200rpm, pelletizing and drying to obtain polypropylene / polyethylene terephthalate composite pellets. The composite pellets are placed in an extrusion casting machine with an extrusion temperature of 275℃, a screw speed of 50rpm, a melt stretch ratio of 2, and cooling and winding to obtain a polypropylene / polyethylene terephthalate primary composite film. Finally, the obtained polypropylene / polyethylene terephthalate primary composite film is heated to 130° C. and solid-state stretched with a solid-state stretching ratio of 2. After winding, the final composite film, namely, the polypropylene / polyethylene terephthalate composite dielectric film, is obtained.
[0075] Comparative Example 3
[0076] Weigh 950g of polypropylene and 50g of polyethylene terephthalate and place them in a twin-screw extruder for melt blending. The melt index of polypropylene at 230℃×2.16kg load is 3.3g / 10min, and the intrinsic viscosity of polyethylene terephthalate measured according to GB / T14190 is 0.7dL / g. The melt blending process is: extrusion temperature 275℃, screw speed 200rpm, pelletizing and drying to obtain polypropylene / polyethylene terephthalate composite pellets. The composite pellets are placed in an extrusion casting machine with an extrusion temperature of 275℃, a screw speed of 50rpm, a melt stretch ratio of 30, and cooling and winding to obtain a polypropylene / polyethylene terephthalate primary composite film. Finally, the obtained polypropylene / polyethylene terephthalate primary composite film is heated to 50° C. and solid-state stretched with a solid-state stretching ratio of 2. After winding, the final composite film, ie, the polypropylene / polyethylene terephthalate composite dielectric film, is obtained.
[0077] Comparative Example 4
[0078] Weigh 950g of polypropylene and 50g of polyethylene terephthalate and place them in a twin-screw extruder for melt blending. The melt index of polypropylene at 230℃×2.16kg load is 3.3g / 10min, and the intrinsic viscosity of polyethylene terephthalate measured according to GB / T14190 is 0.7dL / g. The melt blending process is: extrusion temperature 275℃, screw speed 200rpm, pelletizing and drying to obtain polypropylene / polyethylene terephthalate composite pellets. The composite pellets are placed in an extrusion casting machine with an extrusion temperature of 275℃, a screw speed of 50rpm, a melt stretch ratio of 30, and cooling and winding to obtain a polypropylene / polyethylene terephthalate primary composite film. Finally, the obtained polypropylene / polyethylene terephthalate primary composite film is heated to 130° C. and solid-state stretched with a solid-state stretching ratio of 8. After winding, the final composite film, namely the polypropylene / polyethylene terephthalate composite dielectric film, is obtained.
[0079] Comparative Example 5
[0080] Weigh 950g of polypropylene and 50g of polyethylene terephthalate and place them in a twin-screw extruder for melt blending. The melt index of polypropylene at 230℃×2.16kg load is 8g / 10min, and the intrinsic viscosity of polyethylene terephthalate measured according to GB / T14190 is 0.7dL / g. The melt blending process is: extrusion temperature 275℃, screw speed 200rpm, pelletizing and drying to obtain polypropylene / polyethylene terephthalate composite pellets. The composite pellets are placed in an extrusion casting machine with an extrusion temperature of 275℃, a screw speed of 50rpm, a melt stretch ratio of 30, and cooling and winding to obtain a polypropylene / polyethylene terephthalate primary composite film. Finally, the obtained polypropylene / polyethylene terephthalate primary composite film is heated to 130° C. and solid-state stretched with a solid-state stretching ratio of 2. After winding, the final composite film, namely, the polypropylene / polyethylene terephthalate composite dielectric film, is obtained.
[0081] Comparative Example 6
[0082] Weigh 950g of polypropylene and 50g of polyethylene terephthalate and place them in a twin-screw extruder for melt blending. The melt index of polypropylene at 230℃×2.16kg load is 3.3g / 10min, and the intrinsic viscosity of polyethylene terephthalate measured according to GB / T14190 is 1.1dL / g. The melt blending process is: extrusion temperature 275℃, screw speed 200rpm, pelletizing and drying to obtain polypropylene / polyethylene terephthalate composite pellets. The composite pellets are placed in an extrusion casting machine with an extrusion temperature of 275℃, a screw speed of 50rpm, a melt stretch ratio of 30, and cooling and winding to obtain a polypropylene / polyethylene terephthalate primary composite film. Finally, the obtained polypropylene / polyethylene terephthalate primary composite film is heated to 130° C. and solid-state stretched with a solid-state stretching ratio of 2. After winding, the final composite film, namely, the polypropylene / polyethylene terephthalate composite dielectric film, is obtained.
[0083] The proportions and process parameters of Examples 1-9 and Comparative Examples 1-6 are shown in Table 1.
[0084] Table 1 Preparation process conditions of Examples 1-9 and Comparative Examples 1-6
[0085]
[0086]
[0087] The properties of the polypropylene / polyethylene terephthalate composite dielectric films prepared in Examples 1-9 and Comparative Examples 1-6 were characterized as follows:
[0088] The dielectric properties of the composite dielectric film were tested using a broadband dielectric spectrometer (Concept 50, Novocontrol GmbH, Germany), the withstand voltage of the composite dielectric film was tested using a withstand voltage tester (19057 20, Chroma, China), and the leakage current density and energy storage performance of the composite dielectric film were tested using a high voltage ferroelectric test system (Premier II, Radiant Technologies, Inc., USA). The test results are shown in Table 2.
[0089] Table 2 Performance data of Examples 1-9 and Comparative Examples 1-6
[0090]
[0091]
[0092] It can be seen from the test results in Table 2 that, compared with the composite dielectric film sample prepared by hot pressing molding in Comparative Example 1, the composite dielectric film prepared by extrusion casting and solid-state stretching under heating conditions in the present invention has a higher breakdown field strength and a lower leakage current density, showing better insulation performance and electric energy storage capacity. Among them, the polyethylene terephthalate content, melt stretching ratio, solid-state stretching temperature and solid-state stretching ratio have a greater influence on the performance of the composite dielectric film. When the polyethylene terephthalate content is low, such as in Example 2, its breakdown field strength and energy release density are reduced; when the polyethylene terephthalate content is high, such as in Example 3, its dielectric constant is high, but the breakdown field strength, energy release density and energy release efficiency are significantly reduced, and the leakage current density is significantly increased; when the melt stretching is relatively small, such as in Example 4, its breakdown field strength and energy release density both decrease; when the solid-state stretching temperature is too low, such as in Example 6, its breakdown field strength decreases; when the solid-state stretching is relatively large, such as in Example 9, its breakdown field strength decreases and the energy release density both decrease significantly; when the polyethylene terephthalate content, melt stretching ratio, solid-state stretching temperature and solid-state stretching ratio are moderate, such as in Example 1, Example 5, Example 7 and Example 8, the prepared composite dielectric film has excellent insulation properties and electrical energy storage capacity, among which the performance of Example 1 is the best.
[0093] In Comparative Example 1, due to the insufficient compatibility between polypropylene and polyethylene terephthalate, the polyethylene terephthalate phase in the thermoformed polypropylene / polyethylene terephthalate composite film is dispersed in the polypropylene matrix in the form of spherical particles, and its breakdown field strength is only 416.9 MV / m, and the leakage current density is as high as 9.6×10 -9 A / cm 2 , the energy release efficiency density and energy release efficiency are the lowest, only 1.5J / cm 3and 80.3%. In Example 1, after melt stretching and solid-state stretching under heating conditions, the spherical particles undergo a phase transformation and evolve into micron fibers, and the interface defects between polypropylene and are also significantly improved. Its breakdown field strength is as high as 672.2MV / m, and the leakage current density is only 0.6×10 -9 A / cm 2 , showing excellent insulation properties and the ability to limit carrier transport, so the energy release density is as high as 4.1J / cm 3 , the energy release efficiency is also as high as 92.8%.
[0094] The melt stretching ratio of Comparative Example 2 is too low, and the breakdown field strength of the composite dielectric film prepared therefrom is low, and the leakage current density is high, resulting in low energy release density and energy release efficiency of the composite dielectric film prepared therefrom. The solid-state stretching temperature of Comparative Example 3 is too low, and the breakdown field strength and energy release density of the composite dielectric film prepared therefrom are low. The solid-state stretching ratio of Comparative Example 4 is too high, and its breakdown field strength and energy release density are both low, wherein the breakdown field strength is only 402.1MV / m. The polypropylene melt index of Comparative Example 5 is too high, and the film-forming quality is poor, resulting in low breakdown field strength, energy release density and energy release efficiency of the composite dielectric film. The polyethylene terephthalate characteristic viscosity of Comparative Example 6 is too large, and it is not easy to deform under the melt stretching external field during the extrusion casting process, resulting in low breakdown field strength, energy release density and energy release efficiency of the composite dielectric film. Within the process parameter range of the present invention, the prepared polypropylene / polyethylene terephthalate composite dielectric film has good comprehensive performance.
[0095] The polypropylene / polyethylene terephthalate composite dielectric films prepared in Example 1 and Comparative Example 1 were tested by scanning electron microscopy to observe their microscopic morphologies. Figure 1 This is a scanning electron microscope photograph of a cross section of a polypropylene / polyethylene terephthalate composite dielectric film of Comparative Example 1 after low temperature quenching; Figure 2The scanning electron microscope photograph of the cross section of the polypropylene / polyethylene terephthalate composite dielectric film of Example 1 after low temperature quenching. In the polypropylene / polyethylene terephthalate composite dielectric film of Comparative Example 1, the polyethylene terephthalate phase is dispersed in the polypropylene matrix in the form of spherical particles. In the polypropylene / polyethylene terephthalate composite dielectric film of Example 1, after melt stretching and solid-state stretching treatment under heating conditions, the spherical polyethylene terephthalate particles undergo a phase morphology transformation from spherical to micron fibers, and the interface defects between the polypropylene and polyethylene terephthalate phases are also significantly improved. Moreover, the interface between the fiber and the polypropylene matrix is parallel to the film surface, which is conducive to suppressing carrier transport under an external electric field, thereby increasing the breakdown field strength, suppressing the leakage current density and charge and discharge losses, and making the film have excellent insulation properties and electrical energy storage capacity.
[0096] Figure 3 This is a scanning electron microscope photograph of the fiber of the polypropylene / polyethylene terephthalate composite dielectric film of Example 1 after being etched with xylene. Figure 3 It can be seen that after melt stretching and solid-state stretching under heating conditions, the polyethylene terephthalate dispersed phase is in a fibrous state.
[0097] The crystal structure of the polypropylene / polyethylene terephthalate composite dielectric film prepared in Example 1 and Comparative Example 1 was tested by wide-angle X-ray diffraction characterization method. The results are as follows: Figure 4 As shown. The wide-angle X-ray diffraction results of Example 1 and Comparative Example 1 both show the lamellae signal of polypropylene, wherein the diffraction rings of the film of Comparative Example 1 are isotropic, indicating that the polypropylene lamellae inside the film are not oriented. The diffraction rings of the film of Example 1 are concentrated in the horizontal direction, indicating that the polypropylene lamellae are oriented along the stretching direction of the film. It is generally believed that such oriented lamellae are conducive to suppressing carrier transport under the electric field, thereby improving the breakdown field strength and energy release efficiency of the film.
[0098] Figure 5 1 is a performance comparison chart of the polypropylene / polyethylene terephthalate composite dielectric film of Example 1 and Comparative Example 1. Figure 5 It can be seen that the composite dielectric film of Example 1 has better performance than the composite dielectric film prepared in Comparative Example 1.
[0099] In summary, through the analysis of performance tests and phase morphology / crystal structure characterization results, it can be seen that the preparation method can achieve coordinated regulation of phase morphology and crystal structure, inhibit carrier transport, and improve the insulation performance of the film. The obtained polypropylene / polyethylene terephthalate composite film has the characteristics of good insulation performance, high energy storage, and low loss, and can be widely used in the field of polymer capacitors as a dielectric material for polymer film capacitors. The preparation process of the present invention is simple and has the potential for large-scale industrial production.
[0100] Although the specific embodiments of the present invention are described above, it should be understood by those skilled in the art that these are only examples, and various changes or modifications can be made to the embodiments without departing from the principles and essence of the present invention. Therefore, these modifications or improvements made on the basis of not departing from the spirit of the present invention all belong to the scope of protection claimed by the present invention.
Claims
1. A method for preparing a polypropylene / polyethylene terephthalate composite dielectric film, characterized in that: The steps include: (1) preparing polypropylene / polyethylene terephthalate composite pellets: melt-blending polypropylene and polyethylene terephthalate, and pelletizing to obtain polypropylene / polyethylene terephthalate composite pellets; Wherein, the content of polyethylene terephthalate is 1 to 30 wt%; (2) preparing a primary composite film: extruding and casting the polypropylene / polyethylene terephthalate composite pellets, and then melt stretching the composite pellets at a melt stretching ratio of 5 to 60, and then cooling and winding the composite pellets to obtain a primary composite film; Wherein, the melt stretch ratio is the ratio of the cross-sectional area of the free cast film to the cross-sectional area of the extrusion cast film; (3) solid-state stretching the primary composite film under heating conditions, with a solid-state stretching ratio of 1 to 5, to obtain a polypropylene / polyethylene terephthalate composite dielectric film; The solid-state stretching ratio is the ratio of the linear speed of the stretching roller to the linear speed of the preheating roller.
2. The method for preparing a polypropylene / polyethylene terephthalate composite dielectric film according to claim 1, characterized in that: The temperature of the melt blending in step (1) is 140 to 280°C.
3. The method for preparing a polypropylene / polyethylene terephthalate composite dielectric film according to claim 1, characterized in that: The temperature of the extrusion casting in step (2) is 140-280°C.
4. The method for preparing a polypropylene / polyethylene terephthalate composite dielectric film according to claim 1, characterized in that: The temperature at which the primary composite film is heated in step (3) is 80 to 150°C.
5. The method for preparing the polypropylene / polyethylene terephthalate composite dielectric film according to claim 1, characterized in that: The polypropylene includes any one or more of homopolypropylene, copolymer polypropylene and polypropylene derivatives.
6. The method for preparing the polypropylene / polyethylene terephthalate composite dielectric film according to claim 1, characterized in that: The polypropylene has a melt index of 1 to 5 g / 10 min at 230° C.×2.16 kg load.
7. The method for preparing a polypropylene / polyethylene terephthalate composite dielectric film according to claim 1, characterized in that: The intrinsic viscosity of the polyethylene terephthalate measured according to GB / T14190 is 0.5 to 1 dL / g.
8. The polypropylene / polyethylene terephthalate composite dielectric film prepared by the preparation method according to any one of claims 1 to 7.
9. Application of polypropylene / polyethylene terephthalate composite dielectric film in polymer film capacitors.
Citation Information
Patent Citations
Polypropylene / polyvinylidene fluoride / polymethyl methacrylate composite dielectric film as well as preparation method and application thereof
CN118107193A
Cited By
Method for modifying polypropylene energy storage dielectric film through melt blending and application