Laser additive and impact synchronous composite repairing method for Ti2AlNb alloy aviation component

Through the laser additive and impact synchronous composite repair method, the problems of coarse tissue and uneven stress in the repair of Ti2AlNb alloy aerial components are solved, efficient micro defect elimination and phase change control are achieved, and fatigue performance and wear resistance are significantly improved.

CN118979135AInactive Publication Date: 2024-11-19BEIHANG UNIV

Patent Information

Application Number
CN202411074412.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The prior art is difficult to effectively repair the micro cracks caused by the coupling effects of high-period fatigue, thermal mechanical fatigue, creep and corrosion of Ti2AlNb alloy aviation components, and the thick tissue, tensile residual stress and pore defects after repair affect the mechanical properties, which cannot be achieved. Uniform distribution of overall structure and stress.

Method used

Using laser additive and impact synchronous composite repair method, the laser beam trajectory is designed by computer-aided, Ti2AlNb powder is stacked layer by layer and preheated by laser quenching. Combined with continuous and pulsed laser heating, a deposition layer is formed and laser impact strengthened to ensure deposition The layer temperature is between 500-800℃, achieving micro defect elimination, phase change control and stress reconstruction.

Benefits of technology

The fatigue performance and wear resistance of Ti2AlNb alloy aviation components are significantly improved, the stress distribution is improved, the overall performance of the repair components is enhanced, the operation is simplified and the cost is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979135A_ABST
    Figure CN118979135A_ABST
Patent Text Reader

Abstract

The invention discloses a laser additive material and impact synchronous composite repairing method for a Ti2AlNb alloy aviation component, and belongs to the technical field of additive material repairing. Comprising the following steps that the damaged position of a to-be-repaired component is ground, polished and cleaned; collecting and establishing a damage model contour, and designing and determining a two-dimensional scanning track of a laser beam under the protection of inert gas; a to-be-repaired component is preheated through laser quenching, Ti2AlNb powder is conveyed to a damaged position through a continuous laser coaxial powder feeding device to be stacked and repaired layer by layer, and pulse laser is applied during stacking or after stacking. Under the cooperative action of the continuous additive laser and the pulse impact laser, microdefect elimination, phase change control, structure refinement and stress reconstruction are achieved in a repairing area of the damaged part of the to-be-repaired component, the fatigue performance is remarkably improved, the method is easy and convenient to operate, the repairing efficiency is high, the repairing quality is high, and the reliability is remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of additive repair, and more particularly to a laser additive and impact synchronous composite repair method for a Ti2AlNb alloy aviation component. Background Art

[0002] Ti2AlNb alloy, which is formed by adding Nb element to TiAl alloy to form Ti2AlNb intermetallic compound, has high specific strength, high oxidation resistance and corrosion resistance, good high temperature service performance, and is widely used in aerospace, chemical industry, and energy fields. However, when it is used as a large load-bearing component or a component with complex geometric shape in the aviation field, it will be subject to coupling effects such as high cycle fatigue, thermomechanical fatigue, creep and corrosion. Once tiny cracks are generated on the surface of the component, it will seriously affect its normal operation and easily cause catastrophic accidents. In actual production, Ti2AlNb alloy is difficult to disassemble or replace for a long period of time as some large load-bearing components or complex structural components in aviation. High load will continuously promote crack propagation, and components that are not repaired in time may be further damaged, so new requirements are put forward for its efficient maintenance. Laser additive manufacturing technology is a method of manufacturing three-dimensional solid components by stacking materials layer by layer. It has the advantages of high reliability, low cost, and the ability to produce parts with complex geometric shapes, which can meet the production of large structural parts. The laser shock peening process uses a high-power density short-pulse laser beam to irradiate the surface of the metal target, causing plastic deformation of the metal surface. This not only promotes the closure of pores, but also obtains large-value and deep-thickness residual compressive stress, significantly improving the material's comprehensive properties such as fatigue resistance, wear resistance and corrosion resistance. It is widely used in the post-processing of laser additive repair components.

[0003] At present, most repair methods cannot provide timely and reliable repairs for Ti2AlNb alloy aviation structural parts that are difficult to disassemble or have complex geometric shapes. Although laser additive repair can achieve rapid remanufacturing, the coarse microstructure of the repaired Ti2AlNb alloy leads to poor strength, and the tensile residual stress generated during the repair process not only easily causes the component to deform, but is also not conducive to fatigue performance. The resulting pore defects will also deteriorate the mechanical properties and fatigue properties of the repaired component. At the same time, the phase transformation law of Ti2AlNb alloy is relatively complex, and changes in local areas during the solidification process will affect the overall mechanical properties. Laser shock strengthening can only produce a certain thickness of gradient structure and compressive residual stress near the surface of the Ti2AlNb alloy, and cannot achieve homogenization of the overall integrity of the repaired component.

[0004] The existing technology uses dual laser beams to repair complex metal parts, achieving their reliable service, but the existing process method cannot guarantee the impact at the optimal forging temperature, which makes it difficult to regulate stress and microstructure. The existing technology uses laser polishing and laser shock strengthening to process the workpiece after welding or additive repair, reducing the surface roughness and improving the surface quality of the workpiece. However, this method can only perform surface treatment on the workpiece, and has limited impact on the inside of the workpiece, and cannot achieve uniform distribution of the overall structure and stress of the repaired component. There is also existing technology that uses pulsed laser to disturb the molten pool, and improves the forming quality of the cladding layer by controlling the morphology and flow of the molten pool. However, this process method uses pulsed laser to impact the molten pool, which may cause molten droplets to splash and damage aviation structural parts. At the same time, the Ti2AlNb alloy has a complex structure, and this method is difficult to meet the directional regulation of the alloy structure.

[0005] In summary, a single repair method cannot guarantee the use requirements of large and complex Ti2AlNb alloy aviation components. Ensuring its rapid remanufacturing and good service reliability after repair is a technical problem that technicians in this field need to solve urgently. Therefore, in view of the above-mentioned repair environment limitations and repair technology deficiencies, a laser additive and laser shock strengthening composite repair process is used to develop a repair method for rapid remanufacturing and high-performance service of Ti2AlNb alloy. Summary of the invention

[0006] In view of this, the present invention provides a laser additive and impact synchronous composite repair method for Ti2AlNb alloy aviation components.

[0007] In order to achieve the above object, the present invention adopts the following technical solution:

[0008] A laser additive and impact synchronous composite repair method for a Ti2AlNb alloy aviation component comprises the following steps:

[0009] (1) Grinding, polishing and cleaning the damaged parts of the Ti2AlNb alloy aviation components to be repaired;

[0010] (2) Based on the size and shape of the damage location, the damage model contour is collected and established using computer-aided software, the two-dimensional scanning trajectory of the laser beam is designed and determined, and the component to be repaired is placed in a vacuum box and continuously introduced with inert gas;

[0011] (3) First, the component to be repaired is preheated by laser quenching, and then the Ti2AlNb powder is transported to the damaged position by a continuous laser coaxial powder feeding device to ensure the stable flow of the powder. During the powder feeding process, the Ti2AlNb powder is heated by continuous laser and the damaged position is melted to form a molten pool at the damaged position. When the Ti2AlNb powder enters the molten pool, it quickly melts and merges with the partially melted substrate at the damaged position. After the molten pool cools to form a deposition layer, the deposition layer is continuously heated by laser quenching, and the temperature of the deposition layer is monitored in real time to ensure that the temperature of the deposition layer is 500-800°C;

[0012] (4) stacking the deposited layers layer by layer until the original size and shape of the component to be repaired are obtained, and laser shock strengthening is performed on the surface of the entire deposited layer using a pulsed laser;

[0013] Or, after stacking several layers layer by layer, the deposited layer is laser-shock-hardened by using a pulsed laser, and then several layers of the deposited layer are stacked layer by layer, and the above steps are repeated until the original size and shape of the component to be repaired are obtained;

[0014] Alternatively, after each deposition layer is stacked, the deposition layer is laser-shock-hardened using a pulsed laser, and the above steps are repeated until the original size and shape of the component to be repaired are obtained;

[0015] During the laser shock peening process, the laser quenching is always maintained to continuously heat the deposited layer, and the temperature of the deposited layer is monitored in real time to ensure that the temperature of the deposited layer is 500-800℃.

[0016] Furthermore, in step (2), the inert gas is continuously introduced, and the washing time is 10-30 minutes.

[0017] The beneficial effect of adopting the above further technical solution is to prevent the deposited layer from being oxidized during the repair process.

[0018] Furthermore, in step (3), the continuous laser power is 2000-3500 W, and the scanning speed is 600-900 mm / min.

[0019] The beneficial effects of adopting the above further technical solution are: ensuring the quality of the additive deposition layer and the optimal forming temperature node.

[0020] Furthermore, in step (3), an Ar gas gun is used to spray Ar gas into the molten pool area.

[0021] The beneficial effect of adopting the above further technical solution is: preventing the molten pool from oxidation.

[0022] Furthermore, in step (4), the pulsed laser energy is a circular or square spot of 0.5-30 J, the spot overlap rate is 30-90%, and the angle between the pulsed laser and the deposited layer is 0-180°;

[0023] The deposited layers are stacked layer by layer until the original size and shape of the component to be repaired are obtained, and the surface of the entire deposited layer is laser-shock-hardened 1-5 times using a pulsed laser;

[0024] Or, after stacking several layers layer by layer, laser shock strengthening is performed on several deposited layers by using a pulsed laser for 1-5 times, and then several deposited layers are stacked layer by layer, and the above steps are repeated until the original size and shape of the component to be repaired are obtained;

[0025] Alternatively, after each deposition layer is stacked, the deposition layer is laser-shock-hardened 1-5 times using a pulsed laser, and the above steps are repeated until the original size and shape of the component to be repaired are obtained.

[0026] Furthermore, in step (4), the motion trajectory of the pulsed laser is consistent with the continuous laser used in step (3).

[0027] Beneficial effects of the present invention: (1) The present invention preheats the component to be repaired by laser quenching. If the size of the area to be repaired is large and heat dissipation in the repair area is considered, the substrate needs to be preheated before the first layer is clad to ensure good cladding of the first layer. Laser shock strengthening is introduced in the process of laser coaxial powder feeding to repair Ti2AlNb alloy, which overcomes the problem of difficult disassembly and assembly of Ti2AlNb alloy aviation components in actual production, saves time, and improves repair efficiency. At the same time, the present invention is also suitable for the remanufacturing of large and complex Ti2AlNb components.

[0028] (2) The present invention significantly improves the quality of repaired components. Under the synergistic effect of continuous additive laser and pulsed impact laser, micro-defect elimination, phase change control, microstructure refinement, and stress reconstruction are achieved in the repair area of ​​the damaged part of the Ti2AlNb alloy, significantly improving fatigue performance. The laser additive-impact composite repair method for Ti2AlNb alloy aviation components is simple to operate, has high repair efficiency, high repair quality, and significantly improved reliability. Therefore, the present invention is also suitable for the remanufacturing of large and complex Ti2AlNb components.

[0029] (3) After the optimal forming temperature is determined by laser quenching, the compressive residual stress of the repaired component is increased by 50-100 MPa compared with the repaired component without laser quenching, and the average area of ​​the O phase is reduced by 0.51 μm. 2 The average area of ​​β phase decreased by 4.16 μm 2 .

[0030] (4) The introduction of laser shock strengthening in the laser additive process not only effectively improved the microstructure of the Ti2AlNb alloy, but also refined the β / B2 phase and O phase of the deposited layer, with an average O phase area of ​​1.80 μm 2 , the average size of the β phase is 24.34 μm 2, the tissue distribution is more uniform, and the undetectable pore defects in the additive process are suppressed. The compressive residual stress of the repaired component is -418MPa, which improves the stress distribution, increases the hardness and strength, and also improves the wear resistance and fatigue performance of the repaired component. The laser quenching is always kept to heat the deposited layer continuously to prevent the temperature change during the laser shock process from affecting the tissue of the repaired area.

[0031] (5) The equipment used in the present invention is simple and does not require a laser shock peening constraint layer and an absorption layer, which saves costs and is easy to operate. At the same time, it avoids the plastic deformation of the material surface caused by laser shock peening, and the surface quality is better. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 It is a schematic diagram of a laser additive and impact synchronous composite repair method for a Ti2AlNb alloy aviation component of the present invention.

[0033] Figure 2 (a) is the microstructure of the repaired area of ​​the Ti2AlNb alloy aviation component of comparative example 2 without laser shock. (b) is the microstructure of the repaired area of ​​the Ti2AlNb alloy aviation component of embodiment 2 by simultaneous composite repair of laser additive and shock.

[0034] Figure 3 Example 2: Microstructure diagram of the repaired area of ​​the Ti2AlNb alloy aviation component repaired by simultaneous composite repair of laser additive and impact.

[0035] Among them: 1-Ar air gun; 2-pulse laser; 3-air inlet; 4-non-contact temperature measuring instrument; 5-Ti2AlNb powder; 6-vacuum box; 7-continuous laser; 8-laser quenching; 9-shock wave; 10-molten pool; 11-deposition layer; 12-component to be repaired; 13-exhaust port. DETAILED DESCRIPTION

[0036] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] Example 1

[0038] The laser additive and impact synchronous composite repair method for Ti2AlNb alloy aviation components includes the following steps:

[0039] (1) grinding, polishing and cleaning the damaged position of the Ti2AlNb alloy aviation component to be repaired 12 with acetone to remove surface oil, dust and other impurities;

[0040] (2) According to the size and shape of the damage location, the damage model contour is collected and established using computer-aided software, and the two-dimensional scanning trajectory of the laser beam is designed and determined. The component to be repaired 12 is placed in the vacuum box 6, and the air inlet 3 and the exhaust port 13 of the vacuum box 6 are opened and inert gas is continuously introduced. The washing time is 10 minutes;

[0041] (3) First, the component 12 to be repaired is preheated by laser quenching 8, and then the Ti2AlNb powder 5 is transported to the damaged position by the coaxial powder feeding device of the continuous laser 7 to ensure the stable flow of the powder. During the powder feeding process, the Ti2AlNb powder 5 is heated and the damaged position is melted by the continuous laser 7 to form a molten pool 10 at the damaged position. Ar gas is sprayed to the molten pool 10 area by an Ar air gun 1. The power of the continuous laser 7 is 2000 W, and the scanning speed is 700 mm / min. When the Ti2AlNb powder 5 enters the molten pool 10, it is rapidly melted and fused with the partially melted substrate at the damaged position. After the molten pool 10 is cooled to form a deposition layer 11, the deposition layer 11 is continuously heated by the laser quenching 8, and the temperature of the deposition layer 11 is monitored in real time by a non-contact temperature measuring instrument 4 to ensure that the temperature of the deposition layer 11 is 600-650°C;

[0042] (4) stacking the deposition layer 11 layer by layer until the original size and shape of the component 12 to be repaired is obtained, and the surface of the entire deposition layer 11 is laser-shock-hardened three times using a pulsed laser 2. During the laser-shock-hardening process, the deposition layer 11 is continuously heated by laser quenching 8, and the temperature of the deposition layer 11 is monitored in real time using a non-contact temperature measuring instrument 4 to control the optimal forming temperature node and ensure that the temperature of the deposition layer 11 is 600-650° C.;

[0043] The pulse laser 2 has a circular spot with an energy of 10 J, a spot overlap rate of 50%, an angle of 90° between the pulse laser 2 and the deposited layer 11, and a motion trajectory of the pulse laser 2 consistent with the continuous laser 7 used in step (3). The shock wave 9 enters from the surface of the material to the inside, improving the organization and performance of the material.

[0044] Example 2

[0045] The laser additive and impact synchronous composite repair method for Ti2AlNb alloy aviation components includes the following steps:

[0046] (1) grinding, polishing and cleaning the damaged position of the Ti2AlNb alloy aviation component to be repaired 12 with acetone;

[0047] (2) According to the size and shape of the damage location, the damage model contour is collected and established using computer-aided software, and the two-dimensional scanning trajectory of the laser beam is designed and determined. The component to be repaired 12 is placed in the vacuum box 6, and the air inlet 3 and the exhaust port 13 of the vacuum box 6 are opened and inert gas is continuously introduced. The washing time is 10 minutes;

[0048] (3) First, the component 12 to be repaired is preheated by laser quenching 8, and then the Ti2AlNb powder 5 is transported to the damaged position by the coaxial powder feeding device of the continuous laser 7 to ensure the stable flow of the powder. During the powder feeding process, the Ti2AlNb powder 5 is heated and the damaged position is melted by the continuous laser 7 to form a molten pool 10 at the damaged position. Ar gas is sprayed to the molten pool 10 area by an Ar air gun 1. The power of the continuous laser 7 is 3500 W, and the scanning speed is 800 mm / min. When the Ti2AlNb powder 5 enters the molten pool 10, it is quickly melted and fused with the partially melted substrate at the damaged position. After the molten pool 10 is cooled to form a deposition layer 11, the deposition layer 11 is continuously heated by the laser quenching 8, and the temperature of the deposition layer 11 is monitored in real time by a non-contact temperature measuring instrument 4 to ensure that the temperature of the deposition layer 11 is 750-800°C;

[0049] (4) After stacking several layers layer by layer, the pulse laser 2 is used to perform laser shock strengthening on the deposited layer 11 twice, and then several layers of the deposited layer 11 are continuously stacked layer by layer, and the above steps are repeated until the original size and shape of the component 12 to be repaired are obtained; during the laser shock strengthening process, the laser quenching 8 is always maintained to continuously heat the deposited layer 11, and the temperature of the deposited layer 11 is monitored in real time by a non-contact temperature measuring instrument 4 to control the optimal molding temperature node to ensure that the temperature of the deposited layer 11 is 750-800°C.

[0050] The energy of the pulse laser 2 is a square spot of 30 J, the spot overlap rate is 90%, the angle between the pulse laser 2 and the deposited layer 11 is 120°, and the movement trajectory of the pulse laser 2 is consistent with the continuous laser 7 used in step (3).

[0051] Subgrain boundaries appear in the microstructure of Ti2AlNb deposited layer 11, proving that the microstructure is refined ( Figure 2 No pore defects were found. Figure 3 ), the compressive residual stress of the repaired area is -350MPa, and at a stress level of 650MPa, the room temperature rotation bending fatigue life is about 740515 cycles, and the average area of ​​the O phase is 2.12μm 2 , the average size of the β phase is 30.57 μm 2 .

[0052] Example 3

[0053] The laser additive and impact synchronous composite repair method for Ti2AlNb alloy aviation components includes the following steps:

[0054] (1) grinding, polishing and cleaning the damaged position of the Ti2AlNb alloy aviation component to be repaired 12 with acetone;

[0055] (2) According to the size and shape of the damage location, the damage model contour is collected and established using computer-aided software, and the two-dimensional scanning trajectory of the laser beam is designed and determined. The component to be repaired 12 is placed in the vacuum box 6, and the air inlet 3 and the exhaust port 13 of the vacuum box 6 are opened and inert gas is continuously introduced. The washing time is 10 minutes;

[0056] (3) First, the component 12 to be repaired is preheated by laser quenching 8, and then the Ti2AlNb powder 5 is transported to the damaged position by the coaxial powder feeding device of the continuous laser 7 to ensure the stable flow of the powder. During the powder feeding process, the Ti2AlNb powder 5 is heated and the damaged position is melted by the continuous laser 7 to form a molten pool 10 at the damaged position. Ar gas is sprayed to the molten pool 10 area by an Ar air gun 1. The power of the continuous laser 7 is 3000 W, and the scanning speed is 750 mm / min. When the Ti2AlNb powder 5 enters the molten pool 10, it is quickly melted and fused with the partially melted substrate at the damaged position. After the molten pool 10 is cooled to form a deposition layer 11, the deposition layer 11 is continuously heated by the laser quenching 8, and the temperature of the deposition layer 11 is monitored in real time by a non-contact temperature measuring instrument 4 to ensure that the temperature of the deposition layer 11 is 700-800°C;

[0057] (4) After each layer of deposited layer 11 is stacked, the deposited layer 11 is laser-shock-hardened once using a pulsed laser 2, and the above steps are repeated until the original size and shape of the component 12 to be repaired are obtained. During the laser-shock-hardening process, the deposited layer 11 is continuously heated by the laser quenching 8, and the temperature of the deposited layer 11 is monitored in real time using a non-contact temperature measuring instrument 4 to control the optimal forming temperature node and ensure that the temperature of the deposited layer 11 is 700-800°C. The energy of the pulsed laser 2 is a square spot of 15 J, the spot overlap rate is 60%, the angle between the pulsed laser 2 and the deposited layer 11 is 90°, and the motion trajectory of the pulsed laser 2 is consistent with the continuous laser 7 used in step (3).

[0058] The compressive residual stress in the repaired area is -418MPa. At a stress level of 650MPa, the room temperature rotation bending fatigue life is about 1483734 cycles, and the average area of ​​the O phase is 1.80μm 2 , the average size of the β phase is 24.34 μm 2 .

[0059] Comparative Example 1

[0060] The laser additive and impact synchronous composite repair method for Ti2AlNb alloy aviation components includes the following steps:

[0061] (1) grinding, polishing and cleaning the damaged position of the Ti2AlNb alloy aviation component to be repaired 12 with acetone;

[0062] (2) According to the size and shape of the damage location, the damage model contour is collected and established using computer-aided software, and the two-dimensional scanning trajectory of the laser beam is designed and determined. The component to be repaired 12 is placed in the vacuum box 6, and the air inlet 3 and the exhaust port 13 of the vacuum box 6 are opened and inert gas is continuously introduced. The washing time is 10 minutes;

[0063] (3) The Ti2AlNb powder 5 is transported to the damaged position by a coaxial powder feeding device of a continuous laser 7 to ensure the stable flow of the powder. During the powder feeding process, the Ti2AlNb powder 5 is heated and the damaged position is melted by a continuous laser 7 to form a molten pool 10 at the damaged position. Ar gas is sprayed to the molten pool 10 area by an Ar air gun 1. The power of the continuous laser 7 is 2000 W and the scanning speed is 700 mm / min. When the Ti2AlNb powder 5 enters the molten pool 10, it is rapidly melted and fused with the partially melted substrate at the damaged position. The molten pool 10 is cooled to form a deposition layer 11.

[0064] (4) stacking the deposited layers 11 layer by layer until the original size and shape of the component 12 to be repaired is obtained, and laser shock strengthening is performed on the surface of the entire deposited layer 11 three times using a pulsed laser 2;

[0065] The pulse laser 2 has a circular spot with an energy of 10 J and a spot overlap rate of 50%. The angle between the pulse laser 2 and the deposited layer 11 is 90°. The motion trajectory of the pulse laser 2 is consistent with the continuous laser 7 used in step (3).

[0066] Compared with Example 1, Comparative Example 1 did not undergo laser quenching 8. Compared with Example 1, which did not undergo laser quenching 8, the compressive residual stress of the repaired area increased by 50-100 MPa, and the average area of ​​the O phase decreased by 0.51 μm. 2 The average area of ​​β phase decreased by 4.16 μm 2 .

[0067] Comparative Example 2

[0068] The laser additive and impact synchronous composite repair method for Ti2AlNb alloy aviation components includes the following steps:

[0069] (1) grinding, polishing and cleaning the damaged position of the Ti2AlNb alloy aviation component to be repaired 12 with acetone;

[0070] (2) According to the size and shape of the damage location, the damage model contour is collected and established using computer-aided software, and the two-dimensional scanning trajectory of the laser beam is designed and determined. The component to be repaired 12 is placed in the vacuum box 6, and the air inlet 3 and the exhaust port 13 of the vacuum box 6 are opened and inert gas is continuously introduced. The washing time is 10 minutes;

[0071] (3) Ti2AlNb powder 5 is delivered to the damaged position by a coaxial powder feeding device of a continuous laser 7 to ensure stable flow of the powder. During the powder feeding process, Ti2AlNb powder 5 is heated and the damaged position is melted by a continuous laser 7 to form a molten pool 10 at the damaged position. Ar gas is sprayed to the molten pool 10 area by an Ar air gun 1. The power of the continuous laser 7 is 3500 W and the scanning speed is 800 mm / min. When the Ti2AlNb powder 5 enters the molten pool 10, it is rapidly melted and fused with the partially melted substrate at the damaged position. After the molten pool 10 is cooled to form a deposition layer 11, the continuous laser 7 is used to stack the layers layer by layer until the original size and shape of the component 12 to be repaired is obtained.

[0072] Compared with Example 2, Comparative Example 2 was not subjected to laser shock 2. The tensile residual stress in the repaired area of ​​Comparative Example 2 reached 368 MPa. At a stress level of 650 MPa, the room temperature rotation bending fatigue life was about 284780 cycles, and the average area of ​​the O phase was 4.05 μm 2 , the average size of the β phase is 42.17 μm 2 .

[0073] Comparative Example 3

[0074] The laser additive and impact synchronous composite repair method for Ti2AlNb alloy aviation components includes the following steps:

[0075] (1) grinding, polishing and cleaning the damaged position of the Ti2AlNb alloy aviation component to be repaired 12 with acetone;

[0076] (2) According to the size and shape of the damage location, the damage model contour is collected and established using computer-aided software, and the two-dimensional scanning trajectory of the laser beam is designed and determined. The component to be repaired 12 is placed in the vacuum box 6, and the air inlet 3 and the exhaust port 13 of the vacuum box 6 are opened and inert gas is continuously introduced. The washing time is 10 minutes;

[0077] (3) The Ti2AlNb powder 5 is transported to the damaged position by a coaxial powder feeding device of a continuous laser 7 to ensure the stable flow of the powder. During the powder feeding process, the Ti2AlNb powder 5 is heated and the damaged position is melted by a continuous laser 7 to form a molten pool 10 at the damaged position. Ar gas is sprayed to the molten pool 10 area by an Ar air gun 1. The power of the continuous laser 7 is 3000 W and the scanning speed is 750 mm / min. When the Ti2AlNb powder 5 enters the molten pool 10, it is rapidly melted and fused with the partially melted substrate at the damaged position. The molten pool 10 is cooled to form a deposition layer 11.

[0078] (4) After each deposition layer 11 is stacked, the deposition layer 11 is laser-shock strengthened once using a pulsed laser 2, and the above steps are repeated until the original size and shape of the component 12 to be repaired are obtained. The energy of the pulsed laser 2 is a circular or square spot of 15 J, the spot overlap rate is 60%, the angle between the pulsed laser 2 and the deposition layer 11 is 90°, and the motion trajectory of the pulsed laser 2 is consistent with the continuous laser 7 used in step (3).

[0079] Compared with Example 3, Comparative Example 3 was not subjected to laser quenching 8. The compressive residual stress of the repaired area of ​​Comparative Example 3 was -386 MPa. At a stress level of 650 MPa, the room temperature rotation bending fatigue life was about 905740 cycles, and the average area of ​​the O phase was 2.14 μm 2 , the average size of the β phase is 34.57 μm 2 .

[0080] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A Ti 2 Laser additive and impact simultaneous composite repair method for AlNb alloy aviation components. It is characterized in that The following steps are involved: (1) Ti 2 Grinding, polishing and cleaning of damaged parts of AlNb alloy aviation components to be repaired; (2) Based on the size and shape of the damage location, the damage model contour is collected and established using computer-aided software, the two-dimensional scanning trajectory of the laser beam is designed and determined, and the component to be repaired is placed in a vacuum box and continuously introduced with inert gas; (3) First, the component to be repaired is preheated by laser quenching, and then the Ti 2 AlNb powder is transported to the damaged location to ensure stable powder flow. During the powder delivery process, Ti is heated by continuous laser. 2 AlNb powder and melt damage position, forming a molten pool at the damage position. 2 The AlNb powder enters the molten pool and melts rapidly, fusing with the partially melted substrate at the damaged position. After the molten pool cools down to form a deposition layer, the deposition layer is continuously heated by laser quenching, and the temperature of the deposition layer is monitored in real time to ensure that the temperature of the deposition layer is 500-800°C. (4) stacking the deposited layers layer by layer until the original size and shape of the component to be repaired are obtained, and laser shock strengthening is performed on the surface of the entire deposited layer using a pulsed laser; Or, after stacking several layers layer by layer, the deposited layer is laser-shock-hardened by using a pulsed laser, and then several layers of the deposited layer are stacked layer by layer, and the above steps are repeated until the original size and shape of the component to be repaired are obtained; Alternatively, after each deposition layer is stacked, the deposition layer is laser-shock-hardened using a pulsed laser, and the above steps are repeated until the original size and shape of the component to be repaired are obtained; During the laser shock peening process, the laser quenching is always maintained to continuously heat the deposited layer, and the temperature of the deposited layer is monitored in real time to ensure that the temperature of the deposited layer is 500-800°C.

2. According to claim 1, a Ti 2 Laser additive and impact simultaneous composite repair method for AlNb alloy aviation components. It is characterized in that In step (2), the inert gas is continuously introduced, and the washing time is 10-30 minutes.

3. A Ti according to claim 1 2 Laser additive and impact simultaneous composite repair method for AlNb alloy aviation components. It is characterized in that In step (3), the continuous laser power is 2000-3500W, and the scanning speed is 600-900mm / min.

4. A Ti according to claim 1 2 Laser additive and impact simultaneous composite repair method for AlNb alloy aviation components. It is characterized in that Step (3) also includes using an Ar air gun to spray Ar gas into the molten pool area.

5. A Ti according to claim 1 2 Laser additive and impact simultaneous composite repair method for AlNb alloy aviation components. It is characterized in that In step (4), the pulsed laser energy is a circular or square spot of 0.5-30 J, the spot overlap rate is 30-90%, and the angle between the pulsed laser and the deposited layer is 0-180°; The deposited layers are stacked layer by layer until the original size and shape of the component to be repaired are obtained, and the surface of the entire deposited layer is laser-shock-hardened 1-5 times using a pulsed laser; Or, after stacking several layers layer by layer, laser shock strengthening is performed on several deposited layers by using a pulsed laser for 1-5 times, and then several deposited layers are stacked layer by layer, and the above steps are repeated until the original size and shape of the component to be repaired are obtained; Alternatively, after each deposition layer is stacked, the deposition layer is laser-shock-hardened 1-5 times using a pulsed laser, and the above steps are repeated until the original size and shape of the component to be repaired are obtained.

6. A Ti according to claim 1 2 Laser additive and impact simultaneous composite repair method for AlNb alloy aviation components. It is characterized in that In step (4), the motion trajectory of the pulsed laser is consistent with the continuous laser used in step (3).

Citation Information

Patent Citations

  • Method for adjusting / reducing internal stress of laser additive manufacturing part

    CN107225244A

  • Method for refining laser additive manufacturing titanium alloy grain through ultrasonic impact and induction heating

    CN107649682A

  • Vane wheel piece dropping distressing laser impact forging remanufacturing method and device

    CN107931844A

  • Damaged blade repairing method and device for blisk based on double laser beams

    CN112195468A

  • Multi-heat-source composite additive manufacturing method

    CN117697148A

Cited By

  • High-temperature alloy blade additive manufacturing repair process for improving additive repair interface

    CN119772180A

  • In-situ intelligent repair system and method for first wall component of nuclear fusion device

    CN119772212A

  • In-situ intelligent repair system and method for the first wall components of a nuclear fusion device

    CN119772212B

  • Ta-10W alloy composite welding method with optical fiber laser focus rotating along with welding laser shock

    CN120347527A

  • High-strength aluminum alloy repairing method combining laser shock with laser powder feeding and application

    CN120533117A