Method for comprehensively utilizing dust mud containing zinc and iron

Through suspension roasting technology, the zinc-containing iron-containing dust sludge was oxidized and roasted, which solved the problem of small scale and poor economicality in zinc extraction treatment in the ignition process, achieved efficient recycling and resource utilization of zinc elements, and reduced energy loss and production Cost increases the degree of automation of equipment.

CN118979149APending Publication Date: 2024-11-19SHANGHAI MILESTONE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411068839.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing steel production medium-temperature process has small scale, poor economics, high raw material requirements and easy knotting in the high-temperature sections in the kiln during the zinc extraction process, which leads to waste of zinc resources and damage to the furnace body, limiting the promotion of rotary kiln technology. and development.

Method used

The suspension roasting technology is used to oxidize and roast zinc-containing iron dust sludge. By reacting with air, the zinc content is reduced and the zinc element is converted into recyclable zinc oxide or sub-zinc oxide, reducing the deposition of zinc in the furnace feed and furnace liner, combined with The cyclone separator collects smoke and dust to achieve effective recycling of zinc elements and resource utilization.

Benefits of technology

It improves the removal rate and resource utilization rate of zinc elements, reduces energy loss, reduces production costs, and improves the degree of automation of equipment and the feasibility of industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979149A_ABST
    Figure CN118979149A_ABST
Patent Text Reader

Abstract

The invention relates to a method for comprehensively utilizing dust mud containing zinc and iron, and belongs to the technical field of dressing and smelting. The method comprises the steps that iron-containing materials are preheated after being dried and crushed, the preheated materials enter a suspension roasting device, oxidizing roasting is conducted through the suspension roasting technology, zinc-containing smoke enters a cyclone separator above the suspension roasting device to be separated again, and large-particle materials in the smoke return to the suspension roasting device; and light smoke dust with high zinc content enters smoke dust collecting equipment such as a cloth bag at the rear end. According to the invention, the reaction atmosphere can be accurately controlled, the cost is saved, the reaction efficiency is improved, and the roasted ore cooling link is reduced, so that the energy loss is reduced, and the economic benefit is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallurgy, and in particular relates to a method for comprehensive utilization of zinc- and iron-containing dust and mud. Background Art

[0002] my country's national crude steel output exceeded 1 billion tons in 2021. There are many dust generating points in the existing steel production process, including blast furnace bag ash, blast furnace gravity ash, converter dust removal ash, sintering dust removal ash, etc.

[0003] At present, most of the dust and mud of steel enterprises are returned to sintering for recycling within the enterprise. The treatment process of zinc-containing dust is divided into two categories: wet method and pyrotechnic method. At present, the zinc extraction treatment method commonly used by steel mills is still the pyrotechnic process. Whether it is a rotary kiln or a rotary hearth furnace, the basic principle of the pyrotechnic process is to use the low boiling point of zinc (907℃) and the high temperature volatility of zinc to volatilize the zinc in the dust through reduction and then enrich and recover it. However, in terms of technical operability and the overall nature of the industry, there are also problems such as small scale, poor economy, high raw material requirements, and shallow technical research. In particular, the phenomenon of easy ring formation in the high temperature section of the kiln during the production process seems to have become an industry "chronic disease", which seriously restricts the promotion and development of rotary kiln process technology, and urgently needs to be systematically analyzed, studied and improved from a technical perspective. Due to the iron-making and steel-making processes and other reasons, the zinc element will circulate in the entire process in the form of zinc alone, zinc oxide, etc. This will not only cause a waste of resources, but also lead to a large amount of zinc deposition in the charge, furnace lining and attachments, bringing many hazards to blast furnace production, such as causing the charge to descend smoothly, or deposit in the refractory bricks, causing damage to the furnace body, etc. Summary of the invention

[0004] In order to solve the above technical problems, the present invention proposes a process method for comprehensive utilization of zinc-containing and iron-containing dust and mud by using suspended roasting instead of rotary kiln, solves the problem of harmful elements in the smelting process, and provides a comprehensive solution for smelting zinc-containing and iron-containing dust and mud.

[0005] A method for comprehensive utilization of zinc-containing and iron-containing dust and mud, the specific steps are as follows:

[0006] Step 1: Drying and crushing: Dry and crush the iron-containing material until the moisture content of the material is less than 10% and the particle size is -1mm after drying and crushing;

[0007] Step 2: batching and preheating stage: after the dried and crushed materials enter the silo, they are batched with the bituminous coal in the auxiliary material silo through a feeder and a belt scale, and then enter the mixing device; the mixed materials are preheated and enter the suspension roasting device, the preheating time is 10s-20s, and the preheating temperature is 200℃-300℃;

[0008] Step 3: Suspension roasting and zinc extraction: the material is preheated and then enters the suspension roasting device, where it is subjected to oxidation roasting using the suspension roasting technology. Air is introduced into the roasting chamber, and heavy materials are discharged from the discharge port to obtain roasted ore. The zinc content of the roasted ore is reduced and the iron is reduced, so the ore can be re-entered into the electric furnace for smelting later.

[0009] Step 4: Collection of zinc-containing dust: The zinc-containing dust enters the cyclone separator above the suspension roasting device for separation again. The large particles in the dust return to the suspension roasting device, and the lighter dust with higher zinc content enters the rear-end bag and other dust collection equipment. The collected dust has a Zn content of 45-55%. The collected products can be sold as zinc oxide or zinc suboxide according to the indicators.

[0010] Furthermore, the iron-containing material in step 1 has a TFe content of about 50% and a Zn content of 5-10%.

[0011] Furthermore, the dried and crushed material in step 2 is mixed with the bituminous coal in the auxiliary material silo in a ratio of 1:10-15.

[0012] Furthermore, the oxidation roasting temperature in step 3 is 1000-1050° C., and the roasting time is 55-60 min.

[0013] Furthermore, the total volume of air in step 3 is 20 Nm 3 / h.

[0014] Furthermore, the roasted ore in step 3 has a TFe grade of 55-65%, a Zn content of 45-55%, and a zinc removal rate of 65-75%.

[0015] The chemical reaction equation involved is:

[0016] ZnO+C=Zn+CO

[0017] ZnO+CO=Zn+CO 2

[0018] ZnO·Fe 2 O 3 +4C=Zn+2Fe+4CO

[0019] ZnO·Fe 2 O 3 +2CO=Zn+2CO 2 +2FeO

[0020] 2Zn+O 2 =2ZnO

[0021] Compared with the existing prior art, the characteristics and advantages of the present invention are:

[0022] 1. The reaction atmosphere can be precisely controlled, which saves costs and improves reaction efficiency.

[0023] 2. Small footprint, large processing capacity, silo, suspension roasting device, cyclone separator and other equipment can be arranged vertically.

[0024] 3. The equipment operates stably, has a high degree of automation, and is easy to realize industrial production.

[0025] 4. The iron-containing materials after suspension roasting can directly enter the subsequent smelting device, which reduces the cooling link of the roasted ore, thereby reducing energy loss and improving economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The present invention is a schematic flow chart of a method for comprehensive utilization of zinc- and iron-containing dust and mud. DETAILED DESCRIPTION

[0027] The present invention is further described in detail below in conjunction with the embodiments and drawings.

[0028] Example 1

[0029] A method for comprehensive utilization of zinc-containing iron-containing dust and mud, such as Figure 1 The specific operation method is as follows:

[0030] In this case, the zinc-containing iron dust has a TFe grade of 55.84%, a Zn content of 6.02%, and a SiO 2 The content is 1.59%, the CaO content is 6.21, the MgO content is 1.93%, and the Al 2 O 3 The content is 0.22%, the water content is 8.05%, and the particle size is less than -1mm.

[0031] Step 1: Mixing operation: The material has a moisture content of less than 10% and a particle size of less than 1mm. It does not need to be dried or crushed. It can be directly mixed with bituminous coal in a ratio of 1:10 from the raw material bin through a belt scale and then enter the mixing bin.

[0032] Step 2: Preheating operation: After mixing, the materials are directly weighed into the preheating system through a belt scale for preheating. The feed rate is 100kg / h, the preheating temperature is 200℃-300℃, and the preheating time is 10s-20s to dehydrate and dry the materials.

[0033] Step 3: Suspension roasting - classification operation: After preheating, the material enters the suspension roasting system for suspension roasting. Air is introduced into the reactor with a total gas volume of 20Nm 3 / h, reaction temperature 1000-1050℃, reaction time 55-60min. Zinc-containing smoke enters the cyclone separator above the suspension roasting device for further separation, the heavier smoke particles return to the suspension roasting device, and the lighter smoke with higher zinc content enters the next collection stage process. After roasting, the heavy material is discharged from the discharge port to obtain roasted ore. The roasted ore has a TFe grade of 62.71%, a Zn content of 2.30%, and a zinc removal rate of 71.3%.

[0034] Step 4: Collection of zinc-containing dust: The lighter dust with higher zinc content is separated by a cyclone separator and enters the rear-end bag and other dust collection equipment. The collected dust has a Zn content of 53.66% and can be sold as a zinc-containing product.

[0035] Example 2

[0036] A method for comprehensive utilization of zinc-containing and iron-containing dust and mud, the specific operation method of which is as follows:

[0037] In this case, the zinc-containing iron dust has a TFe grade of 55.28%, a Zn content of 6.09%, and a SiO 2 The content is 2.219%, CaO content is 6.00%, MgO content is 1.79%, Al 2 O3 content is 0.21%, water content is 8.71%, particle size is less than -1mm,

[0038] Step 1: Mixing operation: The material has a moisture content of less than 10% and a particle size of less than 1mm. It does not need to be dried or crushed. It can be directly mixed with bituminous coal in a ratio of 1:10 from the raw material bin through a belt scale and then enter the mixing bin.

[0039] Step 2: Preheating operation: After mixing, the materials are directly weighed into the preheating system through a belt scale for preheating. The feed rate is 100kg / h, the preheating temperature is 200℃-300℃, and the preheating time is 10s-20s to dehydrate and dry the materials.

[0040] Step 3: Suspension roasting - classification operation: After preheating, the material enters the suspension roasting system for suspension roasting. Air is introduced into the reactor with a total gas volume of 20Nm 3 / h, reaction temperature 1000-1050℃, reaction time 55-60min. Zinc-containing smoke enters the cyclone separator above the suspension roasting device for further separation, the heavier smoke particles return to the suspension roasting device, and the lighter smoke with higher zinc content enters the next collection stage process. After roasting, the heavy material is discharged from the discharge port to obtain roasted ore. The roasted ore has a TFe grade of 61.00%, a Zn content of 2.31%, and a zinc removal rate of 71.9%.

[0041] Step 4: Collection of zinc-containing dust: The lighter dust with higher zinc content is separated by a cyclone separator and enters the rear-end bag and other dust collection equipment. The collected dust has a Zn content of 53.40% and can be sold as a zinc-containing product.

[0042] Example 3

[0043] A method for comprehensive utilization of zinc-containing and iron-containing dust and mud, the specific operation method of which is as follows:

[0044] In this case, the zinc-containing iron dust has a TFe grade of 55.34%, a Zn content of 5.90%, and a SiO 2 The content is 2.52%, CaO content is 8.33, MgO content is 1.62%, Al2O 3 The content is 0.31%, the water content is 20.31%, and the particle size is less than -1mm.

[0045] Step 1: Ore drying - crushing - mixing: The moisture content of the material is greater than 10%, so it is dried to reduce the moisture content to less than 10%. Since the material will be partially agglomerated after drying, the crushing equipment is used to crush the material to a particle size of less than 1mm. After crushing, the material is mixed with bituminous coal in a ratio of 1:10 from the raw material bin through a belt scale and then enters the mixing bin.

[0046] Step 2: Preheating operation: After mixing, the materials are directly weighed into the preheating system through a belt scale for preheating. The feed rate is 100kg / h, the preheating temperature is 200℃-300℃, and the preheating time is 10s-20s to dehydrate and dry the materials.

[0047] Step 3: Suspension roasting - classification operation: After preheating, the material enters the suspension roasting system for suspension roasting. Air is introduced into the reactor with a total gas volume of 20Nm 3 / h, reaction temperature 1000-1050℃, reaction time 55-60min. Zinc-containing smoke enters the cyclone separator above the suspension roasting device for further separation, the heavier smoke particles return to the suspension roasting device, and the lighter smoke with higher zinc content enters the next collection stage process. After roasting, the heavy material is discharged from the discharge port to obtain roasted ore. The roasted ore TFe grade is 60.11%, Zn content is 2.11%, and the zinc removal rate reaches 70.6%.

[0048] Step 4: Collection of zinc-containing dust: The lighter dust with higher zinc content is separated by a cyclone separator and enters the rear-end bag and other dust collection equipment. The collected dust has a Zn content of 52.71% and can be sold as a zinc-containing product.

[0049] Example 4

[0050] A method for comprehensive utilization of zinc-containing and iron-containing dust and mud, the specific operation method of which is as follows:

[0051] In this case, the zinc-containing iron dust has a TFe grade of 55.04%, a Zn content of 6.71%, and a SiO 2 The content is 3.50%, the CaO content is 8.13, the MgO content is 1.66%, and the Al 2 O 3 The content is 0.21%, the water content is 24.31%, and the particle size is less than -1mm.

[0052] Step 1: Ore drying - crushing - mixing: The moisture content of the material is greater than 10%, so it is dried to reduce the moisture content to less than 10%. Since the material will be partially agglomerated after drying, the crushing equipment is used to crush the material to a particle size of less than 1mm. After crushing, the material is mixed with bituminous coal in a ratio of 1:10 from the raw material bin through a belt scale and then enters the mixing bin.

[0053] Step 2: Preheating operation: After mixing, the materials are directly weighed into the preheating system through a belt scale for preheating. The feed rate is 100kg / h, the preheating temperature is 200℃-300℃, and the preheating time is 10s-20s to dehydrate and dry the materials.

[0054] Step 3: Suspension roasting - classification operation: After preheating, the material enters the suspension roasting system for suspension roasting. Air is introduced into the reactor with a total gas volume of 20Nm 3 / h, reaction temperature 1000-1050℃, reaction time 55-60min. Zinc-containing smoke enters the cyclone separator above the suspension roasting device for further separation, the heavier smoke particles return to the suspension roasting device, and the lighter smoke with higher zinc content enters the next collection stage process. After roasting, the heavy material is discharged from the discharge port to obtain roasted ore. The roasted ore has a TFe grade of 61.99%, a Zn content of 2.04%, and a zinc removal rate of 70.5%.

[0055] Step 4: Collection of zinc-containing dust: The lighter dust with higher zinc content is separated by a cyclone separator and enters the rear-end bag and other dust collection equipment. The collected dust has a Zn content of 54.71% and can be sold as a zinc-containing product.

[0056] Example 5

[0057] A method for comprehensive utilization of zinc-containing and iron-containing dust and mud, the specific operation method of which is as follows:

[0058] In this case, the zinc-containing iron dust has a TFe grade of 50.91%, a Zn content of 6.82%, and a SiO 2 The content is 4.59%, the CaO content is 7.11, the MgO content is 0.69%, and the Al 2 O 3 The content is 1.55%, the water content is 9.82%, and the particle size is about 10mm.

[0059] Step 1: Crushing-mixing operation: The moisture content of the material is less than 10%, so drying is not required. The material size is greater than 1mm, so the crushing equipment is used to crush the material to a particle size less than 1mm. After crushing, the material is mixed with bituminous coal in a ratio of 1:10 from the raw material bin through a belt scale and then enters the mixing bin.

[0060] Step 2: Preheating operation: After mixing, the materials are directly weighed into the preheating system through a belt scale for preheating. The feed rate is 100kg / h, the preheating temperature is 200℃-300℃, and the preheating time is 10s-20s to dehydrate and dry the materials.

[0061] Step 3: Suspension roasting - classification operation: After preheating, the material enters the suspension roasting system for suspension roasting. Air is introduced into the reactor with a total gas volume of 20Nm 3 / h, reaction temperature 1000-1050℃, reaction time 55-60min. Zinc-containing smoke enters the cyclone separator above the suspension roasting device for further separation, the heavier smoke particles return to the suspension roasting device, and the lighter smoke with higher zinc content enters the next collection stage process. After roasting, the heavy material is discharged from the discharge port to obtain roasted ore. The roasted ore has a TFe grade of 59.61%, a Zn content of 2.13%, and a zinc removal rate of 73.3%.

[0062] Step 4: Collection of zinc-containing dust: The lighter dust with higher zinc content is separated by a cyclone separator and enters the rear-end bag and other dust collection equipment. The collected dust has a Zn content of 54.61% and can be sold as a zinc-containing product.

[0063] Example 6

[0064] A method for comprehensive utilization of zinc-containing and iron-containing dust and mud, the specific operation method of which is as follows:

[0065] In this case, the zinc-containing iron dust has a TFe grade of 50.81%, a Zn content of 6.79%, and a SiO 2 The content is 4.03%, CaO content is 6.91, MgO content is 0.59%, Al 2 O 3 The content is 2.30%, the water content is 9.80%, and the particle size is about 10mm.

[0066] Step 1: Crushing-mixing operation: The moisture content of the material is less than 10%, so drying is not required. The material size is greater than 1mm, so the crushing equipment is used to crush the material to a particle size less than 1mm. After crushing, the material is mixed with bituminous coal in a ratio of 1:10 from the raw material bin through a belt scale and then enters the mixing bin.

[0067] Step 2: Preheating operation: After mixing, the materials are directly weighed into the preheating system through a belt scale for preheating. The feed rate is 100kg / h, the preheating temperature is 200℃-300℃, and the preheating time is 10s-20s to dehydrate and dry the materials.

[0068] Step 3: Suspension roasting - classification operation: After preheating, the material enters the suspension roasting system for suspension roasting. Air is introduced into the reactor with a total gas volume of 20Nm 3 / h, reaction temperature 1000-1050℃, reaction time 55-60min. Zinc-containing smoke enters the cyclone separator above the suspension roasting device for further separation, the heavier smoke particles return to the suspension roasting device, and the lighter smoke with higher zinc content enters the next collection stage process. After roasting, the heavy material is discharged from the discharge port to obtain roasted ore. The roasted ore has a TFe grade of 60.03%, a Zn content of 2.03%, and a zinc removal rate of 73.4%.

[0069] Step 4: Collection of zinc-containing dust: The lighter dust with higher zinc content is separated by a cyclone separator and enters the rear-end bag and other dust collection equipment. The collected dust has a Zn content of 53.95% and can be sold as a zinc-containing product.

Claims

1. A method for comprehensive utilization of zinc-containing and iron-containing dust and mud, characterized in that: The specific steps are as follows: Step 1: Drying and crushing: Dry and crush the iron-containing material until the moisture content of the material is less than 10% and the particle size is -1mm after drying and crushing; Step 2: batching and preheating stage: after the dried and crushed materials enter the silo, they are batched with the bituminous coal in the auxiliary material silo through a feeder and a belt scale, and then enter the mixing device; the mixed materials are preheated and enter the suspension roasting device, the preheating time is 10s-20s, and the preheating temperature is 200℃-300℃; Step 3: Suspension roasting and zinc extraction: the material is preheated and then enters the suspension roasting device, where it is subjected to oxidation roasting using the suspension roasting technology. Air is introduced into the roasting chamber, and heavy materials are discharged from the discharge port to obtain roasted ore. The zinc content of the roasted ore is reduced and the iron is reduced, so the ore can be re-entered into the electric furnace for smelting later. Step 4: Collection of zinc-containing dust: The zinc-containing dust enters the cyclone separator above the suspension roasting device for separation again. The large particles in the dust return to the suspension roasting device, and the lighter dust with higher zinc content enters the rear-end bag and other dust collection equipment. The collected dust has a Zn content of 45-55%. The collected products can be sold as zinc oxide or zinc suboxide according to the indicators.

2. The method for comprehensive utilization of zinc-containing and iron-containing dust and mud according to claim 1, characterized in that: The iron-containing material in step 1 has a TFe content of about 50% and a Zn content of 5-10%.

3. The method for comprehensive utilization of zinc-containing and iron-containing dust and mud according to claim 1, characterized in that: The dried and crushed material in step 2 is mixed with the bituminous coal in the auxiliary material silo in a ratio of 1:10-15.

4. The method for comprehensive utilization of zinc-containing and iron-containing dust and mud according to claim 1, characterized in that: The oxidation roasting temperature in step 3 is 1000-1050° C., and the roasting time is 55-60 min.

5. The method for comprehensive utilization of zinc-containing and iron-containing dust and mud according to claim 1, characterized in that: The total volume of air in step 3 is 20 Nm 3 / h.

6. The method for comprehensive utilization of zinc-containing and iron-containing dust and mud according to claim 1, characterized in that: The roasted ore in step 3 has a TFe grade of 55-65%, a Zn content of 45-55%, and a zinc removal rate of 65-75%.