Electrolyte and application thereof in organic liquid hydrogen storage

By using PBS buffer and phase transfer additives in electrolyte in electrochemical hydrogenation technology, the problems of low solubility and difficulty in separation of organic substrates are solved, and the efficiency of hydrogenation reaction and industrial adaptability are improved.

CN118979261AActive Publication Date: 2024-11-19SHAANXI HYDROGEN ENERGY TECH CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411058762.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-19
Estimated Expiration
2044-08-02

AI Technical Summary

Technical Problem

In the existing electrochemical hydrogenation technology, the organic substrate in the cathode electrolyte is difficult to dissolve, resulting in low hydrogenation efficiency. The existing electrolyte is optimized under acidic or alkaline conditions, making it difficult to separate the aid-solution components from the organic substrate. Influencing the promotion of industrialization.

Method used

An electrolyte consisting of PBS buffer with pH 6.8 to 7.8 and phase transfer additives (such as cetyltrimethylammonium bromide and sodium dodecyl sulfate) as a dielectric to promote unsaturated aromatic compounds and water Phase dissolution increases the contact area between the organic liquid and the catalyst and improves the efficiency of hydrogenation reaction.

Benefits of technology

It realizes efficient dissolution and hydrogenation conversion of organic liquid in a neutral environment, simplifies the reaction steps, reduces energy consumption, and is easy to separate the phase transfer additives, solving the problem of difficulty in separation after reaction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979261A_ABST
    Figure CN118979261A_ABST
Patent Text Reader

Abstract

The invention provides an electrolyte and application thereof in organic liquid hydrogen storage. A catholyte in the electrolyte is composed of a PBS buffer solution with the pH of 6.8-7.8 and a phase transfer additive; the phase transfer auxiliary agent comprises hexadecyl trimethyl ammonium bromide, lauryl sodium sulfate or tetrabutylammonium bromide. The electrolyte is simple in component and only contains two phases, organic solvents with high toxicity and high corrosivity are avoided, and damage to reaction equipment is reduced. And when the electrolyte is applied to organic liquid hydrogenation reaction, the solubility of a substrate can be increased, the contact area of the substrate and a catalyst is increased, and the hydrogenation conversion rate is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of electrochemical technology, and in particular to an electrolyte and its application in organic liquid hydrogen storage. Background Art

[0002] Organic liquid hydrogen storage technology uses organic matter containing unsaturated bonds as hydrogen storage carriers. Under the action of catalysts, unsaturated aromatic compounds react reversibly with hydrogen to achieve hydrogen storage and transportation. At present, conventional unsaturated aromatic compound hydrogenation adopts thermochemical method, but its energy consumption is high. Since electrochemical hydrogenation has lower reaction energy barrier and milder reaction conditions, it is more concerned.

[0003] In electrochemical catalytic hydrogenation, unsaturated aromatic compounds need to be added to the cathode electrolyte as organic substrates. However, organic substrates are difficult to dissolve in the aqueous phase, resulting in extremely low hydrogenation efficiency. On the one hand, methanol, ethanol or other more complex solubilizing components are added in relevant reports to promote the dissolution of organic substrates; on the other hand, existing electrochemical hydrogenation electrolytes are usually optimized under acidic or alkaline conditions with performance as the guide, and are still in the laboratory stage. This makes it difficult to separate the solubilizing components from the organic substrate and the post-processing is complicated, which is not conducive to the advancement of industrialization. Summary of the invention

[0004] To solve the above problems, the present application provides an electrolyte and its application in organic liquid hydrogen storage. The electrolyte has a simple composition, low price, and is easy to separate after the reaction. When the electrolyte is used as a dielectric in organic liquid hydrogen storage, it can promote the dissolution of the organic liquid in the aqueous solution, increase the contact area between the organic phase and the catalyst, and thereby improve the hydrogenation reaction efficiency of the organic phase in a neutral environment.

[0005] In a first aspect, the present application provides an electrolyte, wherein the cathode electrolyte in the electrolyte is composed of a PBS buffer solution with a pH of 6.8 to 7.8 and a phase transfer aid;

[0006] The phase transfer aid includes hexadecyltrimethylammonium bromide, sodium dodecyl sulfate or tetrabutylammonium bromide.

[0007] Optionally, the PBS buffer is deionized water, Na2HPO4, KH2PO4, NaCl and KCl.

[0008] Optionally, the anode electrolyte in the electrolyte includes sulfuric acid solution and / or deionized water.

[0009] Optionally, the concentration of the sulfuric acid solution is 0.1 mol / L to 0.5 mol / L.

[0010] In a second aspect, the present application provides an application of an electrolyte in organic liquid hydrogen storage, wherein the electrolyte is used as a dielectric in an organic liquid hydrogenation reaction, and the unsaturated aromatic compound reacts with the hydrogen protons to obtain a hydrogen-rich organic liquid.

[0011] Optionally, the unsaturated aromatic compound includes one or more of toluene, dibenzyltoluene, N-ethylcarbazole, benzyltoluene, 3-methylindole, 7-methylindole, cyclopentylpyrazine, carbazole, N-methylindole, N-ethylindole, pyrazine, 2,3-dimethylpyrazine, 2,5-dimethylpyrazine, 2-methylpyrazine, pyridazine, pyridine and 3-methylpyridine.

[0012] Optionally, the molar ratio of the phase transfer aid to the unsaturated aromatic compound is 0.5:1 to 5:1.

[0013] Optionally, the molar amount of the unsaturated aromatic compound is 0.1 mmol to 5 mmol.

[0014] Optionally, the hydrogenation reactor for the hydrogenation reaction of unsaturated aromatic compounds comprises: an H-type replaceable membrane electrolyzer (1) or a PEM (2).

[0015] Wherein, the H-type replaceable membrane electrolytic cell (1) comprises a cathode chamber (11), an anode chamber (12) and a proton exchange membrane (13);

[0016] The PEM (2) comprises an anode plate (21), an anode gas diffusion layer (22), a hydrogenation catalyst layer (23), a cathode plate (25), a cathode gas diffusion layer (26), a cathode catalyst layer (27) and a proton exchange membrane (13).

[0017] Optionally, the electrolyte is used as a dielectric in a hydrogenation reaction of an unsaturated aromatic compound, comprising:

[0018] When the hydrogenation reactor is an H-type replaceable membrane electrolytic cell (1), taking an appropriate amount of sulfuric acid solution to form an anolyte, taking an appropriate amount of the PBS buffer and the phase transfer aid, and mixing them to obtain the catholyte;

[0019] Mixing a hydrogenation catalyst and an additive to prepare a catalytic slurry, impregnating a foamed metal with the catalytic slurry, inserting the obtained foamed metal electrode and a reference electrode into the cathode electrolyte, inserting a platinum electrode into the anode electrolyte, adding the unsaturated aromatic compound into the cathode electrolyte to form an electrolysis system, and performing an activation treatment on the electrolysis system;

[0020] After activation is completed, a constant current electrolysis reaction is performed to hydrogenate the unsaturated aromatic compound to obtain a hydrogen-rich organic liquid.

[0021] Optionally, the electrolyte is used as a dielectric in a hydrogenation reaction of an unsaturated aromatic compound, comprising:

[0022] When the hydrogenation reactor is a PEM (2), deionized water is taken to form an anolyte, and an appropriate amount of the PBS buffer and the phase transfer aid are taken and mixed to obtain the catholyte;

[0023] Mixing a hydrogenation catalyst and an additive to prepare a hydrogenation catalyst slurry, and using the catalytic slurry to prepare a hydrogenation catalyst layer (23);

[0024] Inputting the anolyte into the anode of the PEM (2), inputting the catholyte into the cathode of the PEM (2), adding the unsaturated aromatic compound to form an electrolysis system, and performing an activation treatment on the electrolysis system;

[0025] After activation is completed, a constant current electrolysis reaction is performed to hydrogenate the unsaturated aromatic compound to obtain a hydrogen-rich organic liquid.

[0026] Optionally, the activating treatment of the electrolytic system comprises: activating the electrolytic system by sequentially using a cyclic voltammetry scanning method and a linear voltammetry scanning test method;

[0027] The activated electrolytic system is at -30 mA / cm -2 ~-70mA / cm -2 A constant current electrolysis reaction is carried out at a current density of to obtain the hydrogen-rich organic liquid.

[0028] In summary, the present application includes at least one of the following beneficial technical effects:

[0029] 1. The present application provides an electrolyte, in which the cathode electrolyte includes a PBS buffer and a phase transfer aid. A neutral electrolysis environment is provided by adding a PBS buffer. The PBS buffer is inexpensive, widely available, environmentally friendly, and does not require post-treatment. However, there are few proton donors under neutral conditions. Therefore, a phase transfer aid is added to improve the problem of few proton donors. The molecules of the phase transfer aid carry different hydrophilic groups and hydrophobic groups. The amphiphilic structure of the molecule enables it to have a significant solubilizing effect, and can effectively dissolve organic liquid components that are insoluble or poorly soluble in water in an aqueous phase solution, thereby increasing the solubility of the substrate, allowing the product generated during the reaction to quickly enter the aqueous phase containing the buffer solution to increase the amount of proton donors and solve the problem of poor solubility of organic liquids in neutral electrolyte media.

[0030] 2. The present application provides an application of an electrolyte in organic liquid hydrogen storage. During the hydrogenation reaction, the phase transfer aid in the cathode electrolyte promotes the connection between the unsaturated aromatic compound and the aqueous electrolyte, further improving the solubility of the organic liquid in the electrolyte, increasing the contact area between the organic liquid and the catalyst, and realizing homogeneous and efficient dissolution of the organic liquid in the electrolyte. The raw materials used in this method are non-toxic and harmless, environmentally friendly, inexpensive, simple in reaction steps, and short in reaction time, which greatly improves the hydrogenation conversion rate. After the reaction, the phase transfer aid can be discharged together with the aqueous phase solution, solving the problem of difficulty in separation and extraction after the reaction.

[0031] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the description of the embodiments of the present application will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is a process flow chart of a method for applying an electrolyte as a dielectric in an unsaturated aromatic organic liquid hydrogenation reaction as proposed in an embodiment of the present application;

[0033] Figure 2 It is a schematic diagram of the structure of an H-type replaceable membrane electrolytic cell proposed in an embodiment of the present application;

[0034] Figure 3 It is a schematic diagram of the structure of the PEM proposed in the embodiment of the present application;

[0035] Figure 4 It is the linear voltammetric scanning curve before and after adding the substrate (toluene + hexadecyltrimethylammonium bromide) in Example 1 of the present application;

[0036] Figure 5 This is a comparison chart of gas chromatography analysis of the electrolyte solution with and without the phase transfer aid added in Example 1 of the present application after 1 hour of reaction;

[0037] Figure 6 It is the linear voltammetric scanning curve before and after adding the substrate (toluene + sodium dodecyl sulfate) in Example 4 of the present application;

[0038] Figure 7 It is a comparison chart of gas chromatography analysis of the electrolyte solution with and without the phase transfer aid added in Example 4 of the present application after reacting for 1 hour.

[0039] Description of reference numerals:

[0040] 1. H-type replaceable membrane electrolytic cell; 11. cathode chamber; 12. anode chamber; 13. proton exchange membrane;

[0041] 2. PEM; 21. anode plate; 22. anode gas diffusion layer; 23. hydrogenation catalyst layer; 24. cathode plate; 25. cathode gas diffusion layer; 26. cathode catalyst layer; 13. proton exchange membrane. DETAILED DESCRIPTION

[0042] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0043] In the drawings, the size of the constituent elements, the thickness of the layer or the area may be exaggerated for the sake of clarity. Therefore, any implementation of the present disclosure is not necessarily limited to the size shown in the drawings, and the shapes and sizes of the components in the drawings do not reflect the true proportions. In addition, the drawings schematically show ideal examples, and any implementation of the present disclosure is not limited to the shapes or values ​​shown in the drawings.

[0044] In related technologies, hydrogen will become an eco-friendly alternative energy source because of its gravimetric energy density (120MJkg -1 ) than gasoline (44MJkg -1 ) is much higher, and the only product of hydrogen combustion is water, which is environmentally friendly and pollution-free. The safe storage and transportation of large amounts of hydrogen are important for its practical application. Organic hydride systems are applications of hydrogenation / dehydrogenation of unsaturated / saturated organic compounds and have been proposed for the storage and transportation of H2.

[0045] The core principle of organic liquid hydrogen storage technology (LOHC for short) is to make olefins, alkynes, carbocyclic aromatic hydrocarbons, and aromatic compounds with conjugated structures react reversibly with hydrogen under the action of a catalyst. On the one hand, hydrogen is stored in unsaturated aromatic compounds, and on the other hand, hydrogen in hydrogen-rich organic liquids can be released through dehydrogenation reactions, while producing unsaturated aromatic compounds, and the aromatic compounds can be recycled. At present, conventional unsaturated aromatic compounds are hydrogenated by thermochemical methods, but their energy consumption is high. Electrochemical hydrogenation technology (ECH) can carry out hydrogenation reactions at mild temperatures (25°C to 80°C) and normal pressure conditions (1atm), thereby improving the safety of the catalytic hydrogenation process and the stability of the catalyst. Therefore, the electrochemical hydrogenation method can effectively reduce the difficulty of the hydrogenation reaction and reduce the severity of the reaction conditions.

[0046] However, the existing three-electrode electrocatalytic hydrogenation method has problems such as low substrate solubility, complex process, low hydrogenation efficiency, and slow reaction rate. The electrolyte composition in related studies is a microemulsion system composed of an organic phase, water, and a surfactant phase, which can promote the solubility of the organic liquid, thereby achieving electrochemical contact between the electrode and the aqueous phase and the organic phase, and promoting the hydrogenation reaction. The organic phase usually uses tert-butanol, DMF, and acetonitrile; the aqueous phase usually uses an aqueous sulfuric acid solution. However, the system requires the addition of additional organic phase solvents, such as DMF and acetonitrile, which are corrosive to a certain extent, have a great impact on the durability of the hydrogenation unit and the life of the catalyst, and are difficult to separate subsequently, causing serious environmental pollution.

[0047] Based on the above problems, the embodiments of the present application propose an electrolyte and its application in organic liquid hydrogen storage. The electrolyte has simple composition, is easy to separate, and has little environmental pollution. The application of the electrolyte in organic liquid hydrogenation reaction can not only promote the dissolution of organic substrates, but also promote the hydrogenation reaction rate, and has less impact on the durability of the device and the catalyst life.

[0048] In a first aspect, the present application provides an electrolyte, wherein the cathode electrolyte in the electrolyte is composed of a PBS buffer solution with a pH of 6.8 to 7.8 and a phase transfer aid;

[0049] Phase transfer aids include cetyltrimethylammonium bromide, sodium lauryl sulfate or tetrabutylammonium bromide.

[0050] The cathode electrolyte constructed in the embodiment of the present application contains only two phases, and there is no need to introduce a highly toxic and difficult to decompose organic phase as the electrolyte system, thereby avoiding subsequent separation difficulties and serious environmental pollution. Among them, the PBS buffer provides a neutral environment for the reaction, and then by adding a phase transfer agent, the problem of few proton donors in the neutral electrolyte is improved, the electrocatalytic hydrogenation reaction rate is increased, and the difficulty of hydrogenation is reduced; by adding a phase transfer agent, the aqueous electrolyte is connected to the oil phase organic liquid, and the solubility of the organic liquid for hydrogenation in the electrolyte is further improved, and the efficient dissolution of the organic liquid in the electrolyte is achieved, and the contact area between the organic liquid and the catalyst is increased.

[0051] In some embodiments, the PBS buffer is deionized water, Na2HPO4, KH2PO4, NaCl, and KCl.

[0052] In some embodiments, preferably, the pH of the PBS buffer is 7.2-7.4.

[0053] It should be noted that the secondary dissociation characteristics of the Na2HPO4 and KH2PO4 components contained in the PBS buffer solution can increase the number of protons in the aqueous solution and improve the reaction rate; and the NaCl and KCl in PBS can increase the salt ion concentration in the solution, further promoting conductivity, and can promote full contact between the non-conductive organic liquid and the phase transfer aid, thereby achieving efficient hydrogenation in a system without the need for an organic phase.

[0054] In some embodiments, the anolyte in the electrolyte includes sulfuric acid solution and / or deionized water.

[0055] In some embodiments, the concentration of the sulfuric acid solution is 0.1 mol / L to 0.5 mol / L.

[0056] In some embodiments, preferably, the concentration of the sulfuric acid solution is 0.2 mol / L.

[0057] Sulfuric acid solution and / or deionized water provide H for the reaction. + , H + After entering the cathode electrolyte, it promotes the reaction rate of electrocatalytic hydrogenation, thereby improving the hydrogenation efficiency.

[0058] In a second aspect, the present application provides an application of an electrolyte in organic liquid hydrogen storage, wherein the electrolyte is used as a dielectric in an organic liquid hydrogenation reaction.

[0059] When the electrolyte provided in the embodiment of the present application is applied to an organic liquid hydrogenation reaction, the electrolysis reaction efficiency is higher, the reaction conditions are simpler, and the feasibility is stronger.

[0060] In some embodiments, the electrolyte is used as a dielectric in the hydrogenation reaction of unsaturated aromatic compounds, and the unsaturated aromatic compounds react with hydrogen protons to obtain a hydrogen-rich organic liquid. Compared with the electrolyte with an organic phase, the hydrogenation rate is higher.

[0061] In some embodiments, the unsaturated aromatic compound includes one or more of toluene, dibenzyltoluene, N-ethylcarbazole, benzyltoluene, 3-methylindole, 7-methylindole, cyclopentylpyrazine, carbazole, N-ethylcarbazole, benzyltoluene, N-methylindole, N-ethylindole, pyrazine, 2,3-dimethylpyrazine, 2,5-dimethylpyrazine, 2-methylpyrazine, pyridazine, pyridine and 3-methylpyridine.

[0062] Unsaturated aromatic compounds have unique aromatic ring resonance bonds. Compared with the chemical bonds within other organic molecules, it is easier to hydrogenate aromatic organic compounds, and the overall hydrogen storage density is also higher.

[0063] In some embodiments, the molar ratio of the phase transfer aid to the unsaturated aromatic compound is 0.5:1 to 5:1.

[0064] If the phase transfer agent is excessive, it will cause an excess of electrolyte, which will hinder the electrolysis reaction; if it is too little, it will lead to insufficient dissolution of the organic phase and reduce the hydrogenation rate. Therefore, a reasonable molar ratio of the phase transfer agent and the unsaturated aromatic compound will help promote the dissolution of the organic phase, accelerate proton exchange, and increase the hydrogenation rate.

[0065] The optimal molar amount of the phase transfer aid is 0.5 mmol to 2 mmol.

[0066] In some embodiments, the molar amount of the unsaturated aromatic compound is 0.1 mmol to 5 mmol.

[0067] In some embodiments, the molar amount of the unsaturated aromatic compound may be 0.1 mmol, 0.2 mmol, 0.3 mmol, 0.4 mmol, or 0.5 mmol.

[0068] In some embodiments, see Figure 2 and Figure 3 The hydrogenation reactor for the hydrogenation reaction of unsaturated aromatic compounds includes: an H-type replaceable membrane electrolyzer 1 or a PEM 2.

[0069] In some embodiments, the H-type replaceable membrane electrolytic cell 1 includes a cathode chamber 11, an anode chamber 12, and a proton exchange membrane 13;

[0070] The H-type replaceable membrane electrolyzer 1 is an important electrochemical device that uses a special proton exchange membrane 13 to separate the anode and cathode, so that cations and anions can pass through the membrane without mixing during the electrolysis process. Working principle: based on the electrolysis reaction of water; when direct current passes through the electrolyzer, the unsaturated aromatic compound at the cathode absorbs electrons and combines with the hydrogen ions produced by electrolysis to generate hydrogen-rich organic liquid.

[0071] The PEM 2 includes an anode electrode plate 21 , an anode gas diffusion layer 22 , a hydrogenation catalyst layer 23 , a cathode electrode plate 24 , a cathode gas diffusion layer 25 , a cathode catalyst layer 26 , and a proton exchange membrane 13 .

[0072] PEM 2 is generally an electrolysis device that performs water decomposition reaction through proton exchange membrane 13 to produce hydrogen and oxygen. However, it can be used as a hydrogenation reactor, where water is introduced into the anode side and electrolyte is introduced into the cathode side, the anode and cathode are separated by the proton exchange membrane, and voltage / current is applied to achieve electrochemical hydrogenation. Working principle: Based on the electrolysis reaction of water; when direct current passes through the electrolytic cell, the unsaturated aromatic compound at the cathode absorbs electrons and combines with the hydrogen ions produced by electrolysis to generate hydrogen-rich organic liquid.

[0073] The proton exchange membrane 13 serves as a cation-conducting solid electrolyte, which can selectively conduct cations (such as protons) and prevent anions and other molecules from passing through, thereby maintaining the charge balance and electrolyte balance inside the electrolysis device.

[0074] In some embodiments, the proton exchange membrane 13 includes a Nafion 115 membrane, a Nafion 212 membrane, or a Nafion 117 membrane.

[0075] Nafion 115 membrane, Nafion 212 membrane and Nafion 117 membrane are all proton exchange membranes based on perfluorosulfonic acid (PFSA)13.

[0076] In some embodiments, see Figure 1 , the electrolyte is used as a dielectric in the hydrogenation reaction of unsaturated aromatic compounds, including:

[0077] Step S1: when the hydrogenation reactor is an H-type replaceable membrane electrolytic cell 1, take an appropriate amount of sulfuric acid solution to form an anolyte, take an appropriate amount of PBS buffer and a phase transfer aid, and mix them to obtain a catholyte;

[0078] Step S2: mixing a hydrogenation catalyst and an additive to prepare a catalytic slurry, impregnating a foamed metal with the catalytic slurry, inserting the obtained foamed metal electrode and a reference electrode into a cathode electrolyte, inserting a platinum electrode into an anode electrolyte, and then adding an unsaturated aromatic compound into the cathode electrolyte to form an electrolytic system, and performing an activation treatment on the electrolytic system;

[0079] Step S3: After activation, a constant current electrolysis reaction is performed to hydrogenate the unsaturated aromatic compound to obtain a hydrogen-rich organic liquid;

[0080] The embodiment of the present application utilizes the above method to apply the electrolyte to the organic liquid hydrogenation reaction. The phase transfer additive used is not easy to poison the catalyst, and it is non-toxic, harmless, environmentally friendly, and inexpensive. In addition, in the subsequent separation process of the hydrogen-rich organic liquid, the separation and purification steps are simple, ensuring the accuracy and reliability of the performance of the hydrogen-rich organic liquid. In the electrolysis process, no high temperature and high pressure conditions are required, the energy consumption is low, and the hydrogenation efficiency is high.

[0081] In some embodiments, the hydrogenation catalyst may be a PtRu / C catalyst;

[0082] The preparation method of the PtRu / C catalyst comprises:

[0083] Step S11: 120 mg of Ketjen Black EC300J powder was dissolved in a three-necked flask containing 30 mL of ethylene glycol, and ultrasonicated for 15 min to obtain a uniformly dispersed carbon support solution;

[0084] Step S12, set the stirring speed to 400 rpm, slowly add a platinum chloride salt solution with a concentration of 37 mg / ml and a volume of 1.83 ml, and a ruthenium chloride salt solution with a concentration of 23.63 mg / ml and a volume of 2.47 ml to the above carbon support solution, and continue stirring for 30 minutes to form a uniform dispersion system (in the dispersion system, Pt 2+ The mass of the ion is 53.4 mg, Ru 2+ The mass of the ion is 26.6 mg);

[0085] Step S13, adjusting the pH of the dispersed system to 10 with a 4 mol / L NaOH solution, and then moving the dispersed system to an oil bath for high-temperature reduction reaction, with the heating temperature set to 150° C. and the heating time being 1 h;

[0086] Step S14, when the reducing solution after the reaction is completed cools to room temperature, pour the reducing solution into a beaker, add 400 mL of deionized water and stir thoroughly for 1 hour;

[0087] Step S15, filter the reducing liquid in the beaker and wash it with deionized water, collect the product and place it in a vacuum drying oven for drying, set the drying oven temperature to 60°C, and dry it for 10 hours. After drying, grind the product into powder to obtain a PtRu / C catalyst.

[0088] The PtRu / C catalyst nanoparticles are evenly distributed and have controllable sizes. They do not agglomerate or accumulate, have higher intrinsic activity, and are helpful in improving the electrochemical hydrogenation efficiency of unsaturated aromatic compounds.

[0089] In some embodiments, the additive includes deionized water, anhydrous ethanol, and Nafion solution;

[0090] Nafion solution is a perfluorosulfonic acid polymer solution consisting of a fluorinated solvent containing Nafion polymer and additives.

[0091] In some embodiments, the concentration of the Nafion solution is 5 wt %.

[0092] In some embodiments, the method for preparing the catalytic slurry includes: taking appropriate amounts of PtRu / C catalyst, deionized water, anhydrous ethanol and Nafion solution, and ultrasonically mixing for 40 minutes to 50 minutes to prepare the catalytic slurry.

[0093] In some embodiments, the metal foam is immersed in the catalytic slurry for 12 min to 17 min to obtain a metal foam electrode.

[0094] In some embodiments, the foam metal needs to be pretreated before being immersed in the catalytic slurry, and the pretreatment method includes:

[0095] Step S21: Change the size to 1*1.5*0.15cm 3 The foam metal was cut and placed in a 3 mol / L HCl solution to fully immerse it;

[0096] Step S22: ultrasonically clean the impregnated metal foam for 10 minutes to remove the oxide layer and dirt impurities on the surface;

[0097] Step S23: performing ultrasonic oscillation treatment in anhydrous ethanol and acetone for 10 minutes respectively, and then washing with deionized water and anhydrous ethanol alternately for 3 times to remove excess hydrochloric acid on the surface;

[0098] Step S24: the washed product is transferred to a 60° C. forced air drying oven and dried for 1 h to obtain a pretreated foam metal electrode.

[0099] In some embodiments, appropriate amounts of PtRu / C catalyst, deionized water, anhydrous ethanol and Nafion solution are taken, and the temperature during ultrasonic mixing is 20° C. to 25° C., that is, it is carried out at room temperature and pressure.

[0100] In some embodiments, the metal foam includes iron foam, copper foam, or nickel foam.

[0101] In some embodiments, the preferred foam metal is nickel foam. Nickel foam has a three-dimensional structure, and its high specific surface area can significantly increase the contact area between the electrode surface and the electrolyte, thereby accelerating the rate of electrochemical reaction; its pore structure is conducive to the rapid transfer and transportation of electrons and ions, which helps to further improve the reaction speed and efficiency.

[0102] In some embodiments, after the metal foam is immersed in the catalytic slurry for 12 to 17 minutes, the obtained metal foam electrode is taken out and dried at 60 to 80 degrees Celsius for 1 to 2 hours. The dried metal foam electrode and the reference electrode are inserted into the cathode electrolyte to prevent other ions from entering the electrolyte. The reference electrode can be Ag / AgCl.

[0103] In some embodiments, when the hydrogenation reactor is an H-type replaceable membrane electrolytic cell 1, an appropriate amount of sulfuric acid solution is taken to form an anode electrolyte, and sulfuric acid molecules dissociate in the aqueous solution to form hydrogen ions (H + ), sulfate ion (SO4 2- ) is relatively stable and not prone to decomposition reaction at the anode.

[0104] In some embodiments, when the hydrogenation reactor is PEM 2, deionized water is taken to form an anolyte, and an appropriate amount of PBS buffer and a phase transfer aid are taken and mixed to obtain a catholyte;

[0105] Mixing a hydrogenation catalyst and an additive to prepare a hydrogenation catalyst slurry, and using the catalytic slurry to prepare a hydrogenation catalyst layer 23;

[0106] Inputting an anolyte into the anode of PEM 2, inputting a catholyte into the cathode of PEM 2, and adding an unsaturated aromatic compound to form an electrolysis system, and performing an activation treatment on the electrolysis system;

[0107] After activation, a constant current electrolysis reaction is performed to hydrogenate the unsaturated aromatic compounds to obtain a hydrogen-rich organic liquid.

[0108] The PEM 2 electrolysis process requires a high purity of the electrolyte. Deionized water can remove most of the ions in the water and reduce the interference of impurities in the electrolysis process. On the anode side, the water molecules in the deionized water lose electrons under the action of the electric field, undergoing an oxidation reaction to generate oxygen (O2) and hydrogen ions (H + ), the generated hydrogen ions (H + ) in hydrated form (H3O + ) is conducted to the cathode side through the proton exchange membrane 13; on the cathode side, hydrogen ions (H + ) obtains electrons, undergoes a reduction reaction, and hydrogen ions (H + ) with hydrogenation reaction of unsaturated aromatic compounds.

[0109] In some embodiments, performing activation treatment on the electrolytic system includes: performing activation treatment on the electrolytic system using a cyclic voltammetry scanning method and a linear voltammetry scanning method in sequence.

[0110] During activation, the electrolyte was first activated by cyclic voltammetry, with the potential set to -1.6 V to -0.2 V, and the scanning test was performed from positive to negative at a speed of 50 mV / s for 20 cycles;

[0111] After the cyclic voltammetry scan test, a linear voltammetry scan test was continued, with the potential set at -1.6 V to -0.2 V and a scan rate of 10 mV / s, until all activations were completed after the test was completed.

[0112] In some embodiments, the activation test of the electrolyte by cyclic voltammetry is performed twice, the first activation potential is set to -1.6V to -0.9V, and the scanning test is performed from positive to negative at a speed of 50mV / s for 15 cycles, and the second activation potential is set to -0.9V to -0.2V, and the scanning test is performed from positive to negative at a speed of 50mV / s for 5 cycles, and the CV activation is completed. After the cyclic voltammetry scanning test is completed, the linear voltammetry scanning test is continued, the potential is set to -1.6V to -0.2V, the scanning rate is 10mV / s, and all activations are completed after the test is completed.

[0113] Electrochemical activation is based on the fact that the charge layer formed on the electrode surface can change the adsorption capacity and charge state of the reactants, thereby affecting the reaction rate and selectivity. By controlling the shape, material, surface structure and electrode potential of the electrode, the adsorption and electron transfer processes of the reactants can be adjusted, thereby improving the efficiency and selectivity of the catalytic reaction. In the embodiment of the present application, cathode activation is that the electroreduction reaction carried out on the cathode is difficult to absorb electrons. In order to promote its absorption of electrons, it is necessary to make the cathode potential more negative than the equilibrium potential. In this potential range, the adsorption and electron transfer processes of the reactants are greatly improved, and the efficiency of the catalytic reaction is greatly improved.

[0114] In some embodiments, the activated electrolytic system is at -30 mA / cm -2 ~-70mA / cm -2 The electrolysis reaction can be carried out for at least 1h to 2h at a current density of , and a hydrogen-rich organic liquid is obtained. The reaction rate is fast and the hydrogenation rate is higher.

[0115] In order to enable those skilled in the art to better understand the present invention, a method for preparing a catalyst for electrochemical hydrogenation of aromatic compounds provided by the present invention is described below through a number of specific embodiments.

[0116] Example

[0117] Example 1

[0118] 1. Add 70 mL of PBS buffer (deionized water, Na2HPO4, KH2PO4, NaCl and KCl) with a pH of 7.4 and 1 mmol of hexadecyltrimethylammonium bromide into the cathode chamber of the H-type replaceable membrane electrolytic cell and stir for 10 min until completely dissolved;

[0119] 70 mL of 0.2 mol / L sulfuric acid solution was added to the anode chamber, and the anode chamber and cathode chamber were separated by a Nafion115 membrane;

[0120] 2. Add 12 mg of PtRu / C catalyst into a 10 mL glass bottle, add 2.30 mL of deionized water, 600 μL of anhydrous ethanol (95% or more) and 96 μL of Nafion solution (D520, 5 wt%) into the bottle with a pipette, mix and prepare a slurry, and then stir ultrasonically at 20 ° C for 45 min to obtain a catalytic slurry;

[0121] 3. 1*1.5*0.15cm 3The nickel foam was cut and placed in a 3 mol / L HCl solution, fully immersed, and then ultrasonically cleaned for 10 min. Then, it was ultrasonically oscillated in anhydrous ethanol and acetone for 10 min respectively, and then washed alternately with deionized water and anhydrous ethanol for 3 times. The obtained product was transferred to a 60°C forced air drying oven and dried for 1 h to obtain the pretreated nickel foam sample.

[0122] 4. Immerse the pretreated nickel foam sample in the catalytic slurry, take it out after immersion for 15 minutes, dry it at 60°C for 1 hour, insert the dried nickel foam electrode and Ag / AgCl electrode into the cathode electrolyte, insert the platinum wire into the anode electrolyte, and then add 1 mmol toluene into the cathode electrolyte to form an electrolytic system;

[0123] 5. The electrolytic system was activated by cyclic voltammetry. When performing cyclic voltammetry scanning, the potential was set to -1.6V to -0.2V, and the scanning test was performed from positive to negative at a speed of 50mV / s for 20 cycles. After the cyclic voltammetry scanning test, a linear voltammetry scanning test was continued, with the potential set to -1.2V to -0.4V and the scanning rate of 10mV / s. After the test, the activation was completed;

[0124] 6. The activated electrolyte is at -50mA / cm -2 A constant current electrolysis reaction was carried out at a current density of 1 h to obtain a hydrogen-rich organic liquid.

[0125] Embodiments 2 to 10

[0126] The difference between Examples 2 to 6 and Example 1 is that the types of unsaturated aromatic compounds are different, the molar amounts are different, or the added phase transfer aids are different;

[0127] The difference between Examples 7 to 10 and Example 1 is that the types of unsaturated aromatic compounds are different. See Table 1 below for details.

[0128] For the above-mentioned embodiments and comparative examples, a PEM electrolyzer can also be used to perform an electrochemical hydrogenation performance test in a two-electrode mode.

[0129] Embodiment 11

[0130] During the test, PtRu / C catalyst was used as cathode catalyst, IrO2 was used as anode catalyst, the cathode electrolyte was the same as that in Example 1, water was passed into the anode, and the test time was 1 hour.

[0131] Toluene was added to the cathode electrolyte, and the activation test of the electrolyte was performed twice by cyclic voltammetry. The first activation potential was set to -1.6V to -0.9V, and the scanning test was performed from positive to negative at a speed of 50mV / s for 15 cycles. The second activation potential was set to -0.9V to -0.2V, and the scanning test was performed from positive to negative at a speed of 50mV / s for 5 cycles, and the CV activation was completed. After the cyclic voltammetry scanning test, the linear voltammetry scanning test was continued, with the potential set to -1.6V to -0.2V and the scanning rate of 10mV / s, and all activations were completed after the test was completed.

[0132] The activated electrolyte was charged at -50 mA / cm -2 A constant current electrolysis reaction was carried out at a current density of 1 h to obtain a hydrogen-rich organic liquid.

[0133] Table 1

[0134]

[0135]

[0136] It should be noted that in the present application, based on Example 1, when other conditions remain unchanged, the linear voltammetric scan curve of the electrolyte before the addition of substrate (toluene and hexadecyltrimethylammonium bromide) is first tested, and then the linear voltammetric scan curve of the electrolyte after adding 1mmol toluene to the PBS buffer is tested, and finally 1mmol hexadecyltrimethylammonium bromide is added to the PBS buffer, stirred for 10min until completely dissolved, and then the linear voltammetric scan curve of the electrolyte is tested. The test results are shown in Figure 4 During the test, the electrolyte anode was 0.2 mol / L sulfuric acid solution, and the cathode was neutral PBS buffer; Figure 4 "1" means no substrate was added, "2" means only toluene was added, and "3" means toluene and hexadecyltrimethylammonium bromide were added.

[0137] according to Figure 4 It can be obtained that the current density of curves 1, 2 and 3 at low potential is negligible, which indicates that the electrocatalytic hydrogen evolution reaction (HER) performance of PtRu / C catalyst is poor in the solution without toluene. After adding toluene, the linear sweep voltammetry (LSV) curve of curve 2 shows a slight increase in current density and a decrease in the starting potential, which verifies that the hydrogenation reaction of toluene to methylcyclohexane is easier than the competitive HER; and after adding hexadecyltrimethylammonium bromide, the current density increases significantly and the starting potential decreases significantly, indicating that the electrocatalytic hydrogenation of toluene on the PtRu / C catalyst is more energetically favorable than HER, further proving the feasibility and superiority of the electrolysis system for the performance test of organic liquid hydrogenation.

[0138] In this application, based on Example 4, under the condition that other conditions remain unchanged, the linear voltammetric scanning curves of the electrolyte of Example 4 with and without the addition of a phase transfer agent are tested respectively. The results are shown in Figure 6 During the test, the electrolyte anode was 0.2 mol / L sulfuric acid solution, and the cathode was neutral PBS buffer; Figure 6 "1" means no substrate was added, "2" means only toluene was added, and "3" means toluene and sodium dodecyl sulfate were added.

[0139] In summary, according to Figure 4 and 6 It can be obtained that when no phase transfer agent is added, the current density without substrate and only toluene at low potential is negligible. After adding hexadecyltrimethylammonium bromide or sodium dodecyl sulfate, the current density increases significantly and decreases significantly at the starting potential, indicating that the electrocatalytic hydrogenation of toluene on PtRu / C catalyst is more energetically favorable than HER, and the universality of phase transfer agents has also been verified, further demonstrating the feasibility and superiority of this electrolysis system for testing the performance of organic liquid hydrogenation.

[0140] Using the electrolyte system in the present application, after 1h of constant current electrolysis reaction, extraction was performed with 20mL of ethyl acetate, and 1mL of the upper clear liquid was taken after sufficient shaking for 1min to 2min. After filtering out impurities, GC test (chromatography-mass spectrometry test) was performed. The electrochemical hydrogenation effect was verified according to the test results. The test results are shown in Table 1.

[0141] For Example 1, see Figure 5 Under the condition of adding the same unsaturated aromatic compound, the hydrogenation conversion rate of the system without adding hexadecyltrimethylammonium bromide is only 0.75%, while the hydrogenation conversion rate of the system with adding 1mmol hexadecyltrimethylammonium bromide is 15.91%. It can be proved that adding hexadecyltrimethylammonium bromide can promote the dissolution of unsaturated aromatic compounds, increase the contact area between organic liquid and catalyst, and thus achieve a significant improvement in hydrogenation effect.

[0142] For Example 4, see Figure 7 Under the condition of adding the same unsaturated aromatic compound, the hydrogenation conversion rate of the system without sodium dodecyl sulfate was only 0.70%, while the hydrogenation conversion rate of the system with 1mmol sodium dodecyl sulfate was 14.73%. It can be proved that the addition of sodium dodecyl sulfate can promote the dissolution of unsaturated aromatic compounds, increase the contact area between organic liquid and catalyst, and thus achieve a significant improvement in hydrogenation effect.

[0143] In summary, for different types of aromatic organic liquids, the solubility promoted by the phase transfer aid is different, resulting in different hydrogenation effects. However, regardless of the unsaturated aromatic compound, the hydrogenation rate without the phase transfer aid and with the phase transfer agent differs by at least 12%, which can prove that the addition of the phase transfer aid helps to improve the hydrogenation conversion rate. When the amount of phase transfer aid added is the same, when the unsaturated aromatic compound is toluene, the solubility is the highest, the contact area with the catalyst is the largest, and the highest hydrogenation conversion rate is achieved. Compared with Example 1, the molar amount of toluene in Example 2 is reduced, but the hydrogenation conversion rate is increased by 1.94% compared with Example 1. It may be due to the relatively reduced solubility of toluene in the aqueous solution system, so the hydrogenation rate is relatively increased. Compared with Comparative Example 1, the molar amount of toluene in Example 3 is increased, but the hydrogenation conversion rate is reduced by 1.76% compared with Example 1, which may be due to the relatively increased solubility of toluene in the aqueous solution system, resulting in a relatively reduced hydrogenation rate. The hydrogenation conversion rates in Examples 1 to 11 without adding a phase transfer aid are very low, because without adding a phase transfer aid, very little organic liquid is dissolved, and the contact area with the catalyst is very small, which leads to a very low hydrogenation conversion rate.

[0144] In summary, the present application provides an electrolyte with simple composition, low pollution, low price and easy configuration. The electrolyte is applied to the organic liquid hydrogenation reaction, which can further promote the dissolution of the organic liquid, and there is no need to introduce an organic phase as the electrolyte system, further reducing the defects of subsequent separation difficulties and environmental pollution.

[0145] The various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.

[0146] Although the preferred embodiments of the present application have been described, those skilled in the art may make additional changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the embodiments of the present application.

[0147] Finally, it should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or terminal device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or terminal device. In the absence of further restrictions, the elements defined by the sentence "including one..." do not exclude the existence of other identical elements in the process, method, article or terminal device including the elements.

[0148] The above is a detailed introduction to an electrolyte provided by the present application and its application in organic liquid hydrogen storage. Specific examples are used in this article to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea; at the same time, for general technicians in this field, according to the ideas of the present application, there will be changes in the specific implementation methods and application scopes. In summary, the content of this specification should not be understood as a limitation on the present application.

Claims

1. An electrolyte, characterized in that: The cathode electrolyte in the electrolyte is composed of a PBS buffer solution with a pH of 6.8 to 7.8 and a phase transfer aid; The phase transfer aid includes hexadecyltrimethylammonium bromide, sodium dodecyl sulfate or tetrabutylammonium bromide.

2. The electrolyte according to claim 1, characterized in that: The PBS buffer solution is deionized water, Na2HPO4, KH2PO4, NaCl and KCl.

3. The electrolyte according to claim 1, characterized in that: The anode electrolyte in the electrolyte includes sulfuric acid solution and / or deionized water.

4. The electrolyte according to claim 3, characterized in that: The concentration of the sulfuric acid solution is 0.1 mol / L to 0.5 mol / L.

5. Use of the electrolyte according to any one of claims 1 to 4 in organic liquid hydrogen storage, characterized in that: The electrolyte is used as a dielectric in an organic liquid hydrogenation reaction, and the unsaturated aromatic compound reacts with hydrogen protons to obtain a hydrogen-rich organic liquid.

6. The use of the electrolyte in organic liquid hydrogen storage according to claim 5, characterized in that: The unsaturated aromatic compound includes one or more of toluene, dibenzyltoluene, N-ethylcarbazole, benzyltoluene, 3-methylindole, 7-methylindole, cyclopentylpyrazine, carbazole, N-methylindole, N-ethylindole, pyrazine, 2,3-dimethylpyrazine, 2,5-dimethylpyrazine, 2-methylpyrazine, pyridazine, pyridine and 3-methylpyridine.

7. The use of the electrolyte in organic liquid hydrogen storage according to claim 5, characterized in that: The molar ratio of the phase transfer aid to the unsaturated aromatic compound is 0.5:1 to 5:

1.

8. The use of the electrolyte in organic liquid hydrogen storage according to claim 5, characterized in that: The molar amount of the unsaturated aromatic compound is 0.1 mmol to 5 mmol.

9. The use of the electrolyte in organic liquid hydrogen storage according to claim 5, characterized in that: The hydrogenation reactor for the hydrogenation reaction of unsaturated aromatic compounds comprises: an H-type replaceable membrane electrolytic cell (1) or a PEM (2); The H-type replaceable membrane electrolytic cell (1) comprises a cathode chamber (11), an anode chamber (12) and a proton exchange membrane (13); The PEM (2) comprises an anode plate (21), an anode gas diffusion layer (22), a hydrogenation catalyst layer (23), a cathode plate (24), a cathode gas diffusion layer (25), a cathode catalyst layer (26) and a proton exchange membrane (13).

10. The use of the electrolyte according to claim 9 in organic liquid hydrogen storage, characterized in that: The electrolyte is used as a dielectric in the hydrogenation reaction of unsaturated aromatic compounds, and includes: When the hydrogenation reactor is an H-type replaceable membrane electrolytic cell (1), taking an appropriate amount of sulfuric acid solution to form an anolyte, taking an appropriate amount of the PBS buffer and the phase transfer aid, and mixing them to obtain the catholyte; Mixing a hydrogenation catalyst and an additive to prepare a catalytic slurry, impregnating a foamed metal with the catalytic slurry, inserting the obtained foamed metal electrode and a reference electrode into the cathode electrolyte, inserting a platinum electrode into the anode electrolyte, adding the unsaturated aromatic compound into the cathode electrolyte to form an electrolysis system, and performing an activation treatment on the electrolysis system; After activation is completed, a constant current electrolysis reaction is performed to hydrogenate the unsaturated aromatic compound to obtain a hydrogen-rich organic liquid.

11. The use of the electrolyte in organic liquid hydrogen storage according to claim 9, characterized in that: The electrolyte is used as a dielectric in the hydrogenation reaction of unsaturated aromatic compounds, and includes: When the hydrogenation reactor is a PEM (2), deionized water is taken to form an anolyte, and an appropriate amount of the PBS buffer and the phase transfer aid are taken and mixed to obtain the catholyte; Mixing a hydrogenation catalyst and an additive to prepare a hydrogenation catalyst slurry, and using the catalytic slurry to prepare a hydrogenation catalyst layer (23); Inputting the anolyte into the anode of the PEM (2), inputting the catholyte into the cathode of the PEM (2), and adding the unsaturated aromatic compound to form an electrolysis system, and performing an activation treatment on the electrolysis system; After activation is completed, a constant current electrolysis reaction is performed to hydrogenate the unsaturated aromatic compound to obtain a hydrogen-rich organic liquid.

12. Use of the electrolyte according to claim 10 or 11 in organic liquid hydrogen storage, characterized in that: The activation treatment of the electrolytic system includes: sequentially performing activation treatment on the electrolytic system using a cyclic voltammetry scanning method and a linear voltammetry scanning test method; The activated electrolytic system is at -30 mA / cm -2 ~-70mA / cm -2 A constant current electrolysis reaction is carried out at a current density of to obtain the hydrogen-rich organic liquid.

Citation Information

Patent Citations

  • Ionic liquid / surface active agent modified glassy carbon electrode as well as preparation method and application thereof

    CN103940876A

  • Electrochemical hydrogenation cathode electrolyte and electrochemical hydrogenation method

    CN115558947A

  • PEM reactor based on organic liquid electrochemical hydrogenation and system thereof

    CN117004970A

  • PEM reactor for electrochemical hydrogenation and system thereof

    CN117026260A

  • Electrocatalytic hydrogenation and hydrodeoxygenation of oxygenated and unsaturated organic compounds

    US20140110268A1