Anisotropic composite film material as well as preparation method and application thereof

By constructing a composite structure of hydrophobic nanofiber membrane and metal nanowire layer in composite membrane materials, the problem of wet-thermal collaborative management in the prior art is solved, and directional sweat transmission and radiation heat dissipation are realized, providing all-weather humidity and heat management Effect.

CN118979341AActive Publication Date: 2024-11-19INSTITUTE OF MATERIALS & INTELLIGENT MANUFACTURING JIANGXI ACADEMY OF SCIENCES

Patent Information

Application Number
CN202411222376.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-19
Estimated Expiration
2044-09-02

AI Technical Summary

Technical Problem

In the prior art, radiation cooling materials and humidity management materials have their own defects, and they cannot achieve directional sweat transmission and all-weather adjustment of human radiation heating and heat dissipation in an environment with large changes in temperature and humidity, resulting in difficult to achieve joint moisture-heat management.

Method used

Using anisotropic composite membrane material, hydrophobic nanofiber membrane and metal nanowire layer are prepared through electrospinning technology, and through hole arrays and hydrophilic fiber channels are constructed in combination with laser punching and suction filtration technology to form hydrophobic nanofiber membrane/metal nanometers The linear layer composite structure realizes directional transmission of sweat and radiation heat dissipation.

Benefits of technology

It achieves humidity and thermal comfort in temperature and humidity changing environments, improves sweat transmission efficiency and radiation heat dissipation performance, is suitable for wearable humidity and heat management materials in the human body, and enhances the adaptability to complex climate environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979341A_ABST
    Figure CN118979341A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of an anisotropic composite membrane material. The preparation method comprises the following steps: preparing a hydrophobic nanofiber membrane by adopting an electrostatic spinning technology; coating a metal nanowire layer on the nanofiber membrane by adopting a vacuum filtration technology to obtain a hydrophobic nanofiber membrane / metal nanowire layer composite structure membrane; punching holes in the composite structure film by adopting a laser punching technology to form a through hole array penetrating through the composite structure film; the hydrophilic short fiber dispersion liquid is filtered from one side of the nanofiber membrane to one side of the metal nanowire layer through the through hole array by adopting a suction filtration technology, and a hydrophilic fiber channel array is obtained in the through hole array; and spinning a layer of hydrophilic nanofiber membrane on one side of the nanofiber membrane of the composite structure membrane by adopting an electrostatic spinning technology to prepare the anisotropic composite membrane material. The invention also discloses an anisotropic composite film material and application thereof. According to the invention, human body humidity management and heat management can be accurately realized, so that a human body can adapt to a more complex and extreme living environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of composite materials, and relates to a functional composite material that can be worn by the human body, and in particular to an anisotropic composite film material, a preparation method thereof, and an application thereof. Background Art

[0002] Maintaining human thermal comfort is the key to ensuring normal metabolism of the body. When the temperature of the environment in which the human body is located rises or falls sharply, it is difficult for the body temperature regulation system to maintain normal operation. For people engaged in sports, military and other special industries, such as construction workers, firefighters and medical personnel, they are frequently and intensely in extreme environments, which seriously threatens people's health. In order to maintain human thermal comfort, the following two methods are generally used: the first method is active cooling or heating, which generally uses traditional temperature control equipment such as air conditioners, heaters, and electric fans to control the ambient temperature. However, this temperature control method is only applicable to indoor environments, not outdoor environments, and will bring a lot of energy consumption, thereby aggravating the earth's energy crisis and emitting a lot of greenhouse gases; the second method is human thermal management technology. The goal of human thermal management technology is to regulate only personal body temperature. This efficient and energy-saving way to maintain human comfort has great potential and has attracted widespread attention.

[0003] With the progress of materials science and the rapid development of textile technology, a large number of thermal management materials and fabrics have been reported based on different ways of heat dissipation of the human body, such as radiation cooling, thermal conduction cooling, moisture absorption cooling, etc. Among them, radiation cooling materials can achieve passive cooling without external energy input, and will not cause environmental pollution. It is a green and environmentally friendly cooling method; its working principle is to reduce heat absorption by reflecting sunlight in the 0.3-2.5 μm band on the one hand, and on the other hand, the material spontaneously transmits heat in the form of infrared rays through the 8-13 μm "transparent atmospheric window" through the atmosphere to the outer space close to absolute zero, realizing energy transfer, and then making the material achieve the effect of lower than the ambient temperature. For example, low mid-infrared (MIR) (7-14 μm) emissivity and high MIR emissivity materials are coated on both sides of the fabric, so that the fabric can simultaneously obtain dual-mode thermal management characteristics of human body radiation heating or heat dissipation (Hsu P.-C et al, ScienceAdvances, 2017, 3, e1700895). Some smart fabrics composed of nanofibers and nanoparticles have also been successfully applied to human thermal management. They achieve outdoor radiation heat dissipation of the human body by suppressing the absorption of solar radiation and enhancing the fabric MIR emissivity (Cai L. et al, Advanced Materials, 2018, 30, 1802152). However, most of the above thermal management fabrics ignore the human body humidity management function and cannot achieve the synchronous management of human body humidity and heat.

[0004] Human humidity management materials can transport sweat from the surface of human skin to the environment in a directional manner, thereby avoiding the sticky feeling on the surface of the human body. Humidity management materials can transfer sweat from the inner surface of the material to the outer surface of the material under the action of capillary force. In fact, traditional hydrophilic materials such as cotton have strong capillary forces and can easily absorb sweat from the surface of the skin. However, due to its limited one-way liquid transport capacity and relatively slow water evaporation rate, a large amount of sweat still exists in the form of block water and adheres to the skin. Therefore, people will have a sticky and uncomfortable feeling. In order to solve this limitation, researchers have done a lot of research in the field of directional water transport. In nature, researchers have found that the phenomenon of directional liquid transport is common in animals and plants such as shorebird beaks, pitcher plants, spider silk, and cactus thorns (Zheng Y. et al, Nature, 2010,463, 640-643). Inspired by these natural phenomena, researchers have designed some human moisture management fabrics with Janus structures or wettability gradients (Wu J. et al, Soft Matter, 2012, 8, 5996-5999). The above fiber fabrics can successfully avoid the sticky feeling of the human body through directional sweat transmission, but these materials usually ignore the thermal management performance of the human body.

[0005] In summary, various radiation cooling materials and humidity management materials in the prior art have their own defects. Therefore, it is of practical significance to invent a moisture-heat synergistic management material that can achieve all-weather regulation of sweat directional transmission, human body radiation heating and heat dissipation when the temperature and humidity change greatly, but it still faces huge challenges. Summary of the invention

[0006] To solve the above problems, the purpose of the present invention is to provide an anisotropic composite membrane material and a preparation method thereof, as well as the application of the anisotropic composite membrane material, wherein the anisotropic composite membrane material can enable the human body to simultaneously obtain humidity comfort and thermal comfort in an environment where the temperature and humidity change greatly; when one side of the nanofiber membrane with high infrared emissivity, high solar radiation reflectivity and hydrophilicity faces outward, it can achieve excellent outdoor radiation heat dissipation function by reflecting solar radiation and radiating infrared to the environment; sweat can be directionally transmitted from one side of the metal nanowire to the other side of the hydrophilic nanofiber membrane along the hydrophilic fiber channel, thereby achieving the human body humidity management function; when the hydrophobic and low infrared emissivity metal nanowire side faces outward, it can achieve the radiation warmth function by suppressing the infrared radiation of the human body.

[0007] In order to achieve the above-mentioned invention object, the present invention adopts the following technical scheme: A method for preparing an anisotropic composite film material comprises the following steps: S1. Preparation of hydrophobic nanofiber membrane: preparing a hydrophobic nanofiber membrane with a thickness of 80 μm to 120 μm by electrospinning technology; S2, coating a metal nanowire layer: coating a metal nanowire layer with a thickness of 10 μm to 30 μm on the nanofiber membrane in step S1 by vacuum filtration technology to obtain a hydrophobic nanofiber membrane / metal nanowire layer composite structure membrane; S3, constructing a through hole array: using laser punching technology to punch holes in the hydrophobic nanofiber membrane / metal nanowire layer composite structure membrane in step S2 to form a through hole array that penetrates the composite structure membrane; S4, constructing a hydrophilic fiber channel array: using a suction filtration technique to filter the hydrophilic short fiber dispersion from one side of the nanofiber membrane to the side of the hydrophobic metal nanowire layer through the through-hole array in step S3, and obtaining a hydrophilic fiber channel array in the through-hole array; the preparation method of the hydrophilic fiber channel array is as follows: S4.1, adding the nanoparticles to an organic solvent and subjecting the organic solvent to ultrasonic treatment for 1 to 3 h to uniformly disperse the nanoparticles to obtain a nanoparticle dispersion; S4.2, adding a hydrophilic polymer to the nanoparticle dispersion in step S4.1, stirring at room temperature for 12 to 24 hours to fully dissolve, and obtaining a suspension containing 2.0 to 3.9% by mass of nanoparticles and 10 to 20% by mass of the hydrophilic polymer; S4.3, electrospinning the suspension in step S4.2 to obtain hydrophilic polymer-nanoparticle fibers; S4.4, cutting the hydrophilic polymer-nanoparticle fibers in step S4.3, adding deionized water, performing shear treatment, and dispersing them evenly to obtain a hydrophilic fiber dispersion with a mass concentration of 0.005 to 0.01 g / mL; S4.5, filtering the hydrophilic fiber dispersion in step S4.4 by vacuum filtration, with a vacuum degree of -10 to -5 kPa, to obtain a hydrophilic polymer-nanoparticle fiber channel array in the through-hole array on the hydrophobic nanofiber membrane / metal nanowire layer composite structure membrane; S5. Laminating hydrophilic nanofiber membrane: using electrospinning technology to spin a layer of hydrophilic nanofiber membrane with a thickness of 80 to 120 μm on one side of the nanofiber membrane of the hydrophobic nanofiber membrane / metal nanowire layer composite structure membrane in step S4, to prepare an anisotropic composite membrane material.

[0008] Furthermore, in the above-mentioned step S1, the preparation method of the hydrophobic nanofiber membrane is: dissolving a polymer in a solvent, stirring evenly, to obtain a polymer solution with a mass fraction of 6 to 15%; electrospinning the polymer solution to obtain a hydrophobic nanofiber membrane; the solvent is one of acetone, N,N-dimethylformamide, N,N-dimethylacetamide, tetrahydrofuran, or a mixture of two thereof; the polymer is one of polyvinylidene fluoride-hexafluoropropylene, polyurethane, and polyvinylidene fluoride.

[0009] Furthermore, in the above step S1, the step of electrospinning the polymer solution is as follows: the polymer solution is loaded into a syringe, fixed on an electrospinning machine for electrospinning, and a roller covered with tin foil is used to receive the fiber sample to obtain a hydrophobic nanofiber membrane.

[0010] Furthermore, in the above-mentioned step S1, the process parameters of the electrospinning technology are: using tin foil as the receiving substrate, the roller diameter is 13 to 20 cm, the roller speed is 150 to 350 r / min, the receiving distance is 15 to 25 cm, the propulsion speed is 0.5 to 1.0 mL / h, the voltage is 15 to 25 kV, and the spinning time is 60 to 90 min.

[0011] Furthermore, in the above step S1, the pores of the nanofiber membrane are 0.3 μm to 5.0 μm, the diameter of a single fiber is 0.18 μm to 0.9 μm, and the contact angle of the fiber membrane is 130° to 152°.

[0012] Furthermore, in the above step S2, the dispersion of metal nanowires with a mass fraction of 90-97% is diluted with anhydrous ethanol to obtain a dispersion of metal nanowires with a mass fraction of 2-5%; the diluted dispersion of metal nanowires is coated on the nanofiber membrane in step S1 using a vacuum filtration technique, the vacuum degree is -10 to -5 kPa, and the coating thickness is 10 μm to 30 μm, to obtain a hydrophobic nanofiber membrane / metal nanowire layer composite structure membrane.

[0013] Furthermore, in the above step S2, the metal nanowire has a diameter of 0.08 μm to 0.15 μm and a length of 30 μm to 50 μm.

[0014] Furthermore, in the above step S2, the metal nanowire is one of copper nanowire, silver nanowire and nickel nanowire.

[0015] Furthermore, in the above step S2, the dispersion liquid of the metal nanowires is a volatile organic solvent dispersion liquid, including but not limited to methanol, ethanol, and n-hexane.

[0016] Furthermore, in the above step S3, the size of each through hole of the through hole array is 100 μm to 200 μm, and the through hole spacing is 0.7 mm to 1.7 mm.

[0017] Furthermore, in the above step S3, the laser punching technology includes: power of 10 to 30 W, and punching time of 0.15 to 1.00 s.

[0018] Furthermore, in the above step S4.1, the particle size of the nanoparticles is 7 to 40 nm, and the mass fraction of the nanoparticles in the nanoparticle dispersion is 2.3 to 4.4%.

[0019] Furthermore, in the above step S4.1, the nanoparticles are selected from the group consisting of SiO2 nanoparticles, TiO2 nanoparticles, CeO2 nanoparticles, Al2O3 nanoparticles, and ZnO nanoparticles.

[0020] Furthermore, in the above step S4.1, the organic solvent is one of acetone, N,N-dimethylformamide, m-cresol, N,N-dimethylacetamide, and tetrahydrofuran.

[0021] Furthermore, in the above step S4.1, the ultrasonic treatment conditions are: power of 200 to 300 W, and time of 1 to 3 h.

[0022] Furthermore, in the above step S4.2, the hydrophilic polymer is one of polyacrylonitrile, cellulose acetate, and nylon 66.

[0023] Furthermore, in the above step S4.3, the process parameters of the electrospinning technology are: working voltage is 10-20 kV, receiving distance is 15-25 cm, and propulsion rate is 0.5-1 mL / h.

[0024] Furthermore, in the above step S4.5, the hydrophilic fiber channel array protrudes from one side of the metal nanowire layer by 3 μm to 10 μm.

[0025] Furthermore, in the above-mentioned step S5, the method for bonding the hydrophilic nanofiber membrane is: electrospinning one side of the hydrophobic nanofiber membrane of the hydrophobic nanofiber membrane / metal nanowire composite structure membrane containing the hydrophilic fiber channel array in step S4 at a working voltage of 10 to 20 kV and a receiving distance of 15 to 25 cm at a propulsion rate of 0.5 to 1 mL / h to spin a layer of hydrophilic nanofiber membrane.

[0026] The present invention also provides an anisotropic composite membrane material prepared by the preparation method of the above-mentioned anisotropic composite membrane material, which comprises, from bottom to top, a metal nanowire layer, a hydrophobic nanofiber membrane, and a hydrophilic nanofiber membrane. The hydrophobic nanofiber membrane / metal nanowire layer composite structure membrane composed of the metal nanowire layer and the hydrophobic nanofiber membrane has a through hole array, and a hydrophilic fiber channel array is arranged in the through hole array. The hydrophilic fiber channel array forms a layer of short fiber membrane on one side of the hydrophobic nanofiber membrane, which is in contact with the hydrophilic nanofiber membrane; the hydrophobic nanofiber membrane in the hydrophobic nanofiber membrane / metal nanowire composite structure membrane has a thickness of 80 μm to 120 μm, and the thickness of the metal nanowire layer is 10 μm to 30 μm; the thickness of the hydrophilic nanofiber membrane is 80 μm to 120 μm.

[0027] Furthermore, one end of the hydrophilic fiber channel array protrudes from one side of the metal nanowire layer by 3 μm to 10 μm.

[0028] Another object of the present invention is to provide an application of the above-mentioned anisotropic composite film material in wearable moisture and heat management materials for the human body and medical wound dressings.

[0029] Due to the adoption of the above-mentioned technical solution, the present invention has the following advantages: The preparation method of the anisotropic composite membrane material of the present invention is simple, easy to operate, low in cost, recyclable and suitable for large-scale production; the prepared anisotropic composite membrane material has good stability, is safe and environmentally friendly, and efficiently realizes sweat transmission; the thickness and photothermal properties of each layer of the membrane are controllable, and compared with traditional cotton fabrics, the infrared emissivity of the hydrophobic metal nanowires of the anisotropic composite membrane material is lower than that of the cotton fabric, and the solar radiation reflectivity of the hydrophilic nanofiber membrane is higher than that of the cotton fabric; when one side of the metal nanowire layer faces outward, the anisotropic composite membrane material increases the advantage of human body radiation heating; when one side of the hydrophilic nanofiber membrane faces outward and the human body is in a hot sun environment, the anisotropic composite membrane increases the advantage of human body radiation heat dissipation.

[0030] When one side of the hydrophilic nanofiber membrane with high infrared emissivity and high solar radiation reflectivity faces outward, it achieves excellent outdoor radiation heat dissipation function by reflecting solar radiation and radiating infrared to the environment; under the action of Laplace pressure difference and hydrophilic capillary force, sweat can be directionally transmitted from one side of the hydrophobic metal nanowire layer to the other side of the hydrophilic nanofiber membrane along the hydrophilic fiber channel and discharged, which has the effect of moisture absorption and perspiration and breathability, thereby realizing the human body humidity management function; when one side of the hydrophobic and low infrared emissivity metal nanowire layer faces outward, it achieves the radiation warmth function by suppressing the infrared radiation of the human body.

[0031] The anisotropic composite film material of the present invention integrates the functions of perspiration, indoor radiant heating and outdoor radiant cooling, and can be used as a wearable composite material to accurately achieve human body humidity management and thermal management, and provide the human body with a functional material of a physiologically comfortable microclimate, thereby enabling the human body to adapt to a more complex and extreme living environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 It is a process flow chart of the preparation method of the anisotropic composite membrane material of the present invention; Figure 2 It is a schematic structural diagram of a hydrophobic nanofiber membrane / metal nanowire layer composite structure membrane having a through hole array on the anisotropic composite membrane material of the present invention; Figure 3 It is a front structural schematic diagram of a hydrophilic fiber channel array on a hydrophobic nanofiber membrane / metal nanowire layer composite structure membrane of anisotropic composite membrane material of the present invention; Figure 4 It is a schematic diagram of the back structure of a hydrophilic fiber channel array on a hydrophobic nanofiber membrane / metal nanowire layer composite structure membrane of anisotropic composite membrane material of the present invention; Figure 5 It is a schematic structural diagram of the anisotropic composite membrane material of the present invention; Figure 6is a scanning electron microscope (SEM) image of the hydrophobic nanofiber membrane in Example 1 of the anisotropic composite membrane material of the present invention; Figure 7 is a contact angle diagram of the hydrophobic nanofiber membrane in Example 1 of the anisotropic composite membrane material of the present invention; Figure 8 is an optical microscope image of the copper nanowire layer in Example 1 of the anisotropic composite film material of the present invention; Fig. 9 is a scanning electron microscope (SEM) image of the copper nanowire layer in Example 1 of the anisotropic composite film material of the present invention; Fig.10 is a contact angle diagram of the copper nanowire layer surface in Example 1 of the anisotropic composite film material of the present invention; Fig.11 This is an optical microscope image of the copper nanowire layer / hydrophobic nanofiber membrane composite structure after laser punching in Example 1 of the anisotropic composite membrane material of the present invention; Fig.12 a is an optical microscope image of the hydrophilic fiber channel in Example 1 of the anisotropic composite membrane material of the present invention; Fig.12 b is a scanning electron microscope (SEM) image of the hydrophilic fiber channel in Example 1 of the anisotropic composite membrane material of the present invention; Fig.13 is a scanning electron microscope (SEM) image of the hydrophilic PAN-SiO2 fiber membrane in Example 1 of the anisotropic composite membrane material of the present invention; Fig.14 is a contact angle diagram of the hydrophilic nanofiber membrane in Example 1 of the anisotropic composite membrane material of the present invention; Fig.15 is the state diagram of the time when the droplet infiltrates the different hydrophilic nanofiber membranes; Fig.16 is a diagram showing the process of water droplets being transferred from the hydrophobic side to the hydrophilic side along the hydrophilic fiber channel in Example 1 of the present invention; Fig.17 This is a solar radiation reflectivity test diagram of one side of the hydrophilic PAN-SiO2 fiber membrane in Example 1 of the anisotropic composite membrane material of the present invention and a control sample; Fig.18 This is a test diagram of infrared emissivity of one side of the hydrophilic PAN-SiO2 fiber membrane in Example 1 of the anisotropic composite membrane material of the present invention and a control sample; Fig.19 It is a temperature change curve diagram after the artificial skin covers different samples under outdoor sunlight environment, wherein one side of the hydrophilic PAN-SiO2 fiber membrane in Example 1 of the present invention faces outward; Fig. 20 yes Fig.19Comparison of average temperature values ​​of different samples covered by artificial skin; Fig.21 This is a test graph of infrared emissivity of the punched copper nanowires in Example 1 of the anisotropic composite film material of the present invention and a control sample; Fig. 22 is a temperature change curve diagram after the artificial skin covers different samples in an indoor environment, wherein one side of the metal nanowire layer in Example 1 of the present invention faces outward; Fig.23 yes Fig. 22 Comparison of average temperature values ​​after different samples are covered with artificial skin; In the figure: 1 - metal nanowire layer; 2 - through hole; 3 - hydrophobic nanofiber membrane; 4 - hydrophilic fiber channel; 5 - hydrophilic nanofiber membrane. DETAILED DESCRIPTION

[0033] The present invention can be further described in detail with reference to the following examples; however, the following examples are merely illustrative, and the present invention is not limited to these examples.

[0034] like Figure 1 As shown, a method for preparing an anisotropic composite film material comprises the following steps: S1. Preparation of hydrophobic nanofiber membrane: dissolve the polymer in a solvent, stir magnetically at room temperature for 8-12 h until it is evenly dispersed, and obtain a polymer solution with a mass fraction of 6-15%; load the polymer solution into a syringe, fix it on an electrospinning machine for electrospinning, and use a roller with tin foil attached to receive the fiber sample to obtain a hydrophobic nanofiber membrane with a thickness of 80 μm-120 μm. The process parameters of the electrospinning technology are: tin foil is used as the receiving substrate, the roller diameter is 13-20 cm, the roller speed is 150-350 r / min, the receiving distance is 15-25 cm, the propulsion speed is 0.5-1.0 mL / h, the voltage is 15-25 kV, and the spinning time is 60-90 min; Preferably, the solvent is one of acetone (AC), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAC), tetrahydrofuran (THF) or a mixture of two thereof; the polymer is one of polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP), polyurethane (PU), polyvinylidene fluoride (PVDF); Preferably, the pores of the nanofiber membrane are 0.3 μm to 5.0 μm, the diameter of a single nanofiber is 0.18 μm to 0.9 μm, and the contact angle of the fiber membrane is 130° to 152°; S2, coating a metal nanowire layer: diluting a dispersion of metal nanowires having a mass fraction of 90-97% with anhydrous ethanol to obtain a dispersion of metal nanowires having a mass fraction of 2-5%; coating the diluted dispersion of metal nanowires on the nanofiber membrane in step S1 using a vacuum filtration technique, the vacuum degree being -10 to -5 kPa, and the coating thickness being 10 μm to 30 μm, to obtain a hydrophobic nanofiber membrane / metal nanowire layer composite structure membrane; the diameter of the metal nanowires being 0.08 μm to 0.15 μm, and the length being 30 μm to 50 μm; Preferably, the metal nanowire is one of copper nanowire, silver nanowire and nickel nanowire; Preferably, the dispersion of the metal nanowires is a volatile organic solvent dispersion, including but not limited to methanol, ethanol, and n-hexane; S3, constructing a through-hole array: using laser punching technology to punch holes in the hydrophobic nanofiber membrane / metal nanowire layer composite structure membrane in step S2 to form a through-hole array that penetrates the composite structure membrane; preferably, the laser punching technology includes: a power of 10 to 30 W, and a punching time of 0.15 to 1.00 s; preferably, the size of each through-hole of the through-hole array is 100 μm to 200 μm, and the through-hole spacing is 0.7 mm to 1.7 mm; S4, constructing a hydrophilic fiber channel array: using a suction filtration technique to filter the hydrophilic short fiber dispersion from one side of the nanofiber membrane to the side of the hydrophobic metal nanowire layer through the through-hole array in step S3, a hydrophilic fiber channel array is obtained in the through-hole array, one end of the hydrophilic fiber channel array protrudes 3 μm to 10 μm from one side of the metal nanowire layer, and a short fiber membrane is formed on one side of the hydrophobic nanofiber membrane; the preparation method of the hydrophilic fiber channel array is as follows: S4.1. Add nanoparticles with a particle size of 7 to 40 nm into an organic solvent and perform ultrasonic treatment at a power of 200 to 300 W for 1 to 3 h to uniformly disperse the nanoparticles to obtain a nanoparticle dispersion with a nanoparticle mass fraction of 2.3 to 4.4%; Preferably, the nanoparticles are selected from the group consisting of SiO2 nanoparticles, TiO2 nanoparticles, CeO2 nanoparticles, Al2O3 nanoparticles, and ZnO nanoparticles; Preferably, the organic solvent is one of acetone, N,N-dimethylformamide, m-cresol, N,N-dimethylacetamide, and tetrahydrofuran; S4.2, adding a hydrophilic polymer to the nanoparticle dispersion in step S4.1, stirring at room temperature for 12 to 24 hours to fully dissolve, and obtaining a suspension containing 2.0 to 3.9% by mass of nanoparticles and 10 to 20% by mass of the hydrophilic polymer; Preferably, the hydrophilic polymer is one of polyacrylonitrile, cellulose acetate, and nylon 66; S4.3, electrospinning the suspension in step S4.2 at a working voltage of 10 to 20 kV, a receiving distance of 15 to 25 cm, and a propulsion rate of 0.5 to 1 mL / h to obtain hydrophilic polymer-nanoparticle fibers; S4.4, cutting the hydrophilic polymer-nanoparticle fibers in step S4.3, adding deionized water, and performing shearing treatment, with a homogenizer processing speed of 5000-10000 r / min, a processing time of 0.5-1 h, and dispersing them evenly to obtain a hydrophilic fiber dispersion with a mass concentration of 0.005-0.01 g / mL; S4.5, placing one side of the metal nanowire layer of the hydrophobic nanofiber membrane / metal nanowire layer composite structure membrane containing a through-hole array in step S3 on a sand core; filtering the hydrophilic fiber dispersion in step S4.4 by vacuum filtration at a vacuum degree of -10 to -5 kPa, and obtaining a hydrophilic polymer-nanoparticle fiber channel array in the through-hole array on the composite structure membrane; S5. Laminating hydrophilic nanofiber membrane: electrospin one side of the hydrophobic nanofiber membrane of the hydrophobic nanofiber membrane / metal nanowire composite structure membrane containing a hydrophilic fiber channel array in step S4 at a working voltage of 10 to 20 kV and a receiving distance of 15 to 25 cm at a propulsion rate of 0.5 to 1 mL / h to spin a layer of hydrophilic nanofiber membrane with a thickness of 80 to 120 μm to obtain an anisotropic composite membrane material.

[0035] like Figures 2 to 5 As shown, the anisotropic composite membrane material prepared by the preparation method of the anisotropic composite membrane material comprises, from bottom to top, a metal nanowire layer 1, a hydrophobic nanofiber membrane 3, and a hydrophilic nanofiber membrane 5. The hydrophobic nanofiber membrane / metal nanowire layer composite structure membrane composed of the metal nanowire layer and the hydrophobic nanofiber membrane has an array of through holes 2, and an array of hydrophilic fiber channels 4 is arranged in the through hole array. One end of the hydrophilic fiber channel array protrudes 3 μm to 10 μm from one side of the metal nanowire layer, and a layer of short fiber membrane is formed on one side of the hydrophobic nanofiber membrane, which is in contact with the hydrophilic nanofiber membrane. The hydrophobic nanofiber membrane in the hydrophobic nanofiber membrane / metal nanowire composite structure membrane has a thickness of 80 μm to 120 μm, and the thickness of the metal nanowire layer is 10 μm to 30 μm; the thickness of the hydrophilic nanofiber membrane is 80 μm to 120 μm.

[0036] The application method of the anisotropic composite film material prepared by the method of the present invention is that it can realize the functions of radiation heating on one side, heat dissipation on the other side and directional transmission of sweat, thereby simultaneously managing the humidity and heat of the human body. When one side of the metal nanowire with low infrared emissivity faces outward, the anisotropic composite film can achieve excellent radiation heating function because the metal nanowire can effectively isolate the infrared radiation of the human body; and when the hydrophilic side with high solar radiation reflectivity and high infrared emissivity faces outward, under the premise of not hindering the infrared radiation of the human body, the anisotropic composite film can reflect solar radiation, so that the anisotropic composite film shows the advantage of outdoor radiation cooling under sunlight. In addition, when the human body sweats, because the anisotropic composite film has wettability and structural anisotropy, sweat can be directional transmitted from one side of the hydrophobic metal nanowire layer to one side of the hydrophilic fiber membrane along the hydrophilic fiber channel array, thereby realizing the function of human body humidity management. The anisotropic composite film material of the present invention can be used as an all-weather heat and humidity management material, so that people can adapt to a more complex and changeable climate environment. Example 1

[0037] A method for preparing an anisotropic composite film material comprises the following specific steps: S11, preparation of hydrophobic nanofiber membrane: 10 parts by weight of polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) was put into 90 parts by weight of a solvent, wherein the solvent was a mixture of acetone (AC) and N,N-dimethylacetamide (DMAC) in a mass ratio of 9:4, and stirred at room temperature for 8 hours until the mixture was uniformly dispersed to obtain a PVDF-HFP solution with a mass fraction of 10%. The PVDF-HFP solution was loaded into a syringe, fixed on an electrospinning machine for electrospinning, and a roller covered with tin foil was used to receive the fiber sample to obtain a hydrophobic PVDF-HFP nanofiber membrane with a thickness of 80 μm, such as Figure 6 , Figure 7 As shown, the fiber surface is smooth and the contact angle of the fiber film is 142.9°; the process parameters of the electrospinning technology are: tin foil is used as the receiving substrate, the roller diameter is 15 cm, the roller speed is 200 r / min, the receiving distance is 15 cm, the propulsion speed is 0.5 mL / h, the voltage is 15 kV, and the spinning time is 60 min; S12, coating metal nanowire layer: A 97% copper nanowire n-hexane solution produced by Shanghai Aladdin Biochemical Technology Co., Ltd. was selected and diluted with anhydrous ethanol to a 2% copper nanowire dispersion; the diluted copper nanowire dispersion was then coated on the hydrophobic PVDF-HFP nanofiber membrane in step S11 using a vacuum filtration technique at a vacuum degree of -5 kPa, and a 30 μm thick layer of the following was coated. Figure 8 , Fig. 9 The copper nanowire layer shown in the figure obtains a hydrophobic PVDF-HFP nanofiber membrane / copper nanowire layer (Cu NWs) composite structure membrane; Fig.10 As shown, the contact angle of water on the copper nanowire layer side of the hydrophobic PVDF-HFP nanofiber membrane / Cu NWs composite structure membrane is 150.1°; S13, constructing a through hole array: like Fig.11 As shown, a laser punching technique is used to punch holes on a hydrophobic PVDF-HFP nanofiber membrane / Cu NWs composite structure membrane to form a through-hole array penetrating the composite structure membrane, wherein the through-hole size is 150 μm and the through-hole spacing is 0.9 mm; the laser punching power is 10 W and the punching time is 0.35 s; S14, constructing a hydrophilic fiber channel array: First, 3 parts by weight of SiO2 nanoparticles (SiO2NPs) were added to 84 parts by weight of N, N-dimethylformamide (DMF) and ultrasonically treated at a power of 200 W for 1 h to uniformly disperse the SiO2NPs to obtain a SiO2 / DMF dispersion. Then, 13 parts by weight of polyacrylonitrile (PAN) were added to the uniform SiO2 / DMF dispersion and stirred at room temperature for 24 h to fully dissolve the dispersion to obtain a suspension containing 3% by weight of SiO2NPs and 13% by weight of PAN. The prepared suspension was electrospun at a propulsion rate of 0.5 mL / h at a working voltage of 20 kV and a receiving distance of 15 cm to obtain PAN-SiO2 fibers. Next, the PAN-SiO2 fibers were cut, deionized water was added, and a Quhor EA300-T emulsifier homogenizer was used to shear the fibers at a speed of 5000 rpm for 1 h to uniformly disperse the fibers to obtain a PAN-SiO2 fiber with a mass concentration of 0.005. g / mL of hydrophilic PAN-SiO2 fiber dispersion; finally, the Cu NWs side of the hydrophobic PVDF-HFP nanofiber membrane / Cu NWs composite structure membrane containing a through-hole array was placed on the sand core, and the PAN-SiO2 dispersion was filtered by vacuum filtration with a vacuum degree of -5 kPa, and the following was obtained in the through-hole array of the hydrophobic PVDF-HFP nanofiber membrane / Cu NWs composite structure membrane: Fig.12 The PAN-SiO2 fiber channel array shown in the figure has one end protruding 5 μm from the Cu NWs side; a short fiber membrane is formed on one side of the hydrophobic PVDF-HFP nanofiber membrane; S15, laminating hydrophilic nanofiber membrane: on the PVDF-HFP nanofiber membrane side of the hydrophobic PVDF-HFP nanofiber membrane / Cu NWs composite structure membrane in step S14, electrospinning was performed at a propulsion rate of 0.5 mL / h under the conditions of working voltage 20 kV and receiving distance 15 cm to spin a layer of hydrophilic PAN-SiO2 nanofiber membrane with a thickness of 100 μm, and the contact angle of the nanofiber membrane was 0°, as shown in FIG. Fig.13 , Fig.14 As shown, an anisotropic composite membrane material is prepared.

[0038] Performance test of the above anisotropic composite membrane material (1) Wetting properties of hydrophilic PAN-SiO2 nanofiber membrane The purpose of doping SiO2 NPs in the PAN matrix is ​​to enhance the hydrophilicity of PAN fibers. In order to further characterize the dynamic wetting properties of the fiber membrane, 2 μL of droplets were dropped on the surface of the PAN fiber membrane and the PAN-SiO2 fiber membrane, and the time it took for the droplets to completely penetrate the PAN fiber membrane and the PAN-SiO2 fiber membrane was recorded. Fig.15 It can be seen that when a 2 μL droplet is dropped on the PAN fiber membrane, it takes about 9 s for the droplet to completely soak into the PAN fiber membrane; and when a 2 μL droplet is dropped on the surface of the PAN-SiO2 fiber membrane, it only takes about 0.5 s for the droplet to completely soak into the PAN-SiO2 fiber membrane; thus, it can be seen that the doping of SiO2NPs effectively improves the hydrophilicity of the PAN-SiO2 fiber membrane.

[0039] (2) Sweat transmission performance like Fig.16 As shown in the figure, the sample was fixed flat on a glass slide, and a high-speed camera (Olympus, I-speedthree series) was used to record the dynamic transfer process of the droplet at a recording frequency of 100 fps. A 7 μL droplet was dropped on the Cu NWs side of the composite structure membrane using a syringe pump. When the droplet contacted the hydrophilic PAN-SiO2 fiber array, it was quickly transferred to the hydrophilic PAN-SiO2 nanofiber membrane side within 24 s under the action of hydrophilic capillary force and Laplace force.

[0040] (3) Outdoor radiant cooling performance The reflectance spectra of traditional cotton fabric, pure PAN nanofiber membrane and PAN-SiO2 nanofiber membrane in the 0.3-2.5 μm band were measured using a UV-visible-near infrared spectrometer with an integrating sphere. Fig.17As shown in the figure, the reflectivity of PAN-SiO2 nanofiber membrane is 0.93, which is very close to the reflectivity of pure PAN nanofiber membrane 0.91, but significantly higher than the reflectivity of traditional cotton fabric 0.61. According to Mie scattering theory, nanofibers with diameters ranging from 500 nm to 1.2 μm have a strong scattering effect on solar radiation, and the prior art has a theory showing that a porous structure with multi-scale pores of 500 nm to 3 μm can strongly scatter solar radiation. Therefore, compared with traditional cotton fabrics, the PAN-SiO2 nanofiber membrane in the present invention has a significant advantage in scattering solar radiation.

[0041] In order to study the emissivity of one side of the composite membrane PVDF-HFP / PAN-SiO2 of the present invention, a Fourier transform infrared spectrometer (FTIR) equipped with a gold-plated integrating sphere was used to measure the MIR emissivity spectra of PVDF-HFP / PAN-SiO2, PVDF-HFP / PAN composite fiber membranes and traditional cotton fabrics. Fig.18 As shown, the weighted average emissivity of the composite membrane PVDF-HFP / PAN-SiO2 of the present invention in the 7-14 μm band of human body radiation is 0.88, which is slightly higher than the average emissivity of PVDF-HFP / PAN composite fiber membrane 0.86, but slightly lower than the average emissivity of cotton fabric 0.92.

[0042] In order to study the outdoor radiation heat dissipation performance of the composite film of the present invention, a silica gel heater (100 W / m 2 ) to simulate human skin. First, in order to prevent the artificial skin from losing heat through heat conduction and thus affecting the accuracy of the experimental results, the artificial skin was placed on insulating foam; secondly, in order to prevent the foam from absorbing sunlight and affecting the experimental results, the remaining foam position was covered with aluminum foil. The composite film with the PAN-SiO2 side facing outward, the composite film with the pure PAN fiber membrane side facing outward, and the traditional cotton fabric were respectively covered on the artificial skin and exposed to the sun; then, a paperless recorder and a solar irradiation recorder were used to record in real time the changes in solar power and the changes in the surface temperature of the artificial skin from 9:30 to 12:30 in the morning. Fig.19 , Fig. 20As shown, with the increase of solar radiation energy and exposure time, the temperature of artificial skin covered with different fabrics shows a gradual upward trend as a whole. Due to the factor of outdoor air convection, the temperature of artificial skin fluctuates up and down. It can be seen that the average temperature of the artificial skin surface covered by the composite film containing SiO2 is 36.7°C, which is similar to the temperature of 37.1°C of artificial skin covered by pure PAN fiber composite film, but is significantly lower than the temperature of 43.1°C of artificial skin covered by white cotton fabric and 46.8°C of exposed artificial skin. This is because the PVDF-HFP / PAN-SiO2 side of the composite membrane of the present invention has a higher MIR emissivity of 0.88. While not hindering the artificial skin from radiating heat outward, the PAN-SiO2 fiber layer can reflect solar radiation, thereby minimizing the absorption of solar radiation. Therefore, when the PAN-SiO2 side of the composite membrane of the present invention faces outward, the composite membrane has excellent outdoor radiation heat dissipation performance.

[0043] (4) Radiant thermal insulation performance of composite film In an indoor environment without direct sunlight, more than 50% of the heat generated by the human body is dissipated through radiation MIR. Therefore, by adjusting the thermal radiation characteristics of the fabric, the MIR radiation can be controlled to make it have the function of MIR heating or heat dissipation. In order to study the radiation thermal insulation performance of the composite film, Fig.21 As shown in the figure, the MIR emissivity spectrum of the Cu NWs side of the composite film was measured by a Fourier transform infrared spectrometer (FTIR) equipped with a gold-plated integrating sphere, where emissivity (ε) = 1-reflectivity (γ)-transmittance (τ). For traditional cotton fabrics, it contains a large number of functional groups such as -NCO, NC=O, COC, etc. These functional groups have strong infrared absorption capabilities in the MIR radiation wavelength range of 7-14 μm, so that the weighted average emissivity of cotton fabrics in the 7-14 μm band is 0.92, which is significantly higher than the average emissivity of metal copper Cu NWs 0.33. Therefore, when the human body wears cotton fabrics, cotton fabrics will emit a lot of heat in the form of thermal radiation; for the composite film, due to the through-hole array formed by laser punching, the MIR emissivity of the Cu NWs side of the composite film is 0.35, which is close to the average emissivity of metal copper Cu NWs 0.33, and is much lower than the weighted average emissivity of cotton fabrics 0.92. Therefore, when the low-emissivity Cu NWs side faces outward, the composite film can effectively suppress the thermal radiation of the human body and achieve the purpose of keeping warm.

[0044] Finally, the artificial skin (100 W / m 2 ) was placed on the foam, and then the fabric was covered on the artificial skin. The temperature changes of the artificial skin were recorded in real time within 60 minutes using a thermocouple and a paperless recorder, and a temperature value was read every second. Fig. 22 , Fig.23 As shown in the figure, the arithmetic mean of the temperature change in the time period of 30 to 60 minutes is taken as a reference to study the thermal insulation performance of different fabrics. When the indoor ambient temperature is about 26.4°C, the average temperature of the artificial skin not covered with any fabric is 35.6°C, while the average temperatures of the artificial skin covered with cotton fabric, the composite membrane of the present invention with the Cu NWs side facing outward, and the composite membrane without hydrophilic fiber channels rise to 36.5°C, 38.5°C, and 39.0°C, respectively. Therefore, it is shown that the composite membrane of the present invention has excellent radiant thermal insulation performance.

[0045] Example 2 A method for preparing an anisotropic composite film material comprises the following specific steps: S11, preparation of hydrophobic nanofiber membrane: 7 parts by weight of polyurethane (PU) were put into 93 parts by weight of acetone and stirred at room temperature for 10 hours until uniformly dispersed to obtain a PU solution with a mass fraction of 7%; the PU solution was loaded into a syringe and fixed on an electrospinning machine for electrospinning, and a roller with tin foil was used to receive the fiber sample to obtain a hydrophobic PU nanofiber membrane with a thickness of 100 μm. The fiber surface was smooth and the contact angle of the fiber membrane was 130°; the process parameters of the electrospinning technology were: tin foil was used as the receiving substrate, the roller diameter was 14 cm, the roller speed was 260 r / min, the receiving distance was 16 cm, the propulsion speed was 0.7 mL / h, the voltage was 12 kV, and the spinning time was 70 min; S12, coating metal nanowire layer: A n-hexane solution of silver nanowires (Ag NWs) with a mass fraction of 97% is selected and diluted with anhydrous ethanol to a silver nanowire dispersion with a mass fraction of 3.5%; the diluted silver nanowire dispersion is then coated on the hydrophobic PU nanofiber membrane in step S11 by vacuum filtration technology, the vacuum degree is -7 kPa, and a layer of silver nanowires with a thickness of 25 μm is coated to obtain a hydrophobic PU nanofiber membrane / Ag NWs composite structure membrane; the contact angle of water on the silver nanowire layer side of the hydrophobic PU nanofiber membrane / Ag NWs composite structure membrane is 148.2°; S13, constructing a through hole array: The laser punching technology is used to punch holes on the hydrophobic PU nanofiber membrane / Ag NWs composite structure membrane to form a through-hole array penetrating the composite structure membrane, wherein the through-hole size is 130 μm and the through-hole spacing is 0.7 mm; the laser punching power is 20 W and the punching time is 0.60 s; S14, constructing a hydrophilic fiber channel array: First, 2 parts by weight of SiO2 nanoparticles (SiO2NPs) were added to 85 parts by weight of N, N-dimethylformamide (DMF) and ultrasonically treated at 250 W for 2 h to uniformly disperse the SiO2NPs to obtain a SiO2 / DMF dispersion. Then, 13 parts by weight of cellulose acetate (CA) was added to the uniform SiO2 / DMF dispersion and stirred at room temperature for 20 h to fully dissolve the CA to obtain a suspension containing 2% by weight of SiO2NPs and 13% by weight of CA. The prepared suspension was electrospun at a propulsion rate of 0.7 mL / h at an operating voltage of 18 kV and a receiving distance of 20 cm to obtain CA-SiO2 fibers. Next, the CA-SiO2 fibers were cut, deionized water was added, and a Quhor EA300-T emulsifier homogenizer was used to shear the fibers at a speed of 8000 r / min for 0.8 h to uniformly disperse the fibers to obtain a CA-SiO2 fiber with a mass concentration of 0.007. g / mL of hydrophilic CA-SiO2 fiber dispersion; finally, the Ag NWs side of the hydrophobic PU nanofiber membrane / Ag NWs composite structure membrane containing a through-hole array was placed on a sand core, and the CA-SiO2 dispersion was filtered by vacuum filtration with a vacuum degree of -7 kPa, and a CA-SiO2 fiber channel array was obtained in the through-hole array of the hydrophobic PU nanofiber membrane / Ag NWs composite structure membrane, and one end of the CA-SiO2 fiber channel array protruded 3 μm from the Ag NWs side, forming a layer of short fiber membrane on one side of the hydrophobic PU nanofiber membrane; S15. Laminating hydrophilic nanofiber membrane: On one side of the PU nanofiber membrane of the hydrophobic PU nanofiber membrane / Ag NWs composite structure membrane in step S14, electrospinning is performed at a propulsion rate of 0.7 mL / h at a working voltage of 20 kV and a receiving distance of 19 cm to spin a layer of hydrophilic CA-SiO2 fiber membrane with a thickness of 100 μm. The contact angle of the fiber membrane is 0°, thereby preparing an anisotropic composite membrane material.

[0046] Performance test of the above anisotropic composite membrane material (1) Wetting properties of hydrophilic CA-SiO2 fiber membrane The purpose of doping SiO2 NPs in the CA matrix is ​​to enhance the hydrophilicity of CA fibers. In order to further characterize the dynamic wetting properties of the fiber membrane, 2 μL of droplets were dropped on the surface of the CA fiber membrane and the CA-SiO2 fiber membrane, and the time for the droplets to completely penetrate the CA fiber membrane and the CA-SiO2 fiber membrane was recorded. When a 2 μL droplet was dropped on the CA fiber membrane, it took about 10 s for the droplet to completely infiltrate the CA fiber membrane; and when a 2 μL droplet was dropped on the surface of the CA-SiO2 fiber membrane, it only took about 1.5 s for the droplet to completely infiltrate the CA-SiO2 fiber membrane; thus, it was known that the doping of SiO2 NPs effectively improved the hydrophilicity of the CA-SiO2 fiber membrane.

[0047] (2) Sweat transmission performance The sample was fixed flat on a glass slide, and a high-speed camera (Olympus, I-speed threeseries) was used to record the dynamic transfer process of the droplet at a recording frequency of 100 fps. A 7 μL droplet was dropped on the Ag NWs side of the composite structure membrane using a syringe pump. When the droplet contacted the hydrophilic CA-SiO2 fiber array, the droplet was quickly transferred to the hydrophilic CA-SiO2 fiber membrane side within 23 s under the action of hydrophilic capillary force and Laplace force.

[0048] (3) Outdoor radiant cooling performance The reflectance spectra of traditional cotton fabric, pure CA nanofiber membrane and CA-SiO2 nanofiber membrane in the 0.3-2.5 μm band were measured by UV-visible-near infrared spectrometer with integrating sphere. The reflectance of CA-SiO2 nanofiber membrane is 0.95, which is very close to the reflectance of pure CA nanofiber membrane 0.93, but significantly higher than the reflectance of traditional cotton fabric 0.61. Therefore, compared with traditional cotton fabric, the CA-SiO2 nanofiber membrane in the present invention has obvious advantages in scattering solar radiation.

[0049] In order to study the emissivity of one side of the composite membrane PU / CA-SiO2 of the present invention, a Fourier transform infrared spectrometer (FTIR) equipped with a gold-plated integrating sphere was used to measure the MIR emissivity spectra of PU / CA-SiO2, PU / CA composite fiber membrane and traditional cotton fabric. The weighted average emissivity of the composite membrane PU / CA-SiO2 of the present invention in the 7-14 μm band of human body radiation is 0.91, which is slightly higher than the average emissivity of the PU / CA composite fiber membrane of 0.90, but slightly lower than the average emissivity of cotton fabric of 0.92.

[0050] In order to study the outdoor radiation heat dissipation performance of the composite film of the present invention, a silica gel heater (100 W / m 2) to simulate human skin. First, in order to prevent the artificial skin from losing heat through heat conduction and thus affecting the accuracy of the experimental results, the artificial skin was placed on the insulating foam; secondly, in order to prevent the foam from absorbing sunlight and affecting the experimental results, the remaining position of the foam was covered with aluminum foil. The composite film with the CA-SiO2 side facing outward, the composite film with the pure CA fiber membrane side facing outward, and the traditional cotton fabric were respectively covered on the artificial skin and exposed to the sun; then, the changes in solar power and surface temperature of the artificial skin in the time period of 9:30 to 12:30 in the morning were recorded in real time using a paperless recorder and a solar irradiation recorder. With the increase of solar radiation energy and exposure time, the temperature of the artificial skin covered with different fabrics showed a gradual upward trend as a whole. Due to the factors of outdoor air convection, the temperature of the artificial skin fluctuated up and down. It can be seen that the average temperature of the artificial skin surface covered by the composite film containing SiO2 is 36.4°C, which is similar to the temperature of 37.1°C of the artificial skin covered by the pure CA fiber composite film, but significantly lower than the temperature of 42.9°C of the artificial skin covered by white cotton fabric and 46.8°C of the exposed artificial skin. This is because the PU / CA-SiO2 side of the composite film of the present invention has a higher MIR emissivity of 0.91. While not hindering the artificial skin from radiating heat outward, the CA-SiO2 fiber layer can reflect solar radiation, thereby minimizing the solar radiation absorption. Therefore, when the CA-SiO2 side of the composite film of the present invention faces outward, the composite film has excellent outdoor radiation heat dissipation performance.

[0051] (4) Radiant thermal insulation performance of composite film In an indoor environment without direct sunlight, more than 50% of the heat generated by the human body is dissipated through radiation MIR. Therefore, by adjusting the thermal radiation characteristics of the fabric, the MIR radiation can be controlled to make it have the function of MIR heating or heat dissipation. In order to study the radiative thermal insulation performance of the composite film, a Fourier transform infrared spectrometer (FTIR) equipped with a gold-plated integrating sphere was used to measure the MIR emissivity spectrum of the Ag NWs side of the composite film, where emissivity (ε) = 1-reflectivity (γ)-transmittance (τ). For traditional cotton fabrics, it contains a large number of functional groups such as -NCO, NC=O, COC, etc. These functional groups have strong infrared absorption ability in the MIR radiation wavelength range of 7 to 14 μm, so that the weighted average emissivity of cotton fabrics in the 7 to 14 μm band is 0.92, which is significantly higher than the average emissivity of Ag NWs 0.31. Therefore, when the human body wears cotton fabrics, the cotton fabrics will emit a large amount of heat in the form of thermal radiation; for the composite film, due to the through-hole array formed by laser punching, the MIR emissivity of 0.33 on the Ag NWs side of the composite film of the present invention is close to the average emissivity of Ag NWs 0.31, which is much lower than the weighted average emissivity of cotton fabrics 0.92. Therefore, when the low-emissivity Ag NWs side faces the outside, the composite film of the present invention can effectively suppress the thermal radiation of the human body to achieve the purpose of keeping warm.

[0052] Finally, the artificial skin (100 W / m 2 ) was placed on the foam, and then the fabric was covered on the artificial skin, and the temperature change of the artificial skin within 60 minutes was recorded in real time with a thermocouple and a paperless recorder, and a temperature value was read every second. The arithmetic mean of the temperature change in the time period of 30 to 60 minutes was taken as a reference to study the thermal insulation performance of different fabrics. When the indoor ambient temperature was about 26.4°C, the average temperature of the artificial skin not covered with any fabric was 34.3°C, while the average temperature of the artificial skin covered with cotton fabric, the composite membrane of the present invention with the Ag NWs side facing the outside, and the composite membrane without hydrophilic fiber channels rose to 36.2°C, 38.7°C and 39.2°C, respectively. Therefore, it is shown that the composite membrane of the present invention has excellent radiant thermal insulation performance.

[0053] Example 3 A method for preparing an anisotropic composite film material comprises the following specific steps: S11, preparation of hydrophobic nanofiber membrane: 15 parts by weight of polyvinylidene fluoride (PVDF) were placed in 85 parts by weight of a solvent, wherein the solvent was a mixed solvent of analytically pure N,N-dimethylformamide and acetone in a mass ratio of 4:5, and stirred at room temperature for 12 hours until uniformly dispersed to obtain a PVDF solution with a mass fraction of 15%; the PVDF solution was loaded into a syringe and fixed on an electrospinning machine for electrospinning, and a roller covered with tin foil was used to receive the fiber sample to obtain a hydrophobic PVDF nanofiber membrane with a thickness of 120 μm, a smooth fiber surface, and a contact angle of the fiber membrane of 140.1°; the process parameters of the electrospinning technology were: tin foil was used as the receiving substrate, the roller diameter was 14 cm, the roller speed was 300 r / min, the receiving distance was 13 cm, the propulsion speed was 1.0 mL / h, the voltage was 17 kV, and the spinning time was 80 min; S12, coating metal nanowire layer: A n-hexane solution of nickel nanowires with a mass fraction of 97% produced by Shanghai Aladdin Biochemical Technology Co., Ltd. was selected and diluted with anhydrous ethanol to a nickel nanowire dispersion with a mass fraction of 4.5%; the diluted nickel nanowire dispersion was then coated on the hydrophobic PVDF nanofiber membrane in step S11 by vacuum filtration technology, with a vacuum degree of -6 kPa, and a nickel nanowire layer with a thickness of 25 μm was coated to obtain a hydrophobic PVDF nanofiber membrane / nickel nanowire layer (Ni NWs) composite structure membrane; the contact angle of water on the nickel nanowire layer side of the hydrophobic PVDF nanofiber membrane / Ni NWs composite structure membrane was 148.1°; S13, constructing a through hole array: Laser punching technology is used to etch a through-hole array penetrating the hydrophobic PVDF nanofiber membrane / Ni NWs composite structure membrane, wherein the through-hole size is 150 μm and the through-hole spacing is 0.9 mm. The power of the laser punching is 30 W and the punching time is 0.80 s. S14, constructing a hydrophilic fiber channel array: Firstly, 3 parts by weight of ZnO nanoparticles (ZnO NPs) were added to 85 parts by weight of m-cresol and ultrasonically treated at 300 W for 2 h to uniformly disperse the ZnO NPs to obtain a ZnO / m-cresol dispersion. Then, 12 parts by weight of nylon 66 were added to the uniform ZnO / m-cresol dispersion and stirred at room temperature for 24 h to fully dissolve the mixture to obtain a suspension containing 6% by weight of ZnO NPs and 12% by weight of nylon 66. The prepared suspension was electrospun at a propulsion rate of 0.9 mL / h at a working voltage of 15 kV and a receiving distance of 13 cm to obtain nylon 66-ZnO fibers. Next, the nylon 66-ZnO fibers were cut, deionized water was added, and a Quhor EA300-T emulsifier homogenizer was used to shear the fibers at a speed of 6000 r / min for 1 h to uniformly disperse the fibers to obtain a nylon 66-ZnO fiber with a mass concentration of 0.01. g / mL of hydrophilic nylon 66-ZnO fiber dispersion; finally, the Ni NWs side of the hydrophobic PVDF nanofiber membrane / Ni NWs composite structure membrane containing a through-hole array was placed on the sand core; the nylon 66-ZnO dispersion was filtered by vacuum filtration with a vacuum degree of -10 kPa, and a nylon 66-ZnO fiber channel array was obtained in the through-hole array of the hydrophobic PVDF nanofiber membrane / NiNWs composite structure membrane, and one end of the nylon 66-ZnO fiber channel array protruded 8 μm from the Ni NWs side, forming a layer of short fiber membrane on one side of the hydrophobic PVDF nanofiber membrane; S15. Laminating hydrophilic nanofiber membrane: On one side of the PVDF nanofiber membrane of the hydrophobic PVDF nanofiber membrane / Ni NWs composite structure membrane in step S14, electrospinning is performed at a propulsion rate of 1.0 mL / h at an operating voltage of 17 kV and a receiving distance of 13 cm to spin a layer of hydrophilic nylon 66-ZnO fiber membrane with a thickness of 100 μm. The contact angle of the fiber membrane is 0°, thereby preparing an anisotropic composite membrane material.

[0054] Performance test of the above anisotropic composite membrane material (1) Wetting properties of hydrophilic nylon 66-ZnO fiber membrane The purpose of doping ZnO NPs in the nylon 66 matrix is ​​to enhance the hydrophilicity of nylon 66 fiber. In order to further characterize the dynamic wetting properties of the fiber membrane, 2 μL of droplets were dropped on the surface of nylon 66 fiber membrane and nylon 66-SiO2 fiber membrane, and the time for the droplets to completely penetrate the nylon 66 fiber membrane and nylon 66-ZnO fiber membrane was recorded. When 2 μL of droplets were dropped on the nylon 66 fiber membrane, the droplets completely infiltrated the nylon 66 fiber membrane after about 12 s; and when 2 μL of droplets were dropped on the surface of nylon 66-ZnO fiber membrane, the droplets only took about 2 s to completely infiltrate the nylon 66-ZnO fiber membrane; thus, it was known that the doping of ZnO NPs effectively improved the hydrophilicity of nylon 66-ZnO fiber membrane.

[0055] (2) Sweat transmission performance The sample was fixed flat on a glass slide, and a high-speed camera (Olympus, I-speed threeseries) was used to record the dynamic transfer process of the droplet at a recording frequency of 100fps. A 7μL droplet was dropped on the Ni NWs side of the composite structure membrane using a syringe pump. When the droplet contacted the hydrophilic nylon 66-ZnO fiber array, it was quickly transferred to the hydrophilic nylon 66-ZnO fiber membrane side within 22 s under the action of hydrophilic capillary force and Laplace force.

[0056] (3) Outdoor radiant cooling performance The reflectance spectra of traditional cotton fabric, pure nylon 66 nanofiber membrane and nylon 66-ZnO nanofiber membrane in the 0.3-2.5 μm band were measured by using an ultraviolet-visible-near infrared spectrometer with an integrating sphere. The reflectance of nylon 66-ZnO nanofiber membrane is 0.91, which is very close to the reflectance of pure nylon 66 nanofiber membrane 0.90, but significantly higher than the reflectance of traditional cotton fabric 0.61. Therefore, compared with traditional cotton fabric, the hydrophilic nylon 66-ZnO fiber membrane in the present invention has obvious advantages in scattering solar radiation.

[0057] In order to study the emissivity of one side of the composite membrane PVDF / nylon 66-ZnO of the present invention, a Fourier transform infrared spectrometer (FTIR) equipped with a gold-plated integrating sphere was used to measure the MIR emissivity spectra of PVDF / nylon 66-ZnO, PVDF / nylon 66 composite fiber membranes and traditional cotton fabrics. The weighted average emissivity of the composite membrane PVDF / nylon 66-ZnO of the present invention in the 7-14 μm band of human body radiation is 0.90, which is slightly higher than the average emissivity of the PVDF / nylon 66 composite fiber membrane of 0.89, but slightly lower than the average emissivity of the cotton fabric of 0.92.

[0058] In order to study the outdoor radiation heat dissipation performance of the composite film of the present invention, a silica gel heater (100 W / m2 ) to simulate human skin. First, in order to prevent the artificial skin from losing heat through heat conduction and thus affecting the accuracy of the experimental results, the artificial skin was placed on the thermal insulation foam; secondly, in order to prevent the foam from absorbing sunlight and affecting the experimental results, the remaining position of the foam was covered with aluminum foil. The composite film with the nylon 66-ZnO side facing outward, the composite film with the pure nylon 66 fiber membrane side facing outward, and the traditional cotton fabric were respectively covered on the artificial skin and exposed to the sun; then, the changes in solar power and surface temperature of the artificial skin in the time period of 9:30 to 12:30 in the morning were recorded in real time using a paperless recorder and a solar irradiation recorder. With the increase of solar radiation energy and exposure time, the temperature of the artificial skin covered with different fabrics showed a gradual upward trend as a whole. Due to the factors of outdoor air convection, the temperature of the artificial skin fluctuated up and down. It can be seen that the average temperature of the surface of the artificial skin covered by the composite film containing ZnO is 36.5°C, which is similar to the temperature of 37.0°C of the artificial skin covered by the pure nylon 66 fiber composite film, but significantly lower than the temperature of 43.1°C of the artificial skin covered by white cotton fabric and 46.8°C of the exposed artificial skin. This is because the PVDF / nylon 66-ZnO side of the composite film of the present invention has a higher MIR emissivity of 0.90. While not hindering the artificial skin from radiating heat outward, the nylon 66-ZnO fiber layer can reflect solar radiation, thereby minimizing the solar radiation absorption. Therefore, when the nylon 66-ZnO side of the composite film of the present invention faces outward, the composite film has excellent outdoor radiation heat dissipation performance.

[0059] (4) Radiant thermal insulation performance of composite film In an indoor environment without direct sunlight, more than 50% of the heat generated by the human body is dissipated through radiation MIR. Therefore, by adjusting the thermal radiation characteristics of the fabric, the MIR radiation can be controlled to have the function of MIR heating or heat dissipation. In order to study the radiative thermal insulation performance of the composite film, a Fourier transform infrared spectrometer (FTIR) equipped with a gold-plated integrating sphere was used to measure the MIR emissivity spectrum of the Ni NWs side of the composite film, where emissivity (ε) = 1-reflectivity (γ)-transmittance (τ). For traditional cotton fabrics, it contains a large number of functional groups such as -NCO, NC=O, COC, etc. These functional groups have strong infrared absorption ability in the MIR radiation wavelength range of 7-14 μm, so that the weighted average emissivity of cotton fabrics in the 7-14 μm band is 0.92, which is significantly higher than the average emissivity of Ni NWs 0.35. Therefore, when the human body wears cotton fabrics, the cotton fabrics will emit a lot of heat in the form of thermal radiation; for the composite film, due to the through-hole array caused by laser punching, the MIR emissivity of 0.37 on the Ni NWs side of the composite film is close to the average emissivity of 0.35 of metal Ni NWs, which is much lower than the weighted average emissivity of 0.92 of cotton fabrics. Therefore, when the low-emissivity Ni NWs side faces the outside, the composite film of the present invention can effectively suppress the thermal radiation of the human body to achieve the purpose of keeping warm.

[0060] Finally, the artificial skin (100 W / m 2 ) was placed on the foam, and then the fabric was covered on the artificial skin, and the temperature change of the artificial skin within 60 minutes was recorded in real time with a thermocouple and a paperless recorder, and a temperature value was read every second. The arithmetic mean of the temperature change in the time period of 30 to 60 minutes was taken as a reference to study the thermal insulation performance of different fabrics. When the indoor ambient temperature was about 26.4°C, the average temperature of the artificial skin not covered with any fabric was 34.3°C, while the average temperature of the artificial skin covered with cotton fabric, the composite membrane of the present invention with one side of Ni NWs facing outward, and the composite membrane without hydrophilic fiber channels rose to 36.2°C, 38.2°C, and 38.8°C, respectively. Therefore, it is shown that the composite membrane of the present invention has excellent radiant thermal insulation performance.

[0061] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing an anisotropic composite membrane material, characterized in that: It includes the following steps: S1. Preparation of hydrophobic nanofiber membrane: preparing a hydrophobic nanofiber membrane with a thickness of 80 μm to 120 μm by electrospinning technology; S2, coating a metal nanowire layer: coating a metal nanowire layer with a thickness of 10 μm to 30 μm on the nanofiber membrane in step S1 by vacuum filtration technology to obtain a hydrophobic nanofiber membrane / metal nanowire layer composite structure membrane; S3, constructing a through hole array: using laser punching technology to punch holes in the hydrophobic nanofiber membrane / metal nanowire layer composite structure membrane in step S2 to form a through hole array that penetrates the composite structure membrane; S4, constructing a hydrophilic fiber channel array: using a suction filtration technique to filter the hydrophilic short fiber dispersion from one side of the nanofiber membrane to the side of the hydrophobic metal nanowire layer through the through-hole array in step S3, and obtaining a hydrophilic fiber channel array in the through-hole array; the preparation method of the hydrophilic fiber channel array is as follows: S4.1, adding the nanoparticles to an organic solvent and subjecting the solvent to ultrasonic treatment for 1 to 3 h to uniformly disperse the nanoparticles to obtain a nanoparticle dispersion; S4.2, adding a hydrophilic polymer to the nanoparticle dispersion in step S4.1, stirring at room temperature for 12 to 24 hours to fully dissolve, and obtaining a suspension containing 2.0 to 3.9% by mass of nanoparticles and 10 to 20% by mass of the hydrophilic polymer; S4.3, electrospinning the suspension in step S4.2 to obtain hydrophilic polymer-nanoparticle fibers; S4.4, cutting the hydrophilic polymer-nanoparticle fibers in step S4.3, adding deionized water, performing shear treatment, and dispersing them evenly to obtain a hydrophilic fiber dispersion with a mass concentration of 0.005 to 0.01 g / mL; S4.5, filtering the hydrophilic fiber dispersion in step S4.4 by vacuum filtration, with a vacuum degree of -10 to -5 kPa, to obtain a hydrophilic polymer-nanoparticle fiber channel array in the through-hole array on the hydrophobic nanofiber membrane / metal nanowire layer composite structure membrane; S5. Laminating hydrophilic nanofiber membrane: using electrospinning technology to spin a layer of hydrophilic nanofiber membrane with a thickness of 80 to 120 μm on one side of the nanofiber membrane of the hydrophobic nanofiber membrane / metal nanowire layer composite structure membrane in step S4, to prepare an anisotropic composite membrane material.

2. The method for preparing anisotropic composite membrane material according to claim 1, characterized in that: In step S1, the preparation method of the hydrophobic nanofiber membrane is as follows: dissolving a polymer in a solvent and stirring evenly to obtain a polymer solution with a mass fraction of 6 to 15%; loading the polymer solution into a syringe, fixing it on an electrospinning machine for electrospinning, and using a roller with tin foil attached to receive the fiber sample to obtain a hydrophobic nanofiber membrane; the process parameters of the electrospinning technology are as follows: using tin foil as a receiving substrate, a roller diameter of 13 to 20 cm, a roller speed of 150 to 350 r / min, a receiving distance of 15 to 25 cm, a propulsion speed of 0.5 to 1.0 mL / h, a voltage of 15 to 25 kV, and a spinning time of 60 to 90 min; the solvent is one of acetone, N,N-dimethylformamide, N,N-dimethylacetamide, and tetrahydrofuran, or a mixture of two of them; the polymer is one of polyvinylidene fluoride-hexafluoropropylene, polyurethane, and polyvinylidene fluoride.

3. The method for preparing anisotropic composite membrane material according to claim 1 or 2, characterized in that: In step S1, the pores of the nanofiber membrane are 0.3 μm to 5.0 μm, the diameter of a single nanofiber is 0.18 μm to 0.9 μm, and the contact angle of the fiber membrane is 130° to 152°.

4. The method for preparing anisotropic composite membrane material according to claim 1, characterized in that: In step S2, a dispersion of metal nanowires having a mass fraction of 90 to 97% is diluted with anhydrous ethanol to obtain a dispersion of metal nanowires having a mass fraction of 2 to 5%; the diluted dispersion of metal nanowires is coated on the nanofiber membrane in step S1 using a vacuum filtration technique, the vacuum degree is -10 to -5 kPa, and the coating thickness is 10 μm to 30 μm, to obtain a hydrophobic nanofiber membrane / metal nanowire layer composite structure membrane.

5. The method for preparing the anisotropic composite membrane material according to claim 1 or 4, characterized in that: In step S2, the diameter of the metal nanowire is 0.08 μm to 0.15 μm, and the length is 30 μm to 50 μm; the metal nanowire is one of copper nanowire, silver nanowire and nickel nanowire.

6. The method for preparing anisotropic composite membrane material according to claim 1, characterized in that: In step S3, the size of each through hole of the through hole array is 100 μm to 200 μm, and the through hole spacing is 0.7 mm to 1.7 mm; the laser punching technology includes: power of 10 to 30 W, and punching time of 0.15 to 1.00 s.

7. The method for preparing anisotropic composite membrane material according to claim 1, characterized in that: It also includes any one or more of the following features: (1) In step S4.1, the particle size of the nanoparticles is 7 to 40 nm, and the mass fraction of the nanoparticles in the nanoparticle dispersion is 2.3 to 4.4%; (2) In step S4.1, the nanoparticles are selected from the group consisting of SiO2 nanoparticles, TiO2 nanoparticles, CeO2 nanoparticles, Al2O3 nanoparticles, and ZnO nanoparticles; (3) In step S4.1, the organic solvent is one of acetone, N,N-dimethylformamide, m-cresol, N,N-dimethylacetamide, and tetrahydrofuran; (4) In step S4.1, the ultrasonic treatment conditions are: power of 200-300 W and time of 1-3 h; (5) In step S4.2, the hydrophilic polymer is one of polyacrylonitrile, cellulose acetate, and nylon 66; (6) In step S4.3, the process parameters of the electrospinning technology are: working voltage of 10-20 kV, receiving distance of 15-25 cm, and propulsion rate of 0.5-1 mL / h; (7) In step S4.5, the hydrophilic fiber channel array protrudes from one side of the metal nanowire layer by 3 μm to 10 μm.

8. The method for preparing anisotropic composite membrane material according to claim 1, characterized in that: In step S5, the method for laminating the hydrophilic nanofiber membrane is as follows: electrospinning one side of the hydrophobic nanofiber membrane of the hydrophobic nanofiber membrane / metal nanowire composite structure membrane containing the hydrophilic fiber channel array in step S4 at a working voltage of 10 to 20 kV and a receiving distance of 15 to 25 cm at a propulsion rate of 0.5 to 1 mL / h to spin a layer of hydrophilic nanofiber membrane.

9. An anisotropic composite membrane material prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The invention discloses a hydrophobic nanofiber membrane / metal nanowire layer composite structure membrane, which comprises a metal nanowire layer, a hydrophobic nanofiber membrane and a hydrophilic nanofiber membrane in order from bottom to top. The hydrophobic nanofiber membrane / metal nanowire layer composite structure membrane composed of the metal nanowire layer and the hydrophobic nanofiber membrane has a through hole array, in which a hydrophilic fiber channel array is arranged. The hydrophilic fiber channel array forms a layer of short fiber membrane on one side of the hydrophobic nanofiber membrane, which is in close contact with the hydrophilic nanofiber membrane. The hydrophobic nanofiber membrane in the hydrophobic nanofiber membrane / metal nanowire composite structure membrane has a thickness of 80 μm to 120 μm, and a thickness of the metal nanowire is 10 μm to 30 μm. The hydrophilic nanofiber membrane has a thickness of 80 μm to 120 μm.

10. Use of an anisotropic composite film material obtained by the preparation method according to any one of claims 1 to 8 or the anisotropic composite film material according to claim 9 in wearable heat and moisture management materials for the human body and medical wound dressings.

Citation Information

Patent Citations

  • Novel 3D bionic skin dressing and preparation method thereof

    CN112190750A

  • Temperature difference power generation device based on solar interface evaporation

    CN112555786A

  • Conductive self-adhesive nanofiber membrane as well as preparation method and application thereof

    CN116289226A

  • Knitted sports socks with high one-way moisture conduction capability and preparation process thereof

    CN117166249A

  • Asymmetric functional fiber membrane as well as preparation method and application thereof

    CN117488480A

Cited By

  • Human body heat and humidity responsive dynamic temperature adjusting fiber membrane and preparation method thereof

    CN120719462A