Anti-static flame-retardant curtain and preparation method thereof

Polyester is solved by using a combination technology of phospho-containing siloxane, fabric surface grafting high-phosphorus-containing substances, amine-based end tannin crosslinking agents and cyclodextrin-embedded phosphorus-containing flame retardant on polyester curtain fabrics The problems of poor flame retardant performance and poor anti-static performance of curtain fabrics achieve long-lasting flame retardant and anti-static effects.

CN118979383AInactive Publication Date: 2024-11-19寿光天和窗饰有限公司
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411472085.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-22
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing polyester curtain fabrics have problems of poor flame retardant performance and poor anti-static performance, especially after washing, the flame retardant performance rapidly decays and makes it difficult to achieve a lasting flame retardant effect.

Method used

Using a combination technology of phospho-containing siloxane, fabric surface grafting high-phosphorus-containing substances, amine-based end tannin crosslinking agent and cyclodextrin-embedded phosphorus-containing flame retardant, the flame retardant coating is applied through dipping, Enhance the flame retardant and anti-static properties of the polyester fiber surface.

Benefits of technology

The long-lasting and excellent flame retardant and anti-static properties of polyester curtains are achieved. The renewal time and smoldering time are guaranteed before and after washing, and the limit oxygen index and charge surface density have also been significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to an anti-static flame-retardant curtain and a preparation method thereof, and belongs to the technical field of textile finishing, and the preparation method of the anti-static flame-retardant curtain comprises the following five steps: preparing phosphorus-containing siloxane, grafting a high phosphorus-containing substance on the surface of a fabric, preparing an amino-terminated tannic acid cross-linking agent aqueous solution, preparing a cyclodextrin-embedded phosphorus-containing flame retardant, and dipping and coating a flame-retardant coating. According to the obtained anti-static flame-retardant curtain, the afterflame time and the smoldering time are both 0 second before washing and after washing for 30 times, the limit oxygen index before washing is 34-34.5, the limit oxygen index after washing for 30 times is 33-34, the charge surface density before washing is 0.3-0.4 [mu] C / m < 2 >, and the charge surface density after washing for 30 times is 0.4-0.5 [mu] C / m < 2 >.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an anti-static and flame-retardant curtain and a preparation method thereof, belonging to the technical field of textile finishing. Background Art

[0002] Curtains are an indispensable part of home decoration. They not only block light and protect privacy, but also add beauty to the interior. With the rapid development of textile materials and related technologies, people have also put forward more functional requirements for curtains, such as flame retardancy, heat insulation, sound insulation, antibacterial, mildew resistance, waterproof, oil resistance, antifouling, dust resistance, antistatic, wear resistance, etc. Among them, flame retardancy is related to the safety of everyone's life and property, especially in high-rise buildings in cities and other public buildings where people gather. These places have high fire risks and strict fire protection requirements, and the requirements for flame retardancy of curtains are naturally more stringent. The fabrics of curtain fabrics include pure cotton, linen, polyester, silk, etc., as well as blends and weaves of these fabrics. Currently, about 70% to 80% or even more than 90% of the curtains sold on the market are made of polyester or polyester-based blends and weaves. Polyester is also called polyester fiber. It has the advantages of high strength, good elasticity, good drape, crisp and wrinkle-resistant, easy to clean, wear-resistant, heat-resistant, good light aging resistance, durable, not easy to fade, and low price. However, polyester also has very significant disadvantages, such as flammability and poor hygroscopicity, and easy to generate static electricity. The limiting oxygen index (LOI) of polyester is only about 21%, which is very easy to burn, and a large amount of thick smoke and molten droplets will be generated under the action of fire, which is easy to cause secondary ignition and even secondary disasters. Therefore, the development of flame-retardant and anti-static polyester curtain fabrics has become a focus of attention in the home textile industry.

[0003] There are many types of flame retardants that can be used for polyester fibers. According to the elements they contain, they can be divided into inorganic non-metallic compound flame retardants such as halogen, phosphorus, and nitrogen, and inorganic metal compound flame retardants. Due to the safety and environmental protection issues of halogen flame retardants, phosphorus and nitrogen flame retardants are mainly used on the market. However, after conventional impregnation and padding of flame retardants, due to the high viscosity of the flame retardant finishing agent, the fabric mainly captures particles by blocking, resulting in a large amount of flame retardant additives attached to the surface of the fabric, which is difficult to enter the interior of the fabric, and the fiber has a weak binding ability. After multiple washings, it will fall off from the surface, affecting its flame retardant effect. In addition, this process will consume a lot of water resources and generate a large amount of printing and dyeing wastewater. Further treatment of printing and dyeing wastewater will increase the production cost of the enterprise, but if it is not handled properly, it will cause serious environmental damage. Based on this, how to obtain a flame-retardant textile with strong binding ability between the flame retardant finishing agent and the textile and not easy to be washed off is a problem that needs to be solved. In addition, existing textiles are also treated with antistatic finishing agents to make the textiles have antistatic properties, but as time goes by, the antistatic properties of the textiles will weaken and the textiles will lose their antistatic properties. Therefore, how to obtain a textile with continuous antistatic properties is also an urgent problem to be solved.

[0004] Chinese patent CN108891109A discloses a novel flame-retardant and environmentally friendly cloth curtain, a novel flame-retardant and environmentally friendly cloth curtain, comprising a curtain cloth body, a base cloth layer, a lining layer and an outer lining surface, the curtain cloth body is composed of a base cloth layer, a lining layer and an outer lining surface from bottom to top, the base cloth layer is provided with dense micropores, the lining layer is woven by warp and weft, and the warp and weft woven together are arranged in a honeycomb shape, and the warp and weft woven together in the honeycomb shape form a plurality of reaction chambers. The novel flame-retardant and environmentally friendly cloth curtain of the present invention uses yarn with flame-retardant and negative oxygen ion releasing functions as the main raw material, thereby effectively improving people's demand for functional curtains, and effectively improving the flame retardancy of cloth curtains and the adsorption of dust and impurities on the premise of ensuring the improvement of people's quality of life. The flame-retardant and environmentally friendly cloth curtains prepared by this patent are mainly based on blended polyester yarns with flame-retardant and negative oxygen ion-releasing functions. This multifunctional polyester yarn requires the addition of flame-retardant monomer components when synthesizing polyester resin. This method of flame-retardant modification from the very starting raw materials is generally costly and difficult to promote and apply on a large scale. In addition, this patent does not solve the static electricity problem of polyester.

[0005] Chinese patent CN115284701A discloses an environmentally friendly, waterproof, flame-retardant, fully blackout curtain fabric and a manufacturing method thereof, comprising the following steps: S1, selecting fabric base fabrics A and B, and performing flame-retardant slurry treatment on both of them respectively through a slurry dipping machine; S2, selecting a flame-retardant TPU black film as a composite film; using a composite device to first uniformly transfer the PUR hot melt adhesive to any side of the composite film through a glue roller; then bonding the glued surface of the composite film and the fabric base fabric A together through the composite roller; finally entering the cooling roller for cooling treatment; S3, placing the composite semi-finished product after the first composite treatment into a constant temperature and humidity room for the first curing treatment, repeating the above-mentioned composite and curing steps, and composite the fabric base fabric B on the other side of the composite film to obtain a composite finished product. The full-blackout curtain fabric prepared by this patent is mainly made of polyester, and its flame retardant performance is mainly achieved by impregnating polyphosphate and attaching a flame retardant TPU black film. These two flame retardant substances do not have any chemical bonding reaction with the polyester material, but are only physically adsorbed. This will cause the above two flame retardant substances to be lost during the curtain washing process, and the flame retardant performance will decay rapidly, making it difficult to obtain long-lasting or semi-long-lasting flame retardant performance. In addition, this patent does not pay attention to the anti-static performance of the curtain fabric.

[0006] From the above, we can see that curtain fabrics mainly made of polyester still have problems such as poor flame retardancy and poor anti-static performance. Therefore, it is of great practical significance to develop a polyester fabric for anti-static and flame-retardant curtains. Summary of the invention

[0007] In view of the deficiencies in the above-mentioned prior art, the present invention provides an anti-static and flame-retardant curtain and a preparation method thereof to achieve the following invention objectives: to prepare a curtain with polyester as the main material and having long-lasting excellent flame retardant and anti-static properties.

[0008] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions: An anti-static flame-retardant curtain and a preparation method thereof, the preparation method of the anti-static flame-retardant curtain comprising five steps of preparing phosphorus-containing siloxane, grafting high-phosphorus-containing substances onto the surface of the fabric, preparing an amino-terminated tannic acid cross-linking agent aqueous solution, preparing a cyclodextrin-embedded phosphorus-containing flame retardant, and dipping and coating a flame-retardant coating; The following are further improvements to the above technical solution: Step 1: Preparation of phosphorus-containing siloxane The reaction kettle was controlled at 0°C with an ice-water bath, and after nitrogen was passed to replace the air in the kettle, diethyl chlorophosphate and tetrahydrofuran were added under nitrogen protection, and the stirring rate was controlled to 400-800 rpm. After the liquid in the kettle was cooled again and kept at a constant temperature of 0°C, triethylamine was added, and then the silane coupling agent solution was added dropwise, and the dropping speed was controlled at 0.1-0.6 g / s. During the dropping process, the temperature in the kettle was controlled to be 0-5°C, and nitrogen protection was maintained. After the dropwise addition was completed, the temperature in the kettle was quickly raised and kept at a constant temperature of 30-40°C. After the reaction was stirred at a constant temperature for 6-11 hours, the liquid obtained by the reaction was transferred to a rotary evaporator for vacuum rotary evaporation. After the tetrahydrofuran was evaporated, the solid obtained was phosphorus-containing siloxane, which was placed in a dry container for storage; In the silane coupling agent solution, the silane coupling agent is one of 3-aminopropyltriethoxysilane, diethylaminomethyltriethoxysilane, and bis[3-(trimethoxysilyl)propyl]ethylenediamine; The silane coupling agent solution comprises a silane coupling agent and tetrahydrofuran, and the mass ratio of the silane coupling agent to the tetrahydrofuran is 75-95:100; The feeding mass ratio of the diethyl chlorophosphate, tetrahydrofuran, triethylamine and silane coupling agent solution is 20-45:90-140:0.5-1.5:10-20.

[0009] Step 2: Graft high phosphorus content substances onto the surface of fabric The polyester curtain fabric is immersed in a sodium hydroxide aqueous solution with a mass concentration of 15-20 g / L, the temperature of the sodium hydroxide aqueous solution is controlled to be 70-80°C, the mass ratio of the polyester curtain fabric to the sodium hydroxide aqueous solution is 1:30-40, and after the immersion treatment for 40-65 minutes, the polyester curtain fabric is washed with water until the washing liquid is neutral, and then placed in a vacuum oven at 40-60°C for drying for 2-5 hours to obtain the alkali-reduced polyester curtain fabric, and then the alkali-reduced polyester curtain fabric is placed in the immersion solution 1 and immersed for 50- 80 minutes, control the liquid squeezing rate to 80-90%, squeeze out the liquid, then put it into the impregnation liquid 2, immerse for 50-80 minutes, control the liquid squeezing rate to 80-90%, squeeze out the liquid, then pre-bake at 80-90°C for 10-20 minutes, and bake at 170-190°C for 2-4 minutes, then wash with hot water twice and wash with water at room temperature once, the hot water washing temperature is controlled at 50-65°C, after washing, put it into a vacuum oven at 50-70°C for drying for 2-5 hours, and obtain a polyester curtain fabric with a surface grafted high-phosphorus-containing substance; The impregnation solution 1 is obtained by mixing and dissolving phosphorus-containing siloxane, organic polysilazane and acetone into a solution, wherein the mass ratio of phosphorus-containing siloxane, organic polysilazane and acetone is 15-40:1-8:60-150; The organopolysilazane is a colorless, transparent to light yellow liquid with a number average molecular weight of 600-1000 g / mol and a viscosity of 5-50 mPa·s at 25°C; The impregnation solution 2 is obtained by mixing and dissolving phytic acid and acetone into a solution, and the mass ratio of phytic acid to acetone is 20-45:100.

[0010] Step 3: Preparation of an aqueous solution of an amino-terminated tannic acid crosslinking agent Put tannic acid and deionized water into the reactor, control the stirring rate at 300-600 rpm, use an ice-water bath to control the temperature of the materials in the reactor at 0°C, and then add SOCl 2 Then, the temperature is rapidly raised and kept constant at 30-40°C. After 3-6 hours of constant temperature stirring, the unreacted SOCl in the kettle is removed by vacuum distillation at 30-40°C. 2 , obtain a chlorinated tannin solution, then prepare an ethylenediamine aqueous solution in advance in another reaction kettle, control the stirring rate to 400-800 rpm, control the temperature in the kettle to 1-8°C, add triethylamine, and then drop the chlorinated tannin solution into the ethylenediamine aqueous solution at a rate of 0.1-0.5 g / sec. After the dropwise addition is completed, continue to stir and react at a constant temperature for 5-9 hours to obtain an amino-terminated tannic acid crosslinking agent aqueous solution; The tannic acid, deionized water, SOCl 2 The feed mass ratio is 10~30:80~130:2~8; The mass ratio of the ethylenediamine aqueous solution, triethylamine and chlorotannin solution is 30-60:2-9:30-70; In the aqueous solution of ethylenediamine, the mass fraction of ethylenediamine is 50-80wt%.

[0011] Step 4: Preparation of cyclodextrin-embedded phosphorus-containing flame retardant Put β-cyclodextrin and deionized water into a reactor, control the stirring rate to 400-900 rpm, raise the temperature and keep the temperature constant to 50-65°C, continue stirring until β-cyclodextrin is completely dissolved, cool the materials in the reactor to 20-30°C, then drop 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide ethanol solution into the reactor at a rate of 0.1-0.6 g / s, continue to stir and react at a constant temperature for 2-4 hours after the addition is complete, put the material into a 0-4°C environment and let it stand for 24-36 hours, then filter it, dry the filtrate in a vacuum oven at 45-65°C for 10-15 hours, and the obtained dry powder is the cyclodextrin-embedded phosphorus-containing flame retardant; The mass ratio of the β-cyclodextrin, deionized water and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide ethanol solution is 30-60:130-230:30-85; The ethanol solution of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, wherein the mass fraction of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide is 20-45wt%.

[0012] Step 5: Dip-coating of flame retardant coating Add a closed anionic waterborne polyurethane dispersion, N, N-bis(2-hydroxyethyl) aminomethylphosphonic acid diethyl ester, zinc hydroxystannate, nano antimony tin oxide powder, cyclodextrin-embedded phosphorus-containing flame retardant, amino-terminated tannic acid crosslinking agent aqueous solution, and deionized water into a dispersion kettle, and vigorously disperse for 3 to 6 hours at 6000 to 9000 rpm to obtain an impregnation coating liquid, and apply the impregnation coating liquid to a polyester curtain fabric with a high phosphorus-containing substance grafted on the surface by a slit coater, and control the wet film thickness of the impregnation coating liquid on both surfaces of the fabric to be 120 to 200 μm, and pre-bake the coated polyester curtain fabric at 50 to 80° C. for 30 to 50 minutes, and then bake at 130 to 160° C. for 2 to 5 minutes to obtain an antistatic flame-retardant curtain; The solid content of the blocked anionic waterborne polyurethane dispersion is 60-65wt%, and the viscosity at 25°C is 100-400mPa·s; The zinc hydroxystannate is a powder with a particle size of 100-1300 nm; The particle size of the nano antimony tin oxide powder is 10-100 nm; The mass ratio of the blocked anionic waterborne polyurethane dispersion, N, N-bis(2-hydroxyethyl)aminomethylphosphonic acid diethyl ester, zinc hydroxystannate, nano antimony tin oxide powder, cyclodextrin-embedded phosphorus-containing flame retardant, amino-terminated tannic acid crosslinking agent aqueous solution, and deionized water is 30-65:2-5:2-6:0.5-1.3:3-9:10-25:30-80.

[0013] Compared with the prior art, the present invention achieves the following beneficial effects: 1. The present invention uses diethyl chlorophosphate and an amino-containing silane coupling agent as raw materials, and under the action of triethylamine acid binding agent, prepares phosphorus-containing siloxane. This phosphorus-containing siloxane has a very high phosphorus content and very excellent flame retardant properties. The siloxane groups carried thereon can react chemically with the active hydrogen in the hydroxyl group and the carboxyl group. By utilizing the above reaction properties, after the polyester fiber surface is subjected to alkali reduction treatment, the polyester polymer chain on the polyester fiber surface will be slightly decomposed to generate carboxyl groups and hydroxyl groups, and the siloxane groups carried by the phosphorus-containing siloxane react chemically with the carboxyl groups and hydroxyl groups on the polyester surface, so that a large amount of phosphorus-containing organic matter is grafted on the polyester fiber surface, thereby making the polyester fiber have very durable flame retardant properties that are very resistant to water washing; 2. In the step of grafting high-phosphorus-containing substances on the surface of the polyester fiber, in addition to the phosphorus-containing siloxane, a highly reactive organic polysilazane is added, and the fiber is impregnated with phytic acid having a particularly high phosphorus content. The Si-NH-Si bond contained in the organic polysilazane is very active and very easy to react with hydroxyl groups and carboxyl hydroxyl groups. In this way, in addition to the phosphorus-containing siloxane reacting with the hydroxyl groups and carboxyl groups on the surface of the polyester fiber, the organic polysilazane will also graft the carboxyl groups and hydroxyl groups on the surface of the polyester fiber. In addition, the Si-NH-Si bond that has not been completely reacted in the organic polysilazane will also react with the carboxyl groups contained in the phytic acid during the impregnation process of the impregnation solution 2, which will further increase the bonding amount of the high-phosphorus-containing substances on the surface of the polyester fiber, thereby giving the polyester fiber very excellent water-resistant and flame-retardant properties; 3. The present invention uses SOCl 2 After the hydroxyl and carboxylhydroxyl groups at the end of tannic acid are chlorinated, they react with ethylenediamine, and the tannic acid ends become amine groups with very high functionality. Amine groups are very easy to catalyze and participate in the curing reaction of waterborne polyurethane. Therefore, in the impregnation coating solution, these high-functionality tannic acids with amine groups at the ends can act as catalysts and crosslinking agents, promoting the curing of closed anionic waterborne polyurethane into a higher density coating and improving the adhesion of the coating to the surface of polyester fibers. Therefore, the amino-terminated tannic acid crosslinker aqueous solution can give the impregnation coating flame-retardant coating good water-resistant and durable flame retardant and antistatic properties; 4. The cyclodextrin-embedded phosphorus-containing flame retardant prepared by the present invention, firstly, utilizes the water solubility of cyclodextrin and the inclusion effect of cyclodextrin on 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide to uniformly disperse the water-insoluble 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide flame retardant into the aqueous dipping coating liquid, so that the cured coating has very excellent flame retardancy. Secondly, the molecular structure of cyclodextrin itself contains a lot of hydroxyl groups, and it is a multifunctional cross-linking agent for preparing polyurethane coatings. Therefore, it has a similar effect to the amino-terminated tannic acid cross-linking agent, and can also give the dip-coated flame-retardant coating good water-resistant and durable flame retardant and antistatic properties; 5. The anti-static flame-retardant curtains obtained by the present invention have an afterflaming time and a smoldering time of 0 seconds before washing and after washing 30 times, a limiting oxygen index of 34-34.5 before washing and 33-34 after washing 30 times, and a charge surface density of 0.3-0.4 μC / m before washing. 2 , 0.4~0.5μC / m after washing 30 times 2 . DETAILED DESCRIPTION

[0014] The preferred embodiments of the present invention are described below. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0015] Example 1: A method for preparing an anti-static flame-retardant curtain Step 1: Preparation of phosphorus-containing siloxane The reaction kettle was controlled at 0°C with an ice-water bath, and after nitrogen was passed to replace the air in the kettle, diethyl chlorophosphate and tetrahydrofuran were added under nitrogen protection, and the stirring rate was controlled to 650 rpm. After the liquid in the kettle was cooled again and kept at a constant temperature of 0°C, triethylamine was added, and then the silane coupling agent solution was added dropwise, and the dropping speed was controlled at 0.5 g / s. During the dropping process, the temperature in the kettle was controlled to be 1°C, and nitrogen protection was maintained. After the dropwise addition was completed, the temperature in the kettle was quickly raised and kept at a constant temperature of 33°C. After the reaction was stirred at a constant temperature for 9 hours, the liquid obtained by the reaction was transferred to a rotary evaporator for vacuum rotary evaporation. After the tetrahydrofuran was evaporated, the solid obtained was phosphorus-containing siloxane, which was placed in a dry container for storage; In the silane coupling agent solution, the silane coupling agent is 3-aminopropyltriethoxysilane; The silane coupling agent solution comprises a silane coupling agent and tetrahydrofuran, and the mass ratio of the silane coupling agent to the tetrahydrofuran is 90:100; The feed mass ratio of diethyl chlorophosphate, tetrahydrofuran, triethylamine and silane coupling agent solution is 35:110:1:17.

[0016] Step 2: Graft high phosphorus content substances onto the surface of fabric The polyester curtain fabric is immersed in a sodium hydroxide aqueous solution with a mass concentration of 18g / L, the temperature of the sodium hydroxide aqueous solution is controlled to be 77°C, the mass ratio of the polyester curtain fabric to the sodium hydroxide aqueous solution is 1:37, after the immersion treatment for 50 minutes, the polyester curtain fabric is washed with water until the washing liquid is neutral, and then placed in a 45°C vacuum oven for drying for 3 hours to obtain the polyester curtain fabric treated with alkali reduction, and then the polyester curtain fabric treated with alkali reduction is placed in the immersion liquid 1, immersed for 70 minutes, and the liquid squeeze rate is controlled to be 88%. After squeezing out the liquid, it is placed in the immersion liquid 2 again, immersed for 60 minutes, and the liquid squeeze rate is controlled to be 83%. After squeezing out the liquid, it is then pre-baked at 86°C for 14 minutes, and baked at 185°C for 3 minutes, and then washed with hot water twice and washed with water at room temperature once, and the hot water washing temperature is controlled at 60°C. After the washing is completed, it is placed in a 65°C vacuum oven for drying for 3 hours to obtain the polyester curtain fabric with high phosphorus-containing substances grafted on the surface; The impregnation solution 1 is obtained by mixing and dissolving phosphorus-containing siloxane, organic polysilazane and acetone into a solution, wherein the mass ratio of phosphorus-containing siloxane, organic polysilazane and acetone is 20:5:120; The organopolysilazane is a colorless, transparent to light yellow liquid with a number average molecular weight of 900 g / mol and a viscosity of 40 mPa·s at 25° C.; The impregnation solution 2 is obtained by mixing and dissolving phytic acid and acetone into a solution, and the mass ratio of phytic acid to acetone is 35:100.

[0017] Step 3: Preparation of an aqueous solution of an amino-terminated tannic acid crosslinking agent Put tannic acid and deionized water into the reactor, control the stirring rate at 400 rpm, use an ice water bath to control the temperature of the contents at 0°C, and then add SOCl 2 Then the temperature was rapidly raised and kept constant at 36°C. After stirring at constant temperature for 5 hours, the unreacted SOCl in the kettle was removed by vacuum distillation at 36°C. 2 , obtain a chlorinated tannin solution, then prepare an ethylenediamine aqueous solution in advance in another reaction kettle, control the stirring rate to 700 rpm, control the temperature in the kettle to 2°C, add triethylamine, and then drop the chlorinated tannin solution into the ethylenediamine aqueous solution at a rate of 0.2 g / sec. After the dropwise addition is completed, continue to stir and react at a constant temperature for 8 hours to obtain an amino-terminated tannic acid crosslinking agent aqueous solution; The tannic acid, deionized water, SOCl 2 The feed mass ratio is 17:120:5; The mass ratio of the ethylenediamine aqueous solution, triethylamine and chlorotannin solution is 40:5:38; In the aqueous solution of ethylenediamine, the mass fraction of ethylenediamine is 60wt%.

[0018] Step 4: Preparation of cyclodextrin-embedded phosphorus-containing flame retardant β-cyclodextrin and deionized water were placed in a reactor, the stirring rate was controlled to 700 rpm, the temperature was raised and kept constant at 55°C, and the stirring was continued until the β-cyclodextrin was completely dissolved, the temperature of the materials in the reactor was lowered to 28°C, and then an ethanol solution of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide was added dropwise to the reactor at a rate of 0.5 g / s. After the addition was completed, the reaction was continued with constant temperature stirring for 3 hours, the material was placed in a 2°C environment and allowed to stand for 29 hours, and then filtered. The filtrate was dried in a vacuum oven at 60°C for 12 hours, and the obtained dry powder was the cyclodextrin-embedded phosphorus-containing flame retardant; The mass ratio of the β-cyclodextrin, deionized water, and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide ethanol solution is 50:190:60; The ethanol solution of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, wherein the mass fraction of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide is 30wt%.

[0019] Step 5: Dip-coating of flame retardant coating Add a closed anionic waterborne polyurethane dispersion, N, N-bis(2-hydroxyethyl) aminomethylphosphonic acid diethyl ester, zinc hydroxystannate, nano antimony tin oxide powder, cyclodextrin-embedded phosphorus-containing flame retardant, amino-terminated tannic acid crosslinking agent aqueous solution, and deionized water into a dispersion kettle, and vigorously disperse at 8000 rpm for 4 hours to obtain an impregnation coating liquid, and apply the impregnation coating liquid to a polyester curtain fabric with a high phosphorus-containing substance grafted on the surface by a slit coater, and control the wet film thickness of the impregnation coating liquid on both surfaces of the fabric to be 170 μm. After pre-baking the coated polyester curtain fabric at 65° C. for 45 minutes, and then baking at 140° C. for 3 minutes, an antistatic flame-retardant curtain is obtained; The solid content of the blocked anionic waterborne polyurethane dispersion is 62 wt % and the viscosity at 25° C. is 300 mPa·s; The zinc hydroxystannate is a powder with a particle size of 500 nm; The particle size of the nano antimony tin oxide powder is 50 nm; The mass ratio of the blocked anionic waterborne polyurethane dispersion, N, N-bis(2-hydroxyethyl)aminomethylphosphonic acid diethyl ester, zinc hydroxystannate, nano antimony tin oxide powder, cyclodextrin-embedded phosphorus-containing flame retardant, amino-terminated tannic acid crosslinking agent aqueous solution, and deionized water is 50:4:5:0.9:7:17:40.

[0020] Example 2: A method for preparing an anti-static flame-retardant curtain Step 1: Preparation of phosphorus-containing siloxane The reaction kettle was controlled at 0°C with an ice-water bath, and after nitrogen was passed to replace the air in the kettle, diethyl chlorophosphate and tetrahydrofuran were added under nitrogen protection, and the stirring rate was controlled to 400 rpm. After the liquid in the kettle was cooled again and kept at a constant temperature of 0°C, triethylamine was added, and then the silane coupling agent solution was added dropwise, and the dropping speed was controlled at 0.1 g / s. During the dropping process, the temperature in the kettle was controlled to be 0°C, and nitrogen protection was maintained. After the dropwise addition was completed, the temperature in the kettle was quickly raised and kept at a constant temperature of 30°C. After the reaction was stirred at a constant temperature for 6 hours, the liquid obtained by the reaction was transferred to a rotary evaporator for vacuum rotary evaporation. After the tetrahydrofuran was evaporated, the solid obtained was phosphorus-containing siloxane, which was placed in a dry container for storage; In the silane coupling agent solution, the silane coupling agent is diethylaminomethyltriethoxysilane; The silane coupling agent solution comprises a silane coupling agent and tetrahydrofuran, and the mass ratio of the silane coupling agent to the tetrahydrofuran is 75:100; The feed mass ratio of diethyl chlorophosphate, tetrahydrofuran, triethylamine and silane coupling agent solution is 20:90:0.5:10.

[0021] Step 2: Graft high phosphorus content substances onto the surface of fabric The polyester curtain fabric is immersed in a sodium hydroxide aqueous solution with a mass concentration of 15g / L, the temperature of the sodium hydroxide aqueous solution is controlled to be 70°C, the mass ratio of the polyester curtain fabric to the sodium hydroxide aqueous solution is 1:30, after the immersion treatment for 40 minutes, the polyester curtain fabric is washed with water until the washing liquid is neutral, and then placed in a 40°C vacuum oven for drying for 2 hours to obtain the polyester curtain fabric treated with alkali reduction, and then the polyester curtain fabric treated with alkali reduction is placed in the immersion liquid 1, immersed for 50 minutes, the liquid squeeze rate is controlled to be 80%, and after squeezing out the liquid, it is placed in the immersion liquid 2, immersed for 50 minutes, the liquid squeeze rate is controlled to be 80%, and after squeezing out the liquid, it is then pre-baked at 80°C for 10 minutes, and baked at 170°C for 2 minutes, and then washed with hot water twice and washed with water at room temperature once, the hot water washing temperature is controlled at 50°C, and after the washing is completed, it is placed in a 50°C vacuum oven for drying for 2 hours to obtain the polyester curtain fabric with surface grafted high phosphorus-containing substances; The impregnation solution 1 is obtained by mixing and dissolving phosphorus-containing siloxane, organic polysilazane and acetone into a solution, wherein the mass ratio of phosphorus-containing siloxane, organic polysilazane and acetone is 15:1:60; The organopolysilazane is a colorless, transparent to light yellow liquid with a number average molecular weight of 600 g / mol and a viscosity of 5 mPa·s at 25° C.; The impregnation solution 2 is obtained by mixing and dissolving phytic acid and acetone into a solution, and the mass ratio of phytic acid to acetone is 20:100.

[0022] Step 3: Preparation of an aqueous solution of an amino-terminated tannic acid crosslinking agent Put tannic acid and deionized water into the reactor, control the stirring rate at 300 rpm, use an ice water bath to control the temperature of the contents at 0°C, and then add SOCl 2 Then the temperature was rapidly raised and kept constant at 30°C. After stirring at constant temperature for 3 hours, the unreacted SOCl in the kettle was removed by vacuum distillation at 30°C. 2 , obtain a chlorinated tannin solution, then prepare an ethylenediamine aqueous solution in advance in another reaction kettle, control the stirring rate to 400 rpm, control the temperature in the kettle to 1°C, add triethylamine, and then drop the chlorinated tannin solution into the ethylenediamine aqueous solution at a rate of 0.1 g / sec. After the dropwise addition is completed, continue to stir and react at a constant temperature for 5 hours to obtain an amino-terminated tannic acid crosslinking agent aqueous solution; The tannic acid, deionized water, SOCl 2 The feed mass ratio is 10:80:2; The mass ratio of the ethylenediamine aqueous solution, triethylamine and chlorotannin solution is 30:2:30; In the aqueous solution of ethylenediamine, the mass fraction of ethylenediamine is 50wt%.

[0023] Step 4: Preparation of cyclodextrin-embedded phosphorus-containing flame retardant β-cyclodextrin and deionized water are placed in a reactor, the stirring rate is controlled at 400 rpm, the temperature is raised and kept constant at 50°C, and the stirring is continued until the β-cyclodextrin is completely dissolved, the material in the reactor is cooled to 20°C, and then an ethanol solution of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide is added dropwise to the reactor at a rate of 0.1 g / s. After the addition is completed, the reaction is continued with constant temperature stirring for 2 hours, the material is placed in a 0°C environment and allowed to stand for 24 hours, and then filtered. The filtrate is dried in a vacuum oven at 45°C for 10 hours, and the obtained dry powder is the cyclodextrin-embedded phosphorus-containing flame retardant; The mass ratio of the β-cyclodextrin, deionized water and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide ethanol solution is 30:130:30; The ethanol solution of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, wherein the mass fraction of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide is 20wt%.

[0024] Step 5: Dip-coating of flame retardant coating Add a closed anionic waterborne polyurethane dispersion, N, N-bis(2-hydroxyethyl) aminomethylphosphonic acid diethyl ester, zinc hydroxystannate, nano antimony tin oxide powder, cyclodextrin-embedded phosphorus-containing flame retardant, amino-terminated tannic acid crosslinking agent aqueous solution, and deionized water into a dispersion kettle, and vigorously disperse at 6000 rpm for 3 hours to obtain an impregnation coating liquid, and apply the impregnation coating liquid to a polyester curtain fabric with a high phosphorus-containing substance grafted on the surface by a slit coater, and control the wet film thickness of the impregnation coating liquid on both surfaces of the fabric to be 120 μm. After pre-baking the coated polyester curtain fabric at 50° C. for 30 minutes, and then baking at 130° C. for 2 minutes, an antistatic flame-retardant curtain is obtained; The solid content of the blocked anionic waterborne polyurethane dispersion is 60 wt % and the viscosity at 25° C. is 100 mPa·s; The zinc hydroxystannate is powder with a particle size of 100 nm; The particle size of the nano antimony tin oxide powder is 10 nm; The mass ratio of the blocked anionic waterborne polyurethane dispersion, N, N-bis(2-hydroxyethyl)aminomethylphosphonic acid diethyl ester, zinc hydroxystannate, nano antimony tin oxide powder, cyclodextrin-embedded phosphorus-containing flame retardant, amino-terminated tannic acid crosslinking agent aqueous solution, and deionized water is 30:2:2:0.5:3:10:30.

[0025] Example 3: A method for preparing an anti-static flame-retardant curtain Step 1: Preparation of phosphorus-containing siloxane The reaction kettle was controlled at 0°C with an ice-water bath, and after nitrogen was passed to replace the air in the kettle, diethyl chlorophosphate and tetrahydrofuran were added under nitrogen protection, and the stirring rate was controlled to 800 rpm. After the liquid in the kettle was cooled again and kept at a constant temperature of 0°C, triethylamine was added, and then the silane coupling agent solution was added dropwise, and the dropping speed was controlled at 0.6 g / s. During the dropping process, the temperature in the kettle was controlled to be 5°C, and nitrogen protection was maintained. After the dropwise addition was completed, the temperature in the kettle was quickly raised and kept at a constant temperature of 40°C. After the reaction was stirred at a constant temperature for 11 hours, the liquid obtained by the reaction was transferred to a rotary evaporator for vacuum rotary evaporation. After the tetrahydrofuran was evaporated, the solid obtained was phosphorus-containing siloxane, which was placed in a dry container for storage; In the silane coupling agent solution, the silane coupling agent is bis[3-(trimethoxysilyl)propyl]ethylenediamine; The silane coupling agent solution comprises a silane coupling agent and tetrahydrofuran, and the mass ratio of the silane coupling agent to the tetrahydrofuran is 95:100; The feed mass ratio of diethyl chlorophosphate, tetrahydrofuran, triethylamine and silane coupling agent solution is 45:140:1.5:20.

[0026] Step 2: Graft high phosphorus content substances onto the surface of fabric The polyester curtain fabric is immersed in a sodium hydroxide aqueous solution with a mass concentration of 20g / L, the temperature of the sodium hydroxide aqueous solution is controlled to be 80°C, the mass ratio of the polyester curtain fabric to the sodium hydroxide aqueous solution is 1:40, after the immersion treatment for 65 minutes, the polyester curtain fabric is washed with water until the washing liquid is neutral, and then placed in a 60°C vacuum oven for drying for 5 hours to obtain the polyester curtain fabric treated with alkali reduction, and then the polyester curtain fabric treated with alkali reduction is placed in the immersion liquid 1, immersed for 80 minutes, the liquid squeeze rate is controlled to be 90%, and after the liquid is squeezed out, it is placed in the immersion liquid 2, immersed for 80 minutes, the liquid squeeze rate is controlled to be 90%, and after the liquid is squeezed out, it is then pre-baked at 90°C for 20 minutes, and baked at 190°C for 4 minutes, and then washed with hot water twice and washed with water at room temperature once, the hot water washing temperature is controlled at 65°C, and after the washing is completed, it is placed in a 70°C vacuum oven for drying for 5 hours to obtain the polyester curtain fabric with surface grafted high phosphorus-containing substances; The impregnation solution 1 is obtained by mixing and dissolving phosphorus-containing siloxane, organic polysilazane and acetone into a solution, wherein the mass ratio of phosphorus-containing siloxane, organic polysilazane and acetone is 40:8:150; The organopolysilazane is a colorless, transparent to light yellow liquid with a number average molecular weight of 1000 g / mol and a viscosity of 50 mPa·s at 25° C.; The impregnation solution 2 is obtained by mixing and dissolving phytic acid and acetone into a solution, and the mass ratio of phytic acid to acetone is 45:100.

[0027] Step 3: Preparation of an aqueous solution of an amino-terminated tannic acid crosslinking agent Put tannic acid and deionized water into the reactor, control the stirring rate at 600 rpm, use an ice water bath to control the temperature of the contents at 0°C, and then add SOCl 2 Then the temperature was rapidly raised and kept constant at 40°C. After 6 hours of constant temperature stirring, the unreacted SOCl in the kettle was removed by vacuum distillation at 40°C. 2 , obtain a chlorinated tannin solution, then prepare an ethylenediamine aqueous solution in advance in another reaction kettle, control the stirring rate to 800 rpm, control the temperature in the kettle to 8°C, add triethylamine, and then drop the chlorinated tannin solution into the ethylenediamine aqueous solution at a rate of 0.5 g / sec. After the dropwise addition is completed, continue to stir and react at a constant temperature for 9 hours to obtain an amino-terminated tannic acid crosslinking agent aqueous solution; The tannic acid, deionized water, SOCl 2 The feed mass ratio is 30:130:8; The mass ratio of the ethylenediamine aqueous solution, triethylamine and chlorotannin solution is 60:9:70; In the aqueous solution of ethylenediamine, the mass fraction of ethylenediamine is 80wt%.

[0028] Step 4: Preparation of cyclodextrin-embedded phosphorus-containing flame retardant β-cyclodextrin and deionized water were placed in a reactor, the stirring rate was controlled at 900 rpm, the temperature was raised and kept constant at 65°C, and the stirring was continued until the β-cyclodextrin was completely dissolved, the temperature of the materials in the reactor was lowered to 30°C, and then an ethanol solution of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide was added dropwise to the reactor at a rate of 0.6 g / s. After the addition was completed, the reaction was continued at a constant temperature and stirred for 4 hours, the material was placed in a 4°C environment and allowed to stand for 36 hours, and then filtered. The filtrate was dried in a vacuum oven at 65°C for 15 hours, and the obtained dry powder was the cyclodextrin-embedded phosphorus-containing flame retardant; The mass ratio of the β-cyclodextrin, deionized water and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide ethanol solution is 60:230:85; The ethanol solution of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, wherein the mass fraction of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide is 45wt%.

[0029] Step 5: Dip-coating of flame retardant coating Add a closed anionic waterborne polyurethane dispersion, N, N-bis(2-hydroxyethyl) aminomethylphosphonic acid diethyl ester, zinc hydroxystannate, nano antimony tin oxide powder, cyclodextrin-embedded phosphorus-containing flame retardant, amino-terminated tannic acid crosslinking agent aqueous solution, and deionized water into a dispersion kettle, and vigorously disperse at 9000 rpm for 6 hours to obtain an impregnation coating liquid, and apply the impregnation coating liquid to a polyester curtain fabric with a high phosphorus-containing substance grafted on the surface by a slit coater, and control the wet film thickness of the impregnation coating liquid on both surfaces of the fabric to be 200 μm. After pre-baking the coated polyester curtain fabric at 80° C. for 50 minutes, and then baking at 160° C. for 5 minutes, an antistatic flame-retardant curtain is obtained; The solid content of the blocked anionic waterborne polyurethane dispersion is 65 wt % and the viscosity at 25° C. is 400 mPa·s; The zinc hydroxystannate is a powder with a particle size of 1300 nm; The particle size of the nano antimony tin oxide powder is 100 nm; The mass ratio of the blocked anionic waterborne polyurethane dispersion, N, N-bis(2-hydroxyethyl)aminomethylphosphonic acid diethyl ester, zinc hydroxystannate, nano antimony tin oxide powder, cyclodextrin-embedded phosphorus-containing flame retardant, amino-terminated tannic acid crosslinking agent aqueous solution, and deionized water is 65:5:6:1.3:9:25:80.

[0030] Comparative Example 1: Based on Example 1, step 1, preparing phosphorus-containing siloxane and step 2, grafting high-phosphorus-containing substances on the surface of the fabric are not performed. In step 5, dipping and coating the flame-retardant coating, the polyester curtain fabric with high-phosphorus-containing substances grafted on the surface is replaced with polyester curtain fabric. The specific operations are as follows: Step 1, preparing phosphorus-containing siloxane and step 2, grafting high-phosphorus-containing substances onto the surface of the fabric are not performed; The operations of step 3 and step 4 are the same as those of embodiment 1; Step 5: Dip-coating of flame retardant coating The polyester curtain fabric with high phosphorus-containing substances grafted on the surface was replaced with polyester curtain fabric, and the other operations were the same as in Example 1.

[0031] Comparative Example 2: Based on Example 1, in step 2, grafting high-phosphorus-containing substances on the surface of the fabric, no organic polysilazane is added to the impregnation solution 1, 5 parts of organic polysilazane are replaced by 5 parts of acetone, and the impregnation operation of the impregnation solution 2 is not performed. The specific operation is as follows: The operation of step 1 is the same as that of embodiment 1; Step 2: Graft high phosphorus content substances onto the surface of fabric The polyester curtain fabric is immersed in a sodium hydroxide aqueous solution with a mass concentration of 18 g / L, the temperature of the sodium hydroxide aqueous solution is controlled to be 77° C., the mass ratio of the polyester curtain fabric to the sodium hydroxide aqueous solution is 1:37, after the immersion treatment for 50 minutes, the polyester curtain fabric is washed with water until the washing liquid is neutral, and then placed in a 45° C. vacuum oven for drying for 3 hours to obtain the polyester curtain fabric treated with alkali reduction, and then the polyester curtain fabric treated with alkali reduction is placed in the impregnation solution 1, immersed for 70 minutes, and the liquid squeezing rate is controlled to be 88%. After squeezing out the liquid, it is then pre-baked at 86° C. for 14 minutes, and baked at 185° C. for 3 minutes, and then washed with hot water twice and washed with water at room temperature once, and the hot water washing temperature is controlled at 60° C. After the washing is completed, it is placed in a 65° C. vacuum oven for drying for 3 hours to obtain the polyester curtain fabric with high phosphorus-containing substances grafted on the surface; The impregnation solution 1 is obtained by mixing and dissolving phosphorus-containing siloxane, organic polysilazane and acetone into a solution, and the mass ratio of phosphorus-containing siloxane to acetone is 25:120; The operations of steps 3, 4 and 5 are the same as those of Example 1.

[0032] Comparative Example 3: Based on Example 1, step 3, preparing an aqueous solution of an amino-terminated tannic acid crosslinking agent, is not performed. In step 5, in the dip coating of the flame-retardant coating, 17 parts of the aqueous solution of an amino-terminated tannic acid crosslinking agent are replaced by 17 parts of deionized water in equal amounts. The specific operations are as follows: The operations of steps 1 and 2 are the same as those of Example 1; Step 3, preparing an aqueous solution of an amino-terminated tannic acid cross-linking agent, is not performed; The operation of step 4 is the same as that of embodiment 1; Step 5: Dip-coating of flame retardant coating 17 parts of the amino-terminated tannic acid crosslinker aqueous solution were replaced by 17 parts of deionized water, and the other operations were the same as in Example 1.

[0033] Comparative Example 4: Based on Example 1, step 4, preparing the cyclodextrin-embedded phosphorus-containing flame retardant, is not performed. In step 5, in the immersion coating of the flame retardant coating, 7 parts of the cyclodextrin-embedded phosphorus-containing flame retardant are replaced by 7 parts of deionized water. The specific operation is as follows: The operations of steps 1, 2, and 3 are the same as those of Example 1; Step 4, preparing a cyclodextrin-embedded phosphorus-containing flame retardant, is not performed; The operation of step 4 is the same as that of embodiment 1; Step 5: Dip-coating of flame retardant coating The 7 parts of cyclodextrin-embedded phosphorus-containing flame retardant were replaced by 7 parts of deionized water, and the other operations were the same as in Example 1.

[0034] Performance Testing: The anti-static flame retardant curtains obtained in Examples 1, 2, 3 and Comparative Examples 1, 2, 3, and 4 were washed 30 times with reference to GB / T33283-2016 "Textiles - Tests for Color Fastness - Color Fastness to Industrial Washing". The anti-static flame retardant curtains before and after washing were subjected to the following tests: The flame retardancy of fabrics was determined according to GB / T 8745-2001 "Combustion performance of textiles - Determination of surface burning time of fabrics". In the flame retardancy test, the flame height was 4 cm, the fire source ignited the fabric for 12 seconds, and its afterburning time and smoldering time were tested. Refer to FZ / T 50017-2011 "Test method for flame retardancy of polyester fiber - oxygen index method" to test the limiting oxygen index; According to GB / T 12703-2009 "Evaluation of electrostatic properties of textiles Part 2: Charge surface density", the charge surface density is less than 1.5μC / m 2 , test the anti-static performance; The specific test results are shown in Table 1: Table 1

[0035] From the data in Table 1, it can be seen that in Comparative Example 1, the surface of the polyester fiber is not grafted with high-phosphorus substances, and only the flame retardant coating is dipped and coated. The flame retardant performance of Comparative Example 1 drops to the worst value of all embodiments and comparative examples, and after washing 30 times, the flame retardant performance decreases significantly, which indicates that the grafting of high-phosphorus substances on the surface of the polyester fiber plays a vital role in improving the flame retardant performance of the curtain and maintaining the flame retardant performance after multiple washings. In addition, the antistatic performance of Comparative Example 1 is almost the same as that of Example 1 before washing, and the antistatic performance decreases very quickly after washing 30 times. This may be because the polyester fiber without high-phosphorus substances grafted on the surface does not After alkali reduction treatment, during the process of impregnation and coating of flame retardant coating, the adhesion between the coating and the surface of the polyester fiber is not particularly good, so the flame retardant and antistatic properties of the curtain decay rapidly after washing; in Comparative Example 2, in the step of grafting high-phosphorus-containing substances on the surface of the fabric, no organic polysilazane is added to the impregnation solution 1, and no impregnation with phytic acid acetone solution is performed. The flame retardant property of Comparative Example 2 is significantly reduced compared with Example 1, which shows that organic polysilazane and phytic acid can greatly improve the flame retardant property of the curtain fabric through the synergistic effect of the three flame retardant elements of phosphorus, nitrogen and silicon. In addition, the antistatic property of Comparative Example 2 decreases significantly after washing 30 times, which may be Due to the participation of organic polysilazane and phytic acid in the grafting reaction on the surface of polyester fiber, the adhesion between the surface of polyester fiber and the flame retardant coating can be improved, thereby affecting the water washing resistance of the curtain coating; in Comparative Example 3, in the treatment of immersion coating of flame retardant coating, no amino-terminated tannic acid crosslinking agent aqueous solution is added to the immersion coating liquid. Before washing, the flame retardant and antistatic properties of Comparative Example 3 are almost unchanged compared with those of Example 1, but after washing 30 times, the flame retardant and antistatic properties of Comparative Example 3 become very poor, which indicates that the amino-terminated tannic acid in the amino-terminated tannic acid crosslinking agent aqueous solution can improve the water washing resistance of the curtain by increasing the crosslinking degree of the coating. Reduce the loss of flame retardants and antistatic agents caused by washing; in Comparative Example 4, no cyclodextrin-embedded phosphorus-containing flame retardant is added to the dip-coated flame retardant coating. Before washing, the flame retardant performance of Comparative Example 4 is significantly reduced, and the antistatic performance has no significant change. After washing 30 times, the flame retardant and antistatic properties of Comparative Example 4 are greatly reduced, which shows that cyclodextrin-embedded phosphorus-containing flame retardant can not only improve the flame retardant properties of curtains, but also reduce the loss rate of flame retardants and antistatic agents during curtain washing. This may be due to the fact that cyclodextrin has a certain degree of cross-linking reaction on the coating, and the adhesion of the flame retardant and antistatic agent in the coating is improved by increasing the cross-linking density.

[0036] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing an anti-static flame-retardant curtain, characterized in that: The preparation method of the anti-static flame-retardant curtain comprises five steps: preparing phosphorus-containing siloxane, grafting high-phosphorus-containing substances onto the surface of the fabric, preparing an amino-terminated tannic acid cross-linking agent aqueous solution, preparing a cyclodextrin-embedded phosphorus-containing flame retardant, and dipping and coating a flame-retardant coating. The method for preparing the phosphorus-containing siloxane comprises: controlling the temperature of the reaction kettle at 0°C by using an ice-water bath, replacing the air in the kettle with nitrogen, and adding diethyl chlorophosphate and tetrahydrofuran under nitrogen protection, controlling the stirring rate to 400-800 rpm, and adding triethylamine after the liquid in the kettle is cooled again and kept at a constant temperature of 0°C, and then dripping the silane coupling agent solution, and controlling the dripping speed to 0.1-0.6 g / s. During the dripping process, the temperature in the kettle is controlled to be 0-5°C, and nitrogen protection is maintained. After the dripping is completed, the temperature in the kettle is rapidly heated and kept at a constant temperature of 30-40°C, and the reaction is stirred at a constant temperature for 6-11 hours, and the liquid obtained by the reaction is transferred to a rotary evaporator for vacuum rotary evaporation. After the tetrahydrofuran is evaporated, the obtained solid is the phosphorus-containing siloxane, which is placed in a dry container for storage for later use; In the silane coupling agent solution, the silane coupling agent is one of 3-aminopropyltriethoxysilane, diethylaminomethyltriethoxysilane, and bis[3-(trimethoxysilyl)propyl]ethylenediamine; The surface of the fabric is grafted with a high-phosphorus substance, the polyester curtain fabric is immersed in a sodium hydroxide aqueous solution with a mass concentration of 15-20 g / L, the temperature of the sodium hydroxide aqueous solution is controlled to be 70-80° C., the mass ratio of the polyester curtain fabric to the sodium hydroxide aqueous solution is 1:30-40, after the immersion treatment for 40-65 minutes, the polyester curtain fabric is washed with water until the washing liquid is neutral, and then placed in a vacuum oven at 40-60° C. and dried for 2-5 hours to obtain the polyester curtain fabric treated with alkali reduction, and then the polyester curtain fabric treated with alkali reduction is placed in the immersion solution for 1 , immersing in the impregnation liquid 2 for 50-80 minutes, controlling the liquid squeezing rate to be 80-90%, squeezing out the liquid, and then putting it into the impregnation liquid 2, immersing it for 50-80 minutes, controlling the liquid squeezing rate to be 80-90%, squeezing out the liquid, and then pre-baking at 80-90° C. for 10-20 minutes, and baking at 170-190° C. for 2-4 minutes, and then washing it with hot water twice and washing it with water at room temperature once, the hot water washing temperature being controlled at 50-65° C., and after washing, putting it into a vacuum oven at 50-70° C. and drying it for 2-5 hours to obtain a polyester curtain fabric with a surface grafted with a high phosphorus-containing substance; The impregnation solution 1 is obtained by mixing and dissolving phosphorus-containing siloxane, organic polysilazane and acetone into a solution, wherein the mass ratio of phosphorus-containing siloxane, organic polysilazane and acetone is 15-40:1-8:60-150; The organopolysilazane is a colorless, transparent to light yellow liquid with a number average molecular weight of 600-1000 g / mol and a viscosity of 5-50 mPa·s at 25°C; The impregnation solution 2 is obtained by mixing and dissolving phytic acid and acetone into a solution, and the mass ratio of phytic acid to acetone is 20-45:100; The method for preparing the aqueous solution of the amino-terminated tannic acid crosslinking agent comprises: placing tannic acid and deionized water into a reaction kettle, controlling the stirring rate at 300-600 rpm, controlling the temperature of the materials in the kettle at 0°C by using an ice-water bath, adding SOCl2, and then rapidly heating and maintaining the temperature at 30-40°C, stirring and reacting at the constant temperature for 3-6 hours, controlling the temperature at 30-40°C to remove the unreacted SOCl2 in the kettle by vacuum distillation, and obtaining a chlorinated tannin solution; and then preparing an aqueous solution of ethylenediamine in advance in another reaction kettle, controlling the stirring rate at 400-800 rpm, controlling the temperature in the kettle at 1-8°C, and then adding triethylamine, and then dripping the chlorinated tannin solution into the aqueous solution of ethylenediamine at a speed of 0.1-0.5 g / s, and after the dripping is completed, continuing the constant temperature stirring and reacting for 5-9 hours to obtain an aqueous solution of the amino-terminated tannic acid crosslinking agent; The method for preparing the cyclodextrin-embedded phosphorus-containing flame retardant comprises: placing β-cyclodextrin and deionized water into a reactor, controlling the stirring rate to 400-900 rpm, raising the temperature and maintaining the temperature at 50-65° C., and continuously stirring until the β-cyclodextrin is completely dissolved, cooling the material in the reactor to 20-30° C., then dripping an ethanol solution of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide into the reactor at a rate of 0.1-0.6 g / s, and continuing to stir and react at a constant temperature for 2-4 hours after the dripping is completed. The material is placed in an environment of 0-4° C. and allowed to stand for 24-36 hours, and then filtered. The filtrate is dried in a vacuum oven at 45-65° C. for 10-15 hours, and the obtained dry powder is the cyclodextrin-embedded phosphorus-containing flame retardant; The dip-coating flame-retardant coating comprises the following steps: adding a closed anionic waterborne polyurethane dispersion, N, N-bis(2-hydroxyethyl) aminomethylphosphonic acid diethyl ester, zinc hydroxystannate, nano antimony tin oxide powder, cyclodextrin-embedded phosphorus-containing flame retardant, amino-terminated tannic acid crosslinking agent aqueous solution and deionized water into a dispersion kettle, controlling the speed to be 6000-9000 rpm, and dispersing vigorously for 3-6 hours to obtain an dip-coating liquid, and coating the dip-coating liquid onto a polyester curtain fabric with a high phosphorus-containing substance grafted on the surface thereof by a slit coater, controlling the wet film thickness of the dip-coating liquid on both surfaces of the fabric to be 120-200 μm, and pre-baking the coated polyester curtain fabric at 50-80° C. for 30-50 minutes, and then baking at 130-160° C. for 2-5 minutes to obtain an antistatic flame-retardant curtain.

2. The method for preparing the anti-static and flame-retardant curtain according to claim 1, characterized in that: The silane coupling agent solution comprises a silane coupling agent and tetrahydrofuran, and the mass ratio of the silane coupling agent to the tetrahydrofuran is 75-95:100; The feeding mass ratio of the diethyl chlorophosphate, tetrahydrofuran, triethylamine and silane coupling agent solution is 20-45:90-140:0.5-1.5:10-20.

3. The method for preparing the anti-static and flame-retardant curtain according to claim 1, characterized in that: The mass ratio of tannic acid, deionized water and SOCl2 is 10-30:80-130:2-8; The mass ratio of the ethylenediamine aqueous solution, triethylamine and chlorotannin solution is 30-60:2-9:30-70; In the aqueous solution of ethylenediamine, the mass fraction of ethylenediamine is 50-80wt%.

4. The method for preparing the anti-static and flame-retardant curtain according to claim 1, characterized in that: The mass ratio of the β-cyclodextrin, deionized water and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide ethanol solution is 30-60:130-230:30-85; The ethanol solution of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, wherein the mass fraction of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide is 20-45wt%.

5. The method for preparing the anti-static and flame-retardant curtain according to claim 1, characterized in that: The solid content of the blocked anionic waterborne polyurethane dispersion is 60-65wt%, and the viscosity at 25°C is 100-400mPa·s; The zinc hydroxystannate is a powder with a particle size of 100-1300 nm; The particle size of the nano antimony tin oxide powder is 10-100 nm; The mass ratio of the blocked anionic waterborne polyurethane dispersion, N, N-bis(2-hydroxyethyl)aminomethylphosphonic acid diethyl ester, zinc hydroxystannate, nano antimony tin oxide powder, cyclodextrin-embedded phosphorus-containing flame retardant, amino-terminated tannic acid crosslinking agent aqueous solution, and deionized water is 30-65:2-5:2-6:0.5-1.3:3-9:10-25:30-80.

6. The anti-static and flame-retardant curtain obtained by the preparation method according to any one of claims 1 to 5, characterized in that: The anti-static flame-retardant curtain has an afterflaming time and a smoldering time of 0 seconds before and after washing for 30 times, a limiting oxygen index of 34 to 34.5 before washing and 33 to 34 after washing for 30 times, and a charge surface density of 0.3 to 0.4 μC / m before washing. 2 , 0.4~0.5μC / m after washing 30 times 2 .

Citation Information

Patent Citations

  • Novel flame-retardant and environment-friendly cloth curtain

    CN108891109A

  • Environment-friendly waterproof flame-retardant full-shading curtain fabric and manufacturing method thereof

    CN115284701A