Anti-laser viscoelastic composition as well as preparation method and application thereof
By introducing anti-laser dyes and co-solvents into ophthalmic viscoelastic agents, viscoelastic compositions with laser protection functions have been developed, which solves the problem that viscoelastic agents cannot effectively protect corneal endothelial cells in laser surgery in the prior art, and realizes the problem that viscoelastic agents cannot effectively protect corneal endothelial cells in laser surgery. High light transmission and chromogenicity are used to significantly reduce laser damage and postoperative residual risk.
Patent Information
- Application Number
- CN202410937136.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-07-12
AI Technical Summary
The existing ophthalmic viscoelastic agents lack laser protection function in laser surgery, which cannot effectively protect corneal endothelial cells from damage to laser energy, and are difficult to remove, affecting the surgical effect and postoperative recovery.
Develop a anti-laser viscoelastic composition containing rheological active ingredients, anti-laser dyes and co-solvents, with high light transmittance and laser protection characteristics in a specific wavelength range, by adding quinone or azo dyes and co-solvents , realize dissolution and uniform dispersion in the aqueous system, provide good light transmittance and chromogenicity, significantly reduce laser transmittance, and protect intraocular tissue.
This composition significantly reduces the damage to the tissues in the eye by laser surgery, provides significant postoperative removal convenience with color development, reduces complications such as high intraocular pressure, and improves surgical safety and effectiveness.
Smart Images

Figure CN118987369A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of medical biomaterials, and specifically relates to a laser-proof viscoelastic composition and a preparation method and use thereof. Background Art
[0002] Cataract is the most common blinding eye disease in the world. The global blindness caused by cataract accounts for 46%, and the trend continues to rise. According to survey data, among the approximately 5.4 million blind people over the age of 50 in my country, approximately 3.6 million (66.9%) suffer from cataract, which is the leading blinding eye disease in my country. Cataract phacoemulsification surgery is the most advanced and effective treatment technology in the world. The surgery is painless, short in time, with small incisions and fast recovery. There is still a lot of room for improvement in the number of artificial lens implants in my country. At present, laser emulsification can effectively emulsify the hard nucleus of the lens, especially for some complex surgical situations. It has the advantages of smaller corneal incisions, less damage to intraocular tissues, and higher safety. However, the laser energy and frequency intensity used are high, and there is still the possibility of some serious complications that threaten vision, and there is a certain degree of surgical risk. According to the wavelength range, the spectrum can be divided into ultraviolet light (200nm~<400nm), visible light (400nm~<780nm) and infrared light (780nm~1mm). Commonly used lasers or optical instruments include 532nm potassium titanyl phosphate laser, 585 / 595nm pulse dye laser, 694nm ruby laser, 755nm alexandrite laser, 800 / 810nm semiconductor laser, 1064nm neodymium: yttrium aluminum garnet laser, 2940nm erbium laser, 10600nm carbon dioxide (CO2) laser and 400~1200nm intense pulsed light. Various types of lasers are used in dermatology to treat pigmentary diseases, vascular diseases, scars and photoaging, and are also widely used in ophthalmic surgery, such as refractive errors, cataracts, glaucoma, fundus diseases and tear duct diseases. At present, there are many lasers used in ophthalmic treatment at home and abroad (see Table 1): Table 1 Commonly used ophthalmic laser wavelengths (nm)
[0003] The treatment of post-cataract is mainly with 1064nm continuous wave YAG laser. The lasers for fundus diseases are mainly argon laser, krypton laser, dye laser, 532nm frequency-doubled YAG laser, etc. Lasers with different wavelengths are selected according to different situations to achieve the purpose of treatment. Femtosecond laser with a wavelength of 1053nm has also been successfully used in the field of ophthalmic surgery. Studies have found that Nd:YAG laser peripheral iridectomy and posterior capsulotomy cause certain damage to the corneal endothelium.
[0004] In order to improve the quality of surgery, create surgical space, protect corneal endothelial cells, and reduce the damage to corneal endothelial cells caused by surgical operations, viscoelastic agents are necessary auxiliary materials for ophthalmic surgeries such as cataracts. They are a kind of sterile and pyrogen-free biomaterial with certain viscoelasticity. Their main function is to be used by clinicians as a surgical pad for ophthalmic microsurgery to temporarily support the surgical space, protect the tissue from mechanical damage by surgical instruments, and facilitate the smooth implementation of the operation. Commonly used active rheological components of viscoelastics include sodium hyaluronate, sodium chondroitin sulfate, hydroxypropyl methylcellulose, polyacrylamide, etc. Sodium hyaluronate is a chain polyanionic acidic mucopolysaccharide, which is the most common rheological active ingredient of ophthalmic viscoelastics so far. According to their rheological properties, they are divided into cohesive, diffuse and mixed types. Cohesive viscoelastics have better support due to their high shear viscosity, represented by the commercially available Avi and Qisheng. Due to their large molecular weight, they are easy to be removed after surgery; diffuse viscoelastics have lower shear viscosity and better protection of corneal endothelial cells, represented by the commercially available Viscoat, which is relatively difficult to remove after surgery; mixed viscoelastics are represented by AlCON's DuoVisc and ALBOMED's Pe-Ha-Luron F. In theory, mixed viscoelastics can better combine the characteristics of support and endothelial protection, and can be applied to some complex surgical conditions. Especially some formulas that contain sodium hyaluronate of different molecular weights, in which the high molecular weight part can provide better support, and the small molecule part provides better wettability, protection and certain anti-inflammatory effects.
[0005] Currently, the mainstream viscoelastics available on the market are all prepared by dissolving rheologically active ingredients in a buffer system. They mainly play the role of supporting and protecting the corneal endothelium. There are very few products that add other functional ingredients. Patents related to medical sodium hyaluronate gel / viscoelastics include those with single components, composite components or functional components, such as (1) CN1524579B discloses a drug-loaded color-developing composite viscoelastic, which contains an anti-cell metabolism drug and a drug with color or fluorescence as an indicator component; (2) CN105903088A discloses a method for preparing an ophthalmic viscoelastic with selective anterior capsule staining function, in which 0.002-0.6% trypan blue dye is added, and the in vitro release rate is about 15% for 60 minutes. During use, it is continuously and slowly released to the surgical operation site to achieve the purpose of selective staining, and at the same time, it is unlikely to cause damage to tissue cells. However, the viscoelastic provided above can only add a color developer as an indicator, and does not have the ability to prevent laser penetration or absorb laser energy. Therefore, in terms of laser treatment or laser protection, commercially available viscoelastics have no special protective effect against lasers. At present, there is no viscoelastic product and technology that has both light transmittance, color development and laser protection. Therefore, the market is in urgent need of a viscoelastic product with laser protection to match the development of existing ophthalmic surgery (especially cataract surgery) technology. It can also be used in other laser surgeries for postoperative protection and maintenance of the perioperative area and the surgical site. Summary of the invention
[0006] The first object of the present invention is to provide a laser-resistant viscoelastic composition to better match the needs of the current development of ophthalmic surgical technology.
[0007] Specifically, the anti-laser viscoelastic composition provided by the present invention comprises a rheologically active component, an anti-laser dye and a cosolvent; the anti-laser viscoelastic composition has a light transmittance of more than 90% at a visible light wavelength of 550-675 nm, and a light transmittance of less than 70% at a wavelength of 300-450 nm and / or 800-1100 nm.
[0008] Preferably, the light transmittance of the anti-laser viscoelastic composition at a visible light wavelength of 550-675 nm is above 93%, and the light transmittance at a wavelength of 800-1100 nm is below 75%.
[0009] In some embodiments provided by the present invention, the transmittance of the anti-laser viscoelastic composition at a laser wavelength of 800-1100nm is 8%-70%; or, the transmittance at a laser wavelength of 800-1070nm is 8%-50%; more preferably, the transmittance at a laser wavelength of 1000±10nm is less than 10% (including 10%).
[0010] In some embodiments provided by the present invention, the light transmittance of the anti-laser viscoelastic composition at a specific laser wavelength of 1060-1068 nm is 40%-45%, which reduces the light transmittance by 55%-60%.
[0011] In some embodiments provided by the present invention, the light transmittance of the anti-laser viscoelastic composition at a laser wavelength of 300-450 nm is less than 40%.
[0012] In some embodiments provided by the present invention, the light transmittance of the anti-laser viscoelastic composition at a laser wavelength of 450-500 nm is 0-30%.
[0013] Preferably, the transmittance of the laser-resistant viscoelastic composition at a characteristic laser wavelength of 1064 nm is reduced by 50%-70%.
[0014] The anti-laser viscoelastic composition of the present invention has good light transmittance, color rendering and laser protection characteristics in ophthalmic surgery, and exhibits laser protection characteristics in a specific wavelength band, especially laser protection characteristics at a specific surgical wavelength. It can effectively absorb a light source of a specific wavelength and reduce its transmittance by 50% to 70%, thereby effectively protecting intraocular tissues.
[0015] The anti-laser viscoelastic composition provided by the present invention, wherein the anti-laser dye is an azo dye, and the transmittance at a laser wavelength of 300-450nm is 30%-40%; or the anti-laser dye is a quinone dye, and the transmittance at a laser wavelength of 300-450nm is 0-15%.
[0016] Preferably, the anti-laser viscoelastic composition provided by the present invention is -1 The lower shear viscosity is 10-120 Pa·s, and / or the absolute complex viscosity at 0.1 Hz is 10-120 Pa·s.
[0017] More preferably, the laser-resistant viscoelastic composition -1 The lower shear viscosity is 40-90 Pa·s, and / or the absolute complex viscosity at 0.1 Hz is 35-85 Pa·s.
[0018] The present invention also provides another anti-laser viscoelastic composition, which comprises: The molar ratio is 2.5*10 -6 ~6*10 -3 mol / L of rheologically active ingredients; Anti-laser dye with a mass content of 0.0001~0.05%; Solvent; pH buffers; Osmotic pressure regulator.
[0019] The dosage of the cosolvent, pH buffer and osmotic pressure regulator can be determined as appropriate according to the preparation requirements.
[0020] Preferably: In the anti-laser viscoelastic composition provided by the present invention, the rheologically active component is selected from one or more of sodium hyaluronate, chondroitin sulfate, and sodium hydroxypropyl methylcellulose, preferably sodium hyaluronate.
[0021] In a preferred embodiment provided by the present invention, the sodium hyaluronate is selected from a mixture of two or three rheologically active ingredients of high, medium and low molecular weights; for example, two or three of a low molecular weight portion (LMWHA) of 5 to 100 KDa (inclusive), a medium molecular weight portion (MMWHA) of 100 to 2000 KDa (inclusive) and a high molecular weight portion (HMWHA) of 2000 to 4000 KDa (inclusive).
[0022] When sodium hyaluronate is selected as the rheologically active ingredient, the molar proportion of sodium hyaluronate in the viscoelastic composition is 2.5*10 -6 ~6*10 -3 mol / L is appropriate; preferably 1.5*10 -5 ~1.0*10 -4 mol / L; more preferably, the molar ratio of LMWHA in the sodium hyaluronate is 0~1*10 -3 mol / L, the molar proportion of MMWHA is 0~1.5*10 -4 mol / L; the molar proportion of HMWHA is 0~1.4*10 -5 mol / L. It is particularly preferred that the molar ratio of LMWHA in the sodium hyaluronate is 10 -5 ~10 -3 mol / L, the molar ratio of MMWHA is 5*10 -7 ~1.5*10 -4 mol / L; the molar proportion of HMWHA is 10 -6 ~1.4*10 -5 mol / L.
[0023] The above-mentioned anti-laser viscoelastic composition provided by the present invention contains an anti-laser dye, and the anti-laser dye is selected from one or more of quinone dyes, azo dyes, and cyanine dyes; wherein, quinone dyes include 2-hydroxy-1,4-naphthoquinone, anthraquinone dye alizarin green and transparent green 5B, etc.; azo dyes include azobenzene, disperse yellow 7, aniline brown, etc.; cyanine dyes include 3H-indole keto acid cyanine dyes, quinaldine keto acid cyanine dyes, 4-tetranitrophthalocyanine copper dyes, etc.; the anti-laser dye of the present invention is particularly preferably transparent green 5B or aniline brown. The above-mentioned dyes are particularly suitable for the viscoelastic composition system of the present invention at a specific concentration, and can be directly dissolved in an aqueous system under the action of a cosolvent and a dispersant.
[0024] The anti-laser viscoelastic composition provided by the present invention, the content of the anti-laser dye is 0.0001-0.05% of the anti-laser viscoelastic composition; preferably 0.001-0.01% of the anti-laser viscoelastic composition, more preferably 0.002-0.006%, for example 0.001%, 0.002%, 0.003%, 0.004%, 0.005%, 0.006%, etc.
[0025] In some preferred embodiments provided by the present invention, sodium hyaluronate is selected as the rheologically active ingredient and is matched with transparent green 5B or aniline brown as an anti-laser dye, assisted by the wetting and thickening effects of the cosolvent. The use effect of the obtained anti-laser viscoelastic composition is particularly outstanding (especially the laser protection effect), and its effect is better than that of the existing viscoelastic agents used in ophthalmic surgery. Especially in laser cataract surgery, the anti-laser dye component helps to achieve laser protection during the operation, has strong wettability, good light transmittance, and achieves satisfactory maintenance of intraocular space and protection of eye tissues. At the end of the process, it is easy to remove due to color visualization, and can provide obvious protection against laser-induced light damage during the operation.
[0026] In the anti-laser viscoelastic composition provided by the present invention, the cosolvent is selected from one or more of propylene glycol, glycerol, mannitol, P188, RH40, and cocamidopropyl betaine, preferably propylene glycol or glycerol.
[0027] In some preferred embodiments provided by the present invention, the proportion of the co-solvent in the anti-laser viscoelastic composition is 0.5-5%, preferably 1-3%, for example 1%, 1.5%, 1.8%, 2%, 2.5%, 3%, etc.
[0028] The anti-laser viscoelastic composition provided by the present invention has a pH value of 6.0-8.0, preferably a pH value of 6.8-7.6, and more preferably 7.1-7.3, for example 7.10, 7.12, 7.15, 7.18, 7.19, 7.20, 7.22, 7.25, 7.26, etc. Within the above range, the composition of the invention has a pH value similar to and stable to that of aqueous humor, and plays a better protective role during surgery.
[0029] In the anti-laser viscoelastic composition provided by the present invention, the pH buffer is selected from one or more of boric acid / borax, disodium hydrogen phosphate / sodium dihydrogen phosphate, citric acid / sodium citrate, and aminocaproic acid, preferably disodium hydrogen phosphate / sodium dihydrogen phosphate, especially disodium hydrogen phosphate / sodium dihydrogen phosphate in a dosage ratio of 2:1-15:1.
[0030] Preferably, the total amount of the pH buffer in the anti-laser viscoelastic composition does not exceed 1%; preferably 0.35% to 0.6%; more preferably 0.385% to 0.545%.
[0031] In addition, the pH buffer of the present invention also contains hydrochloric acid or sodium hydroxide as a pH adjuster, and the specific amount of hydrochloric acid or sodium hydroxide used is based on the amount required to adjust the pH value of the anti-laser viscoelastic composition, and usually does not exceed 0.5% of the anti-laser viscoelastic composition.
[0032] In the anti-laser viscoelastic composition provided by the present invention, the osmotic pressure regulator is selected from one or more of sodium chloride, potassium chloride, calcium chloride, and magnesium chloride, preferably sodium chloride. The amount of the osmotic pressure regulator is based on adjusting the osmotic pressure of the anti-laser viscoelastic composition to 270-400mOsmol / kg, preferably 280-360mOsmol / kg. Within the above range, the composition of the invention has a stable osmotic pressure value similar to that of aqueous humor, and plays a better protective role during surgery.
[0033] In some preferred embodiments provided by the present invention, the proportion of the osmotic pressure regulator in the anti-laser viscoelastic composition is 0.1-0.5%, preferably 0.1-0.3%, more preferably 0.15%-0.2%, for example 0.15%, 0.16%, 0.18%, 0.2%, etc.
[0034] As a preferred embodiment of the present invention, the formula of the provided anti-laser viscoelastic composition is as follows: The molar ratio is 2.5*10 -6 ~6*10 -3 mol / L sodium hyaluronate composition; Transparent green 5B or aniline brown with a mass content of 0.001~0.01%; Cosolvent propylene glycol or glycerol; pH buffer disodium hydrogen phosphate / sodium dihydrogen phosphate; Osmotic pressure regulator: sodium chloride.
[0035] More preferably, the amount of the co-solvent is 1-3% of the anti-laser viscoelastic composition; The pH value of the laser-proof viscoelastic composition is 6.8-7.6; the osmotic pressure is 280-360 mOsmol / kg.
[0036] In the above sodium hyaluronate composition, the molar proportion of LMWHA is 0-10 -3 mol / L, the molar proportion of MMWHA is 0~1.5*10 -4 mol / L; the molar proportion of HMWHA is 0~1.4*10 -5 mol / L.
[0037] With the anti-laser viscoelastic composition having the above formula, the dye can be more fully and evenly integrated into the anti-laser viscoelastic agent, and the protective effect against laser energy is particularly prominent.
[0038] The second object of the present invention is to provide a method for preparing the above-mentioned laser-resistant viscoelastic composition, which comprises: The anti-laser dye is pre-dispersed with a dispersant, then added into a buffer solution containing a cosolvent, an osmotic pressure regulator and a pH buffer, and then the dispersant is removed by vacuum drying, and finally the rheological active component is added and mixed evenly.
[0039] In order to overcome the shortcomings of incomplete removal and difficult observation of viscoelastics after ophthalmic surgery, and to adapt to the special requirements of laser protection in laser cataract surgery, how to select suitable anti-laser dyes and mix them evenly into the viscoelastic formula to provide an anti-laser viscoelastic with good light transmittance, color development, and easy removal for ophthalmic surgery has become a research topic that needs to be solved urgently.
[0040] As is known to all, laser protection materials are mainly polymer dye particles such as fullerene C60, carbon nanotubes, porphyrins, metal phthalocyanines, polyacetylene, and metal oxide films, etc., which are sensitive to wavelength and light intensity, and can meet the requirements of absorbance or optical density at one or more wavelengths, while maximizing the visible light transmittance of thermoplastic resins, glass or other substrates. The laser protection wavelength, optical density, transparency, laser damage threshold and protection angle of different protective materials are different. However, dye powders can only be dissolved in organic solvents to a certain extent, especially dyes suitable for use in ophthalmic surgery protection wavelengths. Therefore, those skilled in the art cannot directly add anti-laser dyes to aqueous viscoelastic formulations to obtain anti-laser viscoelastics.
[0041] In addition, although quinone dyes (transparent green 5B, etc.), azo dyes (aniline brown, etc.) and other laser absorbing compound dyes can effectively absorb light sources in the 900-1100nm band, covering the laser wavelength of 1064nm commonly used in cataract surgery. 4-tetranitrophthalocyanine copper can provide effective laser protection at 300-400nm, but these dyes can only be dissolved in organic solvents and cannot be directly dissolved in aqueous systems. In order to solve this problem, the present invention selectively adds anti-laser dyes to the viscoelastic formulation by adding cosolvents and pre-dispersing. Different anti-laser dyes have good spectral transmittance within the visible light range of surgical operations, which is above 93%, and do not affect the surgical field of view. During the surgical operation time, the dye will not diffuse from the composition to the surrounding tissues, causing staining of normal tissues in the eye. It has good absorption at specific laser wavelengths and can effectively absorb lasers of different wavelengths during surgery, reducing the impact and damage of lasers on other tissues in the eye.
[0042] In the preparation method of the laser-proof viscoelastic composition provided by the present invention, the dispersant is selected from one of ethanol, n-propanol and isopropanol, preferably ethanol or isopropanol.
[0043] When used, the mass ratio of the anti-laser dye in the dispersant is preferably 1:1000~1:10000; more preferably, the mass ratio is 1:1000~1:5000; for example, 1:1000, 1:1500, 1:2000, 1:2500, 1:3000, 1:5000, etc.
[0044] The preparation method of the anti-laser viscoelastic composition provided by the present invention also includes the step of preparing a buffer solution, specifically: weighing a cosolvent, an osmotic pressure regulator, and a pH buffer, dissolving them with sterile water for injection, mixing them evenly, and filtering and sterilizing them.
[0045] and further including: The anti-laser dye is pre-dispersed in a dispersant, and impurities are removed by filtration. The dye pre-dispersed solution is then added to the buffer solution, and the dispersant is removed by vacuum drying at low temperature. The rheologically active component (such as a sodium hyaluronate composition) is then added thereto, mixed, filled, and sterilized by wet heat to obtain a viscoelastic for ophthalmic surgery.
[0046] The specific conditions for vacuum drying at low temperature to remove the dispersant are not particularly limited in the present invention. Suitable conditions include vacuum drying at 40°C for 10-30 min, vacuum drying at 30°C for 20-30 min, and vacuum drying at 50°C for 10-30 min. It can be a vacuum drying oven or equivalent equipment, and the vacuum condition is above 100Pa, as long as the dispersant can be removed.
[0047] The inventors have found that adding a specific co-solvent can increase the solubility of laser dyes in viscoelastics. However, since the co-solvent itself also has a certain viscosity, it is not conducive to the dissolution of the dye, and the addition content exceeding 5% will cause the osmotic pressure of the entire system to exceed the ophthalmic standard. Therefore, the inventors have innovatively proposed to break down the steps of adding the entire dye to the traditional viscoelastic buffer system into three steps: first, adding the co-solvent to the buffer solution; then pre-dispersing the dye in a dispersant with high solubility to form a pre-dispersion liquid; then adding the pre-dispersion liquid to the buffer solution, mixing evenly and then drying to remove the dispersant, thereby successfully adding the anti-laser dye to the viscoelastic system step by step, and finally adding the rheologically active ingredient, filling and sterilizing to obtain the anti-laser viscoelastic.
[0048] The present invention effectively solves the problem of anti-laser dye being insoluble in water by pre-dispersion, and can have the characteristics of both cohesive and diffuse viscoelastic agents, and is simple to operate, and the hydrogen bonding between the dye and the cosolvent and the rheologically active component allows the dye to be stably dispersed in the viscoelastic agent. The anti-laser viscoelastic provided by the present invention is composed of a rheologically active component, a cosolvent, an anti-laser dye, a pH regulator, and an osmotic pressure regulator, and can effectively play a role in laser protection during laser cataract surgery, using laser dye to absorb laser energy, reducing laser damage to other unexpected parts of the eye, having good visible light transmittance, and developing color during postoperative removal, so that the surgical operator can intuitively observe the part of the viscoelastic agent remaining in the anterior chamber, accurately rinse and remove the local viscoelastic agent, effectively remove the viscoelastic agent remaining in the eye, and reduce complications such as high intraocular pressure caused by postoperative residues.
[0049] The present invention also provides the use of the anti-laser viscoelastic composition in laser surgery, especially in ophthalmic laser surgery; Preferably, the ophthalmic surgery includes intracapsular cataract extraction, phacoemulsification, keratoplasty, intraocular lens implantation and removal, iridotomy, anterior chamber hemorrhage surgery, foreign body and tumor removal, trabeculectomy, vitrectomy or foreign body removal, retinal detachment and epiretinal membrane removal surgery, glaucoma, diabetic retinopathy, and femtosecond laser surgery.
[0050] The anti-laser viscoelastic composition provided by the present invention can be used to assist in ophthalmic surgery, especially laser cataract surgery. The anti-laser viscoelastic agent of the present invention has good light transmittance, color rendering and laser protection characteristics in laser surgery, especially ophthalmic surgery (it can absorb laser energy during surgery and reduce laser damage to other unexpected parts of the eye), and has the characteristic of postoperative removal visualization, which can ensure that the viscoelastic composition is removed as completely as possible, help the surgeon to judge the removal situation, effectively prevent problems such as corneal endothelial cell damage caused by laser during ophthalmic surgery, and reduce complications such as high intraocular pressure caused by postoperative residues. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0052] Figure 1 It is a schematic diagram of the color development state of the laser-resistant viscoelastic composition after being immersed in physiological saline for 15 minutes.
[0053] Figure 2 It is a UV-visible-near infrared spectral transmittance spectrum of the laser-resistant viscoelastic composition.
[0054] Figure 3 It is a characterization spectrum of the weight average molecular weight of the anti-laser viscoelastic composition.
[0055] Figure 4 Schematic diagram of rheological properties-shear viscosity of anti-laser viscoelastic composition.
[0056] Figure 5 Schematic diagram of the rheological properties - absolute complex viscosity of the laser-resistant viscoelastic composition. DETAILED DESCRIPTION
[0057] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the drawings of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0058] Combine the following Figure 1-Figure 5 Various specific embodiments of the present invention are described.
[0059] Example 1
[0060] This embodiment provides a laser-proof viscoelastic composition, the formula of which is as follows (add sterile water for injection to 98 g): 0.50 g disodium hydrogen phosphate, 0.45 g sodium dihydrogen phosphate, 0.15 g sodium chloride, 2 g glycerol, 6.82*10 -6 mol / L of HMWHA with a molecular weight of 2200KDa, 2.08*10 -6 mol / L of MMWHA with a molecular weight of 1200KDa and 4.17*10 -4mol / L LMWHA with a molecular weight of 6KDa, 0.0015g aniline brown: This is achieved by adding 1.5g of pre-dispersion liquid and then vacuum drying to remove ethanol. The pre-dispersion liquid is prepared by pre-dispersing 0.006g of aniline brown with 1000 times the mass of ethanol.
[0061] This embodiment also provides a method for preparing the above-mentioned anti-laser viscoelastic composition, which specifically includes: Weigh 0.50 g of disodium hydrogen phosphate, 0.45 g of sodium dihydrogen phosphate, 0.15 g of sodium chloride, and 2 g of glycerol, dissolve them in sterile water for injection to 98 g, mix them evenly, and filter and sterilize them to obtain a buffer solution; weigh 0.006 g of aniline brown, disperse it in 1000 times the mass of ethanol in advance, filter and remove impurities to obtain a pre-dispersion solution; take 1.5 g of the pre-dispersion solution in step 2 and add it to the buffer solution obtained in step 1, vacuum dry it at 40°C for 10 minutes to remove ethanol, and then add 6.82*10 -6 mol / L of HMWHA with a molecular weight of 2200KDa, 2.08*10 -6 mol / L of MMWHA with a molecular weight of 1200KDa and 4.17*10 -4 mol / L of LMWHA with a molecular weight of 6KDa, and mix them evenly to obtain an anti-laser composition; then fill 1.0mL into a prefilled syringe and sterilize with wet heat to obtain a mixed anti-laser viscoelastic agent. After testing, the anti-laser viscoelastic composition prepared in this embodiment has a pH of 7.12 and an osmotic pressure of 335 mOsmol / kg.
[0062] The implementation process of the remaining embodiments and comparative examples is the same as that of Example 1. The component parameters of each embodiment and comparative example are shown in Tables 2 and 3: Table 2 Component parameters
[0063] Among them, the molecular weight of the high molecular weight sodium hyaluronate HMWHA raw material is 2200KDa, the molecular weight of the medium molecular weight sodium hyaluronate MMWHA raw material is 1200KDa, and the molecular weight of the low molecular weight sodium hyaluronate LMWHA raw material is 6KDa.
[0064] Table 3 Component parameters
[0065] Among them, the molecular weight of the high molecular weight sodium hyaluronate HMWHA raw material is 2000KDa, the molecular weight of the medium molecular weight sodium hyaluronate MMWHA raw material is 1000KDa, and the molecular weight of the low molecular weight sodium hyaluronate LMWHA raw material is 10KDa.
[0066] The performance test data of the anti-laser viscoelastic compositions obtained in Examples 1-8 and Comparative Examples 1-2 are shown in Table 4. The performance test data of the anti-laser viscoelastic compositions obtained in Examples 9-15 are shown in Table 5.
[0067] Table 4 Performance summary
[0068] Table 5 Performance summary
[0069] It can be seen from Table 4 that after adding aniline brown or transparent green anti-laser dye, although the transmittance in the visible light region (represented by 660nm) is lower than that of the control group, the decrease does not exceed 7%, and the solution is clear visually, which does not affect the surgical field of view; at 300-450nm and / or 800-110nm, the transmittance is below 70%, and at 1064nm, which is commonly used in ophthalmic surgery, the transmittance of the control example is 100.3% and 100.0%, respectively, while the transmittance of Examples 1-8 is 20%-50%, a decrease of 50%-80%, indicating that the added anti-laser dye can effectively absorb at the wavelength of 1064nm corresponding to the commonly used laser surgery in ophthalmic surgery, and protect the laser energy from damage to the intraocular tissue.
[0070] Test Example 1
[0071] The performance of the anti-laser viscoelastic agent obtained in the comparative examples of the above embodiments was tested and analyzed, and the results are as follows: 1. The anti-laser viscoelastic composition prepared by the method of the present invention has the characteristics of color development without staining. After being immersed in physiological saline for 15 minutes, the viscoelastic composition is still in a color development state, and an obvious gel-water interface can be seen, and the anti-laser dye does not overflow. Figure 1 As shown, Figure 1 a is the sample of Example 1, the lower layer is a light orange-yellow clear gel, and the upper layer is physiological saline; Figure 1 b is the sample of comparative example 1, the lower layer is colorless clear gel, and the upper layer is physiological saline; Figure 1 c is the sample of Example 2, the lower layer is light green gel, and the upper layer is physiological saline. This indicates that the dye of the composition is evenly and stably dispersed in the composition, and the dye will not migrate to adjacent tissues when used in a short period of time during surgical operations. The depth of the color of the composition is related to the proportion of the dye in the formula.
[0072] 2. The UV-Vis-NIR spectrum of the anti-laser viscoelastic agent obtained in Example 1 is as follows: Figure 2As shown in the curve, compared with Comparative Example 1, the absorbance at 660nm is basically the same, indicating that the viscoelastic agent prepared by the present invention has similar light transmittance to Comparative Example 1 and Comparative Example 2 under visible light, and will not affect the surgical field of view; the transmittance at a laser wavelength of 300-450nm is 30%-40%; in the 800-1100nm band, it is a wide-spectrum anti-laser dye, which has a certain absorption in the entire band, and the overall transmittance is below 70%; in particular, the transmittance at 1064nm, a laser commonly used in ophthalmic surgery, is significantly lower than that of Comparative Example 1 and Comparative Example 2, and the transmittance is 40.7%; It shows that the viscoelastic agent prepared by the present invention has a good laser protection effect, and the transmittance at 1064nm is 59.3% lower than that of Comparative Example 1 and Comparative Example 2 (respectively 100.29% and 100.01%, calculated as 100%), indicating that it has laser protection against nitrogen lasers, neodymium-yttrium aluminum garnet lasers, etc.
[0073] The UV-Vis-NIR spectrum of the laser-resistant viscoelastic agent obtained in Example 2 is as follows: Figure 2 As shown in the curve, compared with Comparative Example 2, the absorbance at 660nm is basically the same, indicating that the viscoelastic agent prepared by the present invention has similar light transmittance to Comparative Examples 1 and 2 under visible light, and will not affect the surgical field of view; the transmittance at a laser wavelength of 300-450nm is 0-15%; the transmittance at a laser wavelength of 450-500nm is 0-30%; in the 800-1100nm band, it is a wide-spectrum anti-laser dye, which has a certain absorption in the entire band, and the overall transmittance is The light transmittance is below 80%; in particular, the light transmittance at 1064nm of the laser commonly used in ophthalmic surgery is significantly lower than that of Comparative Examples 1 and 2, and the light transmittance is 45.9%; this indicates that the viscoelastic agent prepared in the present invention has a good laser protection effect, and the light transmittance at 1064nm is 54.1% lower than that of Comparative Examples 1 and 2 (100.3% and 100.0%, respectively, calculated as 100%), indicating that it has a laser protection effect on nitrogen laser, argon laser, neodymium-yttrium aluminum garnet laser, etc.
[0074] 3. The weight average molecular weight and molecular weight distribution data of the anti-laser viscoelastic agent obtained in Example 1 were tested, and the results were as follows: Figure 3 As shown, it can be seen that no matter it is the laser signal or the differential signal, three peak segments can be clearly observed. PEAK 1, PEAK 2 and PEAK 3 are the peaks corresponding to HMWHA, MMWHA, and LMWHA, respectively, which characterize the composition of three different molecular weight sodium hyaluronates in the anti-laser viscoelastic agent. The test results show that the component peaks of three different molecular weights can be separated and independently calculated for molecular weight characterization. The combined use of sodium hyaluronates with different molecular weights gives the composition the characteristics of small molecule sodium hyaluronate's anti-inflammatory and good coating protection and large molecule sodium hyaluronate's moisturizing and good support.
[0075] 4. The rheological properties of the anti-laser viscoelastic composition obtained in Example 1 are shown in Figure 4 and Figure 5 It can be seen that in this embodiment 1, the anti-laser viscoelastic agent -1 The shear viscosity is 67.8 Pa·s, and the absolute complex viscosity at 0.1 Hz is 60.3 Pa·s. The low viscosity at high shear viscosity facilitates the movement of surgical instruments and surgical devices, and the injection of the composition into relevant use sites, such as the anterior chamber of the eye, through a syringe, etc.; the moderate viscosity at low shear viscosity indicates that the composition can have both support and surface coating properties when used, and has a protective effect on the use site.
[0076] 5. In order to enable the dye to be added to the viscoelastic composition quickly, uniformly and stably, in addition to the design of adding a cosolvent to the buffer system, the dye is creatively pre-dispersed with ethanol in the pre-dispersion stage, and the ethanol is removed by vacuum drying after adding the buffer solution. This operation is conducive to pre-dispersing the dye and then adding it uniformly to the buffer system for rapid dispersion and dissolution; the ethanol solvent is then removed by vacuum drying to avoid irritation of the ethanol solvent to the use site; and this operation and the use of the cosolvent enable the dye component to be stably dispersed in the composition without dye diffusion or precipitation. Comparative Example 1 and Comparative Example 2 respectively implement two operations of adding ethanol and then vacuum drying and not adding ethanol, which have no effect on the performance of the final viscoelastic agent.
[0077] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A laser-proof viscoelastic composition, characterized in that: The viscoelastic composition comprises a rheologically active component, an anti-laser dye and a cosolvent; the light transmittance of the anti-laser viscoelastic composition at a visible light wavelength of 550-675 nm is above 90%, and the light transmittance at a wavelength of 300-450 nm and / or 800-1100 nm is below 70%.
2. The laser-proof viscoelastic composition according to claim 1, characterized in that: The transmittance at 800-1100nm laser wavelength is 8%-70%; or, the transmittance at 800-1070nm laser wavelength is 8%-50%; Preferably, the transmittance at a laser wavelength of 1000±10nm is less than 10%; Preferably, the transmittance at a specific laser wavelength of 1060-1068 nm is 40%-45%, and more preferably, the transmittance at a characteristic laser wavelength of 1064 nm is reduced by 50%-70%; Preferably, the transmittance at a laser wavelength of 300-450 nm is less than 40%; and / or the transmittance at a laser wavelength of 450-500 nm is 0-30%.
3. The laser-proof viscoelastic composition according to claim 1 or 2, characterized in that: The anti-laser dye is an azo dye, and the transmittance at a laser wavelength of 300-450nm is 30%-40%; and / or the anti-laser dye is a quinone dye, and the transmittance at a laser wavelength of 300-450nm is 0-15%.
4. The laser-proof viscoelastic composition according to claim 1 or 2, characterized in that: In 1s -1 The lower shear viscosity is 10-120 Pa·s, and / or the absolute complex viscosity at 0.1 Hz is 10-120 Pa·s.
5. A laser-proof viscoelastic composition, characterized in that: Include: The molar ratio is 2.5*10 -6 ~6*10 -3 mol / L of rheologically active ingredients; Anti-laser dye with a mass content of 0.0001~0.05%; Solvent; pH buffers; Osmotic pressure regulators; Preferably, the rheologically active ingredient is selected from one or more of sodium hyaluronate, sodium hydroxymethylcellulose, and chondroitin sulfate; more preferably sodium hyaluronate; the sodium hyaluronate is selected from two or three of LMWHA with a low molecular weight of 5 to 100 KDa (inclusive), MMWHA with a medium molecular weight of 100 to 2000 KDa (inclusive), and HMWHA with a high molecular weight of 2000 to 4000 KDa (inclusive); Preferably, the molar proportion of sodium hyaluronate in the viscoelastic composition is 2.5*10 -6 ~6*10 -3 mol / L, more preferably 1.5*10 -5 ~1.0*10 -4 mol / L; It is particularly preferred that the molar ratio of LMWHA in the sodium hyaluronate is 0 to 10 -3 mol / L, the molar proportion of MMWHA is 0~1.5*10 -4 mol / L; the molar proportion of HMWHA is 0~1.4*10 -5 mol / L; Preferably, the anti-laser dye is selected from one or more of quinone dyes, azo dyes, and cyanine dyes; more preferably, the quinone dye is one or more of 2-hydroxy-1,4-naphthoquinone, anthraquinone dye alizarin green and transparent green 5B, the azo dye is one or more of azobenzene, disperse yellow 7, and aniline brown, and the cyanine dye is one or more of 3H-indole ketoacid cyanine dyes, quinaldine ketoacid cyanine dyes, and 4-tetranitrophthalocyanine copper dyes; particularly preferably, the anti-laser dye is transparent green 5B or aniline brown; Preferably, the mass content of the anti-laser dye is 0.0001-0.05% of the anti-laser viscoelastic composition; more preferably, it is 0.001-0.01% of the anti-laser viscoelastic composition, and particularly preferably, it is 0.002-0.006%.
6. The laser-resistant viscoelastic composition according to claim 5, characterized in that: The cosolvent is selected from one or more of propylene glycol, glycerol, mannitol, P188, RH40, and cocamidopropyl betaine, preferably propylene glycol or glycerol; more preferably, the proportion of the cosolvent in the anti-laser viscoelastic composition is 0.5-5%, and particularly preferably 1-3%; Preferably, the pH buffer is selected from one or more of boric acid / borax, disodium hydrogen phosphate / sodium dihydrogen phosphate, citric acid / sodium citrate, and aminocaproic acid; more preferably, the pH buffer is disodium hydrogen phosphate / sodium dihydrogen phosphate, and particularly preferably, disodium hydrogen phosphate / sodium dihydrogen phosphate in a dosage ratio of 2:1-15:1; Preferably, the total amount of the pH buffer in the anti-laser viscoelastic composition does not exceed 1%; more preferably 0.35% to 0.6%; particularly preferably 0.385% to 0.545%; Preferably, the pH value of the laser-proof viscoelastic composition is 6.0-8.0, more preferably 6.8-7.6, and particularly preferably 7.1-7.
3.
7. The laser-proof viscoelastic composition according to claim 5 or 6, characterized in that: The osmotic pressure of the laser-proof viscoelastic composition is 270-500 mOsmol / kg, preferably 280-360 mOsmol / kg.
8. The laser-proof viscoelastic composition according to any one of claims 5 to 7, characterized in that: The osmotic pressure regulator is selected from one or more of sodium chloride, potassium chloride, calcium chloride, and magnesium chloride, preferably sodium chloride; Preferably, the ratio of the osmotic pressure regulator to the laser-proof viscoelastic composition is 0.1-0.5%, more preferably 0.1-0.3%, and particularly preferably 0.15%-0.2%.
9. The method for preparing the laser-resistant viscoelastic composition according to any one of claims 1 to 8, characterized in that: include: The anti-laser dye is pre-dispersed with a dispersant, then added into a buffer solution containing a cosolvent, an osmotic pressure regulator, and a pH buffer, then the dispersant is removed by vacuum drying, and finally the rheological active component is added and mixed evenly; Preferably, the dispersant is selected from ethanol, n-propanol, and isopropanol; more preferably, the mass ratio of the anti-laser dye in the dispersant is 1:1000 to 1:10000, and particularly preferably, the mass ratio is 1:1000 to 1:5000; Preferably, the vacuum drying is vacuum drying at 40°C for 10-30 min, vacuum drying at 30°C for 20-30 min, or vacuum drying at 50°C for 10-30 min.
10. Use of the anti-laser viscoelastic composition according to any one of claims 1 to 8 in laser surgery, especially in ophthalmic laser surgery; Preferably, the ophthalmic surgery includes intracapsular cataract extraction, phacoemulsification, keratoplasty, intraocular lens implantation and removal, iridotomy, anterior chamber hemorrhage surgery, foreign body and tumor removal, trabeculectomy, vitrectomy or foreign body removal, retinal detachment and epiretinal membrane removal surgery, glaucoma, diabetic retinopathy, and femtosecond laser surgery.
Citation Information
Patent Citations
Preparation method of ophthalmological viscoelastic agent with selective anterior capsule staining function
CN105903088A
Viscoelastic agent for ophthalmology
CN108578789A
Near infrared light-cutting optical articles with low residual color
CN109844620A
Production method of anti-laser aviation goggle laser protection material
CN112390538A
Laser radiation-absorbing composition and its use
DE102018122838A1