Urea hydrolysis catalyst and preparation method thereof

Through the combination method of high purity phosphate and Mn-Ce/TiO2 and Mn-Co/TiO2 catalysts, the problems of high urea hydrolysis reaction temperature and large energy consumption are solved, and the urea hydrolysis reaction rate and energy saving are improved. Denitrification treatment of flue gas in thermal power plants.

CN118988360APending Publication Date: 2024-11-22BEIJING LIANFA MAITONG TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411304902.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing urea hydrolysis catalysts have problems such as high reaction temperature, large energy consumption and slow reaction rate in flue gas denitrition treatment in thermal power plants, and the preparation method is complex and the cost is high.

Method used

The combination method of high-purity phosphate, Mn-Ce/TiO2 catalyst and Mn-Co/TiO2 catalyst is adopted to achieve sufficient dispersion and fusion of raw material components through drying and stirring, reduce the urea hydrolysis reaction temperature and increase the reaction rate.

Benefits of technology

It significantly reduces the urea hydrolysis reaction temperature, improves the reaction rate, saves energy, simplifies the preparation method, reduces costs, and has small catalyst loss, is not easy to decompose, has strong corrosion resistance, and can effectively meet the nitrogen oxide emission standards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118988360A_ABST
    Figure CN118988360A_ABST
Patent Text Reader

Abstract

The invention provides a urea hydrolysis catalyst and a preparation method thereof, belongs to the technical field of flue gas denitration treatment in a thermal power plant, and solves the technical problem of potential safety hazards in a process for preparing denitration reducing agent ammonia gas from liquid ammonia water. The urea hydrolysis catalyst is prepared from the following raw material components in parts by weight: 98-99 parts of high-purity phosphate, 0.5-1 part of a Mn-Ce / TiO2 catalyst and 0.5-1 part of a Mn-Co / TiO2 catalyst, the high-purity phosphate, the Mn-Ce / TiO2 catalyst and the Mn-Co / TiO2 catalyst are compounded according to a specific proportion, and during preparation, the high-purity phosphate, the Mn-Ce / TiO2 catalyst and the Mn-Co / TiO2 catalyst are mixed in a drying and stirring manner to prepare the urea hydrolysis catalyst. The raw material components are fully dispersed and fused, under the condition that the structure and performance of the raw materials are not damaged, full fusion of the raw material components is kept, the mutual synergistic effect of the raw material components can be fully exerted in the follow-up process, complementation and enhancement of the performance are achieved, and the urea hydrolysis catalyst is prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of flue gas denitration treatment in thermal power plants, and in particular relates to a urea hydrolysis catalyst and a preparation method thereof. Background Art

[0002] Nitrogen oxides (NOX) are one of the main sources of air pollution, causing serious harm to production activities and the natural environment. The harm is mainly manifested in the following three aspects: ① NOX has direct harm to the human body; excessive inhalation of NOX can cause the body to quickly be in a state of hypoxia and suffocation, causing brain damage, central nervous system paralysis and spasm; ② NOX has indirect harm to the human body; when NOX and hydrocarbons (HC) coexist in the atmosphere, photochemical reactions occur under the irradiation of ultraviolet rays to generate highly toxic photochemical smog; photochemical smog causes symptoms such as eye and throat pain, coughing, chills, breathing difficulties, numbness and spasm, and loss of consciousness in the human body, and the mortality rate is greatly increased; ③ NOX has great harm to the ecological environment; NOX can react with water in the atmosphere to generate nitric acid and form acid rain. In view of the severity of NOX pollution to the air, it is urgent to develop denitrification technology for industrial combustion exhaust.

[0003] Common methods of flue gas denitrification (nitrogen oxides) in thermal power plants include selective catalytic reduction (SCR), selective non-catalytic reduction (SNCR), decomposition, adsorption, plasma activation and biochemical methods. Selective catalytic reduction denitrification (SCR) is widely used for its mature technology and good denitrification effect. It is currently a commonly used method for reducing nitrogen oxides in developed thermal power generation units. The reducing agent ammonia (NH3) for SCR denitrification can be obtained from liquid ammonia (NH3), ammonia water (NH4OH), urea (CO (NH2) and other raw materials. The process of using liquid ammonia or ammonia water to produce denitrification reducing agent ammonia is the simplest and most mature, with the lowest operating cost, but there are safety hazards. The investment and operating costs of the urea ammonia production system are higher than those of the liquid ammonia system, and the transportation cost is comparable, but the urea system basically has no safety hazards and is the safest ammonia preparation technology.

[0004] Urea ammonia production technology is divided into urea thermal decomposition ammonia production technology and urea hydrolysis ammonia production technology. Urea hydrolysis ammonia production technology is divided into ordinary urea hydrolysis ammonia production technology and urea catalytic hydrolysis ammonia production technology. Among them, urea catalytic hydrolysis ammonia production technology refers to: under the action of a catalyst, the molten urea is subjected to a rapid hydrolysis reaction at a temperature of 135-150°C and a pressure of about 0.4-0.55MPa. Urea catalytic hydrolysis to ammonia is an endothermic reaction, and its comprehensive reaction formula is: (NH2)2CO+H2O=CO2↑+2NH3↑. The role of urea hydrolysis catalyst is to change the reaction path, accelerate the reaction rate, and reduce the response time. Its catalytic reaction speed is about 10 times higher than that of ordinary urea hydrolysis method, and the response time can be less than 1min, and the energy consumption is about half of that of thermal decomposition technology. Therefore, it is of great significance to study efficient urea hydrolysis catalysts. Summary of the invention

[0005] The purpose of the present invention is to solve the defects of the above-mentioned prior art and provide a urea hydrolysis catalyst and its preparation method which are simple and easy to prepare, significantly improve the urea hydrolysis reaction rate, and reduce the reaction temperature of the urea hydrolysis reactor.

[0006] The purpose of the present invention can be achieved by adopting the following technical scheme: the urea hydrolysis catalyst of the present invention comprises the following raw material components by weight: 98-99 parts of high-purity phosphate, 0.5-1 parts of Mn-Ce / TiO2 catalyst, and 0.5-1 parts of Mn-Co / TiO2 catalyst; the high-purity phosphate is one or both of diammonium hydrogen phosphate and ammonium dihydrogen phosphate.

[0007] Preferably, the preparation method of the Mn-Ce / TiO2 catalyst comprises the following steps:

[0008] Take a certain amount of Mn(CH3COO)2, Ce(NO3)3, TiO2 and water, dissolve the weighed Mn(CH3COO)2 and Ce(NO3)3 in water; then, add the weighed TiO2 solid powder to load Ce and Mn on the carrier TiO2: after heating and stirring thoroughly, let it stand at room temperature, dry it, and calcine it at 600℃ for 5-6h to obtain Mn-Ce / TiO2 catalyst.

[0009] Preferably, the mass ratio of the added amounts of Mn(CH3COO)2, Ce(NO3)3 and TiO2 is Mn(CH3COO)2:Ce(NO3)3:TiO2=86:184:80.

[0010] Preferably, the ratio of the volume (ml) of water to be added to the mass (g) of TiO2 weighed is 1:1.2.

[0011] Preferably, Ce and Mn are loaded on the carrier TiO2 by the following specific operations: heating and stirring for 2 hours, standing at room temperature for 6 hours, drying at 125°C for 8 hours, and calcining at 600°C for 5-6 hours.

[0012] Preferably, the preparation method of the Mn-Co / TiO2 catalyst comprises the following steps:

[0013] Take a certain amount of Mn(CH3COO)2, Co(NO3)3, TiO2 and water, dissolve the weighed Mn(CH3COO)2 and Co(NO3)3 in water; then, add the weighed TiO2 solid powder to load Mn and Co on the carrier TiO2: after sufficient heating and stirring, let it stand at room temperature, dry it, and calcine it at 500℃ for 5-6h to obtain Mn-Co / TiO2 catalyst.

[0014] Preferably, the mass ratio of the added amounts of Mn(CH3COO)2, Co(NO3)3 and TiO2 is Mn(CH3COO)2:Co(NO3)3:TiO2=86:143:80.

[0015] Preferably, the ratio of the volume of water added (ml) to the weighed mass of TiO2 (g) is 1:1.3.

[0016] Preferably, Mn and Co are loaded on the carrier TiO2: heating and stirring for 2 hours, standing at room temperature for 6 hours, drying at 120°C for 6 hours, and calcining at 500°C for 5-6 hours to obtain a Mn-Co / TiO2 catalyst.

[0017] The preparation method of the urea hydrolysis catalyst comprises stirring and mixing the Mn-Co / TiO2 catalyst, the Mn-Ce / TiO2 catalyst and high-purity phosphate at room temperature.

[0018] Compared with the prior art, the embodiments of the present invention mainly have the following beneficial effects:

[0019] (1) The urea hydrolysis catalyst of the present invention is compounded with high-purity phosphate, Mn-Ce / TiO2 catalyst and Mn-Co / TiO2 catalyst in specific proportions. During preparation, the raw material components are fully dispersed and fused by drying and stirring, and the raw material components are fully fused without damaging the raw material structure and performance, so that the synergistic effect between the raw material components can be fully exerted in the subsequent process, and the performance complementarity and enhancement can be achieved, thereby preparing the urea hydrolysis catalyst.

[0020] The urea hydrolysis catalyst is used for the treatment of flue gas denitrification (nitrogen oxides) in thermal power plants, and the treated flue gas can directly meet the emission standards.

[0021] (2) The catalyst provided by the present invention can effectively reduce the hydrolysis temperature of urea, especially urea used for denitrification of industrial combustion exhaust gas, reduce energy consumption, and save energy; and further increase the hydrolysis rate of urea. The preparation method is simple, the raw materials are easy to obtain and the cost is low, and it can be promoted and applied in industry; compared with liquid catalysts, the loss is small, there is no effect on the reaction waste liquid, it is not easy to decompose and produce side reactions, and it has a certain corrosion resistance.

[0022] The reactor is filled with a fixed amount of catalyst, which can be recycled in the reactor and replaced during the overhaul period. In order to keep the reaction rate constant, urea, water and heat must be supplied to the reactor in the correct proportion. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The present invention is a flow chart of a urea catalytic hydrolysis device using a urea hydrolysis catalyst. DETAILED DESCRIPTION

[0024] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, a urea removal hydrolysis catalyst and a preparation method thereof are further described in detail below in conjunction with embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0025] Example 1

[0026] The method for preparing a urea hydrolysis catalyst comprises the following steps:

[0027] Calculated by weight, the raw material components include: 98 parts of high-purity phosphate - diammonium hydrogen phosphate, 1 part of Mn-Ce / TiO2 catalyst, and 1 part of Mn-Co / TiO2 catalyst.

[0028] Preparation of S1, Mn-Ce / TiO2 catalyst:

[0029] Take a certain amount of Mn(CH3COO)2, Ce(NO3)3, TiO2 and water, the mass ratio of Mn(CH3COO)2, Ce(NO3)3 and TiO2 added is Mn(CH3COO)2:Ce(NO3)3:TiO2=86:184:80, the ratio of water volume (ml) to TiO2 mass (g) is 1:1.2, dissolve the weighed Mn(CH3COO)2 and Ce(NO3)3 in water. Then, add weighed TiO2 solid powder so that Ce and Mn are loaded on the carrier TiO2, heat and stir for 2h, stand at room temperature for 6h, dry at 125℃ for 8h, and calcine at 600℃ for 5h to obtain Mn-Ce / TiO2 catalyst.

[0030] Preparation of S2, Mn-Co / TiO2 catalysts:

[0031] Take a certain amount of Mn(CH3COO)2, Co(NO3)3, TiO2 and water. The mass ratio of Mn(CH3COO)2, Co(NO3)3 and TiO2 is Mn(CH3COO)2:Co(NO3)3:TiO2=86:143:80. The ratio of the added water volume (ml) to the mass of TiO2 (g) is 1:1.3. Dissolve the weighed Mn(CH3COO)2 and Co(NO3)3 in water. Then, add the weighed TiO2 solid powder so that Mn and Co are loaded on the carrier TiO2. Heat and stir for 2h, let stand for 6h at room temperature, dry at 120℃ for 6h, and calcine at 500℃ for 5h to obtain Mn-Co / TiO2 catalyst.

[0032] S3. Preparation of urea hydrolysis catalyst:

[0033] The Mn-Co / TiO2 catalyst prepared in step S2, the Mn-Ce / TiO2 catalyst prepared in step S1 and high-purity phosphate, diammonium hydrogen phosphate, are stirred at 25°C at a speed of 115 r / min for 60 minutes to prepare a urea hydrolysis catalyst.

[0034] Example 2

[0035] The method for preparing a urea hydrolysis catalyst comprises the following steps:

[0036] Calculated by weight, the raw material components include: 99 parts of high-purity phosphate - diammonium phosphate, 0.5 parts of Mn-Ce / TiO2 catalyst, and 0.5 parts of Mn-CO / TiO2 catalyst.

[0037] Preparation of S1, Mn-Ce / TiO2 catalyst:

[0038] Take a certain amount of Mn(CH3COO)2, Ce(NO3)3, TiO2 and water, the mass ratio of Mn(CH3COO)2, Ce(NO3)3 and TiO2 added is Mn(CH3COO)2:Ce(NO3)3:TiO2=86:184:80, the ratio of water volume (ml) to TiO2 mass (g) is 1:1.2, dissolve the weighed Mn(CH3COO)2 and Ce(NO3)3 in water. Then, add weighed TiO2 solid powder so that Ce and Mn are loaded on the carrier TiO2, heat and stir for 2h, stand at room temperature for 6h, dry at 125℃ for 8h, and calcine at 600℃ for 5h to obtain Mn-Ce / TiO2 catalyst.

[0039] Preparation of S2, Mn-Co / TiO2 catalysts:

[0040] Take a certain amount of Mn(CH3COO)2, Co(NO3)3, TiO2 and water. The mass ratio of Mn(CH3COO)2, Co(NO3)3 and TiO2 is Mn(CH3COO)2:Co(NO3)3:TiO2=86:143:80. The ratio of the added water volume (ml) to the mass of TiO2 (g) is 1:1.3. Dissolve the weighed Mn(CH3COO)2 and Co(NO3)3 in water. Then, add the weighed TiO2 solid powder so that Mn and Co are loaded on the carrier TiO2. Heat and stir for 2h, let stand for 6h at room temperature, dry at 120℃ for 6h, and calcine at 500℃ for 5h to obtain Mn-Co / TiO2 catalyst.

[0041] S3. Preparation of urea hydrolysis catalyst:

[0042] The Mn-Co / TiO2 catalyst prepared in step S2, the Mn-Ce / TiO2 catalyst prepared in step S1 and high-purity phosphate, diammonium hydrogen phosphate, are stirred at 25°C at a speed of 115 r / min for 60 minutes to prepare a urea hydrolysis catalyst.

[0043] Example 3

[0044] The method for preparing a urea hydrolysis catalyst comprises the following steps:

[0045] Calculated by weight, the raw material components include: 99 parts of high-purity phosphate - diammonium hydrogen phosphate, 0.5 parts of Mn-Ce / TiO2 catalyst, and 0.5 parts of Mn-Co / TiO2 catalyst.

[0046] Preparation of S1, Mn-Ce / TiO2 catalyst:

[0047] Take a certain amount of Mn(CH3COO)2, Ce(NO3)3, TiO2 and water, the mass ratio of Mn(CH3COO)2, Ce(NO3)3 and TiO2 added is Mn(CH3COO)2:Ce(NO3)3:TiO2=86:184:80, the ratio of water volume (ml) to TiO2 mass (g) is 1:1.2, dissolve the weighed Mn(CH3COO)2 and Ce(NO3)3 in water. Then, add weighed TiO2 solid powder so that Ce and Mn are loaded on the carrier TiO2, heat and stir for 2h, stand at room temperature for 6h, dry at 125℃ for 8h, and calcine at 600℃ for 5h to obtain Mn-Ce / TiO2 catalyst.

[0048] Preparation of S2, Mn-Co / TiO2 catalysts:

[0049] Take a certain amount of Mn(CH3COO)2, Co(NO3)3, TiO2 and water. The mass ratio of Mn(CH3COO)2, Co(NO3)3 and TiO2 is Mn(CH3COO)2:Co(NO3)3:TiO2=86:143:80. The ratio of the added water volume (ml) to the mass of TiO2 (g) is 1:1.3. Dissolve the weighed Mn(CH3COO)2 and Co(NO3)3 in water. Then, add the weighed TiO2 solid powder so that Mn and Co are loaded on the carrier TiO2. Heat and stir for 2h, let stand for 6h at room temperature, dry at 120℃ for 6h, and calcine at 500℃ for 5h to obtain Mn-Co / TiO2 catalyst.

[0050] S3. Preparation of urea hydrolysis catalyst:

[0051] The Mn-Co / TiO2 catalyst prepared in step S2, the Mn-Ce / TiO2 catalyst prepared in step S1 and high-purity phosphate, diammonium hydrogen phosphate, are stirred at 25°C at a speed of 115 r / min for 60 minutes to prepare a urea hydrolysis catalyst.

[0052] Example 4

[0053] The method for preparing a urea hydrolysis catalyst comprises the following steps:

[0054] Calculated by weight, the raw material components include: high-purity phosphate - 44 parts of diammonium phosphate and 44 parts of diammonium hydrogen phosphate, 1 part of Mn-Ce / TiO2 catalyst, and 1 part of Mn-Co / TiO2 catalyst.

[0055] Preparation of S1, Mn-Ce / TiO2 catalyst:

[0056] Take a certain amount of Mn(CH3COO)2, Ce(NO3)3, TiO2 and water, the mass ratio of Mn(CH3COO)2, Ce(NO3)3 and TiO2 added is Mn(CH3COO)2:Ce(NO3)3:TiO2=86:184:80, the ratio of water volume (ml) to TiO2 mass (g) is 1:1.2, dissolve the weighed Mn(CH3COO)2 and Ce(NO3)3 in water. Then, add weighed TiO2 solid powder so that Ce and Mn are loaded on the carrier TiO2, heat and stir for 2h, stand at room temperature for 6h, dry at 125℃ for 8h, and calcine at 600℃ for 5h to obtain Mn-Ce / TiO2 catalyst.

[0057] Preparation of S2, Mn-Co / TiO2 catalysts:

[0058] Take a certain amount of Mn(CH3COO)2, Co(NO3)3, TiO2 and water. The mass ratio of Mn(CH3COO)2, Co(NO3)3 and TiO2 is Mn(CH3COO)2:Co(NO3)3:TiO2=86:143:80. The ratio of the added water volume (ml) to the mass of TiO2 (g) is 1:1.3. Dissolve the weighed Mn(CH3COO)2 and Co(NO3)3 in water. Then, add the weighed TiO2 solid powder so that Mn and Co are loaded on the carrier TiO2. Heat and stir for 2h, let stand for 6h at room temperature, dry at 120℃ for 6h, and calcine at 500℃ for 5h to obtain Mn-Co / TiO2 catalyst.

[0059] S3. Preparation of urea hydrolysis catalyst:

[0060] The Mn-Co / TiO2 catalyst prepared in step S2, the Mn-Ce / TiO2 catalyst prepared in step S1 and high-purity phosphate, diammonium hydrogen phosphate, are stirred at 25°C at a speed of 115 r / min for 60 minutes to prepare a urea hydrolysis catalyst.

[0061] Comparative Example 1

[0062] The method for preparing a urea hydrolysis catalyst comprises the following steps:

[0063] Calculated by weight, the raw material components include: 90 parts of high-purity phosphate - diammonium phosphate, 5 parts of Mn-Ce / TiO2 catalyst, and 5 parts of Mn-Co / TiO2 catalyst.

[0064] Preparation of S1, Mn-Ce / TiO2 catalyst:

[0065] Take a certain amount of Mn(CH3COO)2, Ce(NO3)3, TiO2 and water, the mass ratio of Mn(CH3COO)2, Ce(NO3)3 and TiO2 added is Mn(CH3COO)2:Ce(NO3)3:TiO2=86:184:80, the ratio of water volume (ml) to TiO2 mass (g) is 1:1.2, dissolve the weighed Mn(CH3COO)2 and Ce(NO3)3 in water. Then, add weighed TiO2 solid powder so that Ce and Mn are loaded on the carrier TiO2, heat and stir for 2h, stand at room temperature for 6h, dry at 125℃ for 8h, and calcine at 600℃ for 5h to obtain Mn-Ce / TiO2 catalyst.

[0066] Preparation of S2, Mn-Co / TiO2 catalysts:

[0067] Take a certain amount of Mn(CH3COO)2, Co(NO3)3, TiO2 and water. The mass ratio of Mn(CH3COO)2, Co(NO3)3 and TiO2 is Mn(CH3COO)2:Co(NO3)3:TiO2=86:143:80. The ratio of the added water volume (ml) to the mass of TiO2 (g) is 1:1.3. Dissolve the weighed Mn(CH3COO)2 and Co(NO3)3 in water. Then, add the weighed TiO2 solid powder so that Mn and Co are loaded on the carrier TiO2. Heat and stir for 2h, let stand for 6h at room temperature, dry at 120℃ for 6h, and calcine at 500℃ for 5h to obtain Mn-Co / TiO2 catalyst.

[0068] S3. Preparation of urea hydrolysis catalyst:

[0069] The Mn-Co / TiO2 catalyst prepared in step S2, the Mn-Ce / TiO2 catalyst prepared in step S1 and high-purity phosphate, diammonium hydrogen phosphate, are stirred at 25°C at a speed of 115 r / min for 60 minutes to prepare a urea hydrolysis catalyst.

[0070] The actual application performance results of the urea hydrolysis catalyst prepared by the present invention are analyzed as follows:

[0071] Verification Test 1

[0072] The urea hydrolysis catalyst prepared by Example 1 of the present invention is used in China Resources Power (Jinzhou) Branch Figure 1 The urea catalytic hydrolysis unit shown in the figure is being tested. The daily operating liquid level of the hydrolysis reactor in this plant is 750mm, and the corresponding volume is 5.3m 3 According to this volume calculation, 2.5 tons of catalyst is required. The normal configuration reactor contains 340mm catalyst solution, 230mm desalted water, and 180mm urea solution. According to this configuration ratio, urea solution accounts for 24%.

[0073] Usage process:

[0074] (1) Prepare the catalyst solution while preparing the urea solution to prevent the catalyst and urea from being oversaturated and difficult to dissolve in the desalted water. Reduce the proportion of the urea solution from 50% to 40% (originally 1 ton of desalted water was used to prepare 1 ton of urea, now 1 ton of desalted water is used to prepare 0.8 tons of urea and 50 kilograms of catalyst). The catalyst accounts for 5% of the mixed solution.

[0075] (2) When the mixed solution is prepared for the first time, a maximum of 10 tons of the mixed solution is prepared. No abnormality occurs after the mixed solution is transported to the reactor. After the 10 tons of mixed solution are fully transported, the second preparation is carried out, and the catalyst preparation ratio can be adjusted to 10% (4 bags of catalyst).

[0076] (3) When the mixed solution is delivered for the first time, the liquid level of the reactor is maintained between 600-650mm, including 350mm-400mm of desalted water and 300mm of mixed solution. At this time, the urea concentration of the reactor is 25%. If the pressure and temperature of the mixed solution reach the daily operating values ​​after being delivered to the reactor, the ammonia production does not meet the demand. At this time, the mixed solution can continue to be delivered. If the ammonia production is too large, add desalted water in time for dilution. At the same time, adjust the operating pressure and temperature according to the ammonia production.

[0077] The trial results are as follows:

[0078] Reaction mechanism Catalytic hydrolysis General hydrolysis Urea solution concentration 50% 50% Reactor temperature 135-150℃ 150-200℃ Reaction pressure 0.55Mpa >0.55Mpa Response time <5min >1h Start and stop time fast Slow By-products No by-products Load changes can easily produce high molecular solids Nitrogen oxide emission concentration Meet the Standard Occasionally exceed the standard

[0079] It can be seen from the above results that the urea hydrolysis catalyst prepared by using Example 1 of the present invention can significantly reduce the reaction temperature of the urea hydrolysis reactor, significantly increase the hydrolysis rate, reduce the response time and start-stop time of the urea hydrolysis catalyst, and ensure that the nitrogen oxide emission concentration meets the emission standards.

[0080] Verification Test 2

[0081] The urea hydrolysis catalyst prepared by Example 2 of the present invention was used in Huaneng Nanjing Jinling Power Generation Co., Ltd., and 1.8 tons of catalyst was added to each hydrolysis reactor of the plant, which can make the urea solution at a temperature of 135°C-150°C and a pressure of 0.4-0.55MPa. The trial results are as follows:

[0082]

[0083] It can be seen from the results that the use of the urea hydrolysis catalyst prepared by the present invention can significantly reduce the reaction temperature of the urea hydrolysis reactor, increase the hydrolysis rate, reduce the response time and start-stop time of the urea hydrolysis catalyst, and ensure that the nitrogen oxide emission concentration meets the emission standard. The preparation method of the urea hydrolysis catalyst of Comparative Example 1 is the same as that of Example 1, except that the component content of the high-purity phosphate is reduced, resulting in the performance of the urea hydrolysis catalyst finally prepared being significantly lower than that of the urea hydrolysis catalyst prepared in Example 1 of the present invention.

[0084] The experiments show that the urea hydrolysis catalysts prepared in Examples 1 to 4 of the present invention can effectively reduce the hydrolysis temperature of urea, reduce energy consumption, save energy, significantly increase the hydrolysis rate of urea, and no by-products are produced during use, so that the nitrogen oxide emission concentration meets the requirements.

[0085] In summary, the urea hydrolysis catalyst of the present invention can effectively reduce the hydrolysis temperature of urea, reduce energy consumption, and save energy; and further improve the hydrolysis rate of urea, the preparation method is simple, the raw materials are easy to obtain and the cost is low, and it can be promoted and applied in industry; especially the urea for denitrification of industrial combustion tail gas, compared with liquid catalysts, has small loss, no effect on reaction waste liquid, is not easy to decompose and produce side reactions, and has a certain corrosion resistance.

[0086] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the protection scope of the invention. Obviously, the described embodiments are only some embodiments of the present invention, rather than all embodiments. Based on these embodiments, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

Claims

1. A urea hydrolysis catalyst, It is characterized in that The raw material components are as follows: 98-99 parts of high-purity phosphate, Mn-Ce / TiO 2 Catalyst 0.5-1 part, Mn-Co / TiO 2 0.5 to 1 part of catalyst; the high-purity phosphate is one or both of diammonium hydrogen phosphate and ammonium dihydrogen phosphate.

2. A urea hydrolysis catalyst as claimed in claim 1, It is characterized in that The Mn-Ce / TiO 2 The method for preparing the catalyst comprises the following steps: Take a certain amount of Mn(CH 3 COO 2 、Ce(NO 3 ) 3 、TiO 2 and water, and the weighed Mn(CH 3 COO 2 and Ce(NO 3 ) 3 Dissolve in water; then, add weighed TiO 2 Solid powder, so that Ce and Mn are loaded on the carrier TiO 2 Top: After sufficient heating and stirring, the mixture was allowed to stand at room temperature, dried, and calcined at 600℃ for 5-6h to obtain Mn-Ce / TiO 2 catalyst.

3. A urea hydrolysis catalyst as claimed in claim 2, It is characterized in that Mn(CH 3 COO 2 、Ce(NO 3 ) 3 and TiO 2 The mass ratio of the added amount is Mn(CH 3 COO 2 :Ce(NO 3 ) 3 :TiO 2 =86:184:

80.

4. A urea hydrolysis catalyst as claimed in claim 2, It is characterized in that The volume of water to be added (ml) and the weighed TiO 2 The ratio of mass (g) is 1:1.

2.

5. A urea hydrolysis catalyst as claimed in claim 2, It is characterized in that Ce and Mn are loaded on the carrier TiO 2 The specific operation is: heating and stirring for 2 hours, standing at room temperature for 6 hours, drying at 125°C for 8 hours, and calcining at 600°C for 5-6 hours.

6. A urea hydrolysis catalyst as claimed in claim 2, It is characterized in that The Mn-Co / TiO 2 The method for preparing the catalyst comprises the following steps: Take a certain amount of Mn(CH 3 COO 2 、Co(NO 3 ) 3 、TiO 2 and water, and the weighed Mn(CH 3 COO 2 and Co(NO 3 ) 3 Dissolve in water; then, add weighed TiO 2 Solid powder, so that Mn and Co are loaded on the carrier TiO 2 Above: After sufficient heating and stirring, the mixture was allowed to stand at room temperature, dried, and calcined at 500℃ for 5-6h to obtain Mn-Co / TiO 2 catalyst.

7. A urea hydrolysis catalyst as claimed in claim 6, It is characterized in that Mn(CH 3 COO 2 、Co(NO 3 ) 3 and TiO 2 The mass ratio of the added amount is Mn(CH 3 COO 2 :Co(NO 3 ) 3 :TiO 2 =86:143:

80.

8. A urea hydrolysis catalyst as claimed in claim 6, It is characterized in that Volume of water to be added (ml) and weighed TiO 2 The mass (g) ratio is 1:1.

3.

9. A urea hydrolysis catalyst as claimed in claim 6, It is characterized in that Mn and Co are loaded on the carrier TiO 2 Upper: Heating and stirring for 2h, standing at room temperature for 6h, drying at 120℃ for 6h, calcining at 500℃ for 5-6h to obtain Mn-Co / TiO 2 catalyst.