Method and device for preparing fluoride glass optical fiber preform through pipe suction method
Fluoride glass fiber preforms were prepared by tube suction method. By using quartz tube molds and negative pressure suction technology, the problems of interface quality, impurity contamination and diameter uniformity of fluoride glass fiber preforms were solved, and high-quality preform preparation was achieved, reducing fiber loss and process complexity.
Patent Information
- Application Number
- CN202411247085.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-05
AI Technical Summary
Existing methods for preparing fluoride glass optical fiber preforms suffer from problems such as poor core-cladding interface quality, severe crucible contamination, uneven core diameter, and complex preparation processes.
The preparation method adopts the tube suction method, which uses negative pressure to suck up the glass raw materials of the outer cladding, inner cladding and core. The quartz tube is used as a mold and combined with annealing treatment to form a high-quality core-cladding interface, avoids contamination of impurities on the inner wall of the crucible and achieves uniform core diameter.
This method enables the fabrication of fluoride glass fiber preforms with good core-cladding interface quality, low crucible impurity contamination, and uniform core diameter, thereby reducing fiber interface loss and impurity scattering loss and simplifying the fabrication process.
Smart Images

Figure CN118993524A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of optical fiber preform preparation, and in particular relates to a method and a device for preparing a fluoride glass optical fiber preform by a tube suction method. Background Art
[0002] Fluoride glass has the advantages of low phonon energy, excellent mid-infrared transmittance, high rare earth ion solubility, etc. It is an important mid-infrared optical fiber precursor glass material. According to the different compositions of fluoride glass optical fibers, there are currently three main categories: fluorine zirconium glass optical fibers, fluorine indium glass optical fibers, and fluorine aluminum glass optical fibers:
[0003] (1) Fluorozirconium glass fiber uses ZrF4 as its main component, and its infrared absorption edge can reach 7μm, with high infrared transmittance. ZrF4 itself cannot form glass, but after adding BaF2 as a glass network modifier, rare earth elements (La), alkali metal elements (such as Na) and a small amount of AlF3 as a glass stabilizer, it can form a stable glass body. The classic composition of fluorozirconium glass fiber is: 53ZrF4-20BaF2-4LaF3-3AlF3-20NaF, that is, ZBLAN glass fiber. Studies have shown that ZBLAN glass fiber has low phonon energy (550cm -1 ), high rare earth solubility, high laser damage threshold, high fracture toughness, good chemical and thermal stability. After doping with rare earths, it can be used as a gain medium for mid-infrared fiber lasers.
[0004] (2) Fluorine-indium glass fiber is mainly composed of InF3, which is relatively complex and involves a variety of heavy metal fluorides and rare earth elements. It can form ternary, quaternary, quinary, hexavalent or even more ternary glass systems. The atomic equivalent mass is large, and the strength of the formed glass is relatively weak. Therefore, fluorine-indium glass fiber has the lowest phonon energy (510cm) among fluoride glass fibers. -1 ), infrared cutoff edge>8μm. However, due to its loose glass structure, fluorine indium glass is more susceptible to water erosion and more prone to crystallization than ZBLAN glass.
[0005] (3) Fluoroaluminum glass optical fiber is mainly composed of AlF3, and its classic composition is AYF (AlF3-MgF2-CaF2-SrF2-BaF2-YF3), which has low phonon energy (630cm -1 ) and low refractive index, the infrared cutoff edge can reach 6μm, the glass transition temperature is high, and the chemical stability is excellent, which is much better than ZBLAN glass. However, the material properties of fluorine-aluminum glass are shorter than those of ZBLAN glass and fluorine-indium glass, and it is easier to crystallize during the preparation process.
[0006] For fluoride glass optical fiber, loss is one of its most important key indicators. The quality of optical fiber preform plays an important role in the size of optical fiber loss. The factors affecting the quality of optical fiber preform mainly include core-cladding interface, oxide impurity particles, fluoride microcrystals, bubbles, hydroxyl absorption, impurity metal ions, etc. Among them, the oxide impurity particles are mainly ZrO2, which comes from the non-stoichiometric zirconium oxide fluoride formed by ZrF4 hydrate at high temperature; fluoride microcrystals come from glass crystallization, which is mainly related to the glass element composition, molding process, impurity crystallization center, etc.; hydroxyl absorption is due to the introduction of water in raw materials and atmosphere during the steps of melting, casting, and drawing optical fibers, resulting in strong absorption at 2.7μm; impurity metal ions are mainly introduced through raw materials, and metal impurities with specific absorption peaks will greatly increase the absorption loss of optical fibers. Due to the complex composition of fluoride glass, many influencing factors, and the lack of corresponding gaseous compounds, fluoride glass optical fiber preform cannot be prepared by vapor deposition like quartz optical fiber preform. The current methods for preparing fluoride glass optical fiber mainly include tube-rod method, suction injection method, spin casting method and double crucible method.
[0007] The tube-rod method is a commonly used method for making optical fiber preforms. Its main feature is that the core rod and cladding glass tube are made separately by optical grinding and polishing, and the cladding glass tube and the core rod are put together to form an optical fiber preform. The tube-rod method is easy to control the core-cladding diameter ratio, but it has extremely high requirements on the optical processing quality of the inner surface of the cladding tube and the outer surface of the core rod. The surface of the tube-rod is prone to defects such as tiny scratches and pits, and is easily contaminated by polishing materials and impurity particles in the environment. In the optical fiber drawing process, there is an air gap between the inner surface of the cladding tube and the outer surface of the core rod, which makes it easy for the air to be unable to be completely removed and is easily contaminated by environmental impurities, resulting in high interface loss. In addition, due to the existence of the surface energy of the material, glass is more likely to crystallize on the surface when softened, so the inner surface of the cladding tube and the outer surface of the core rod are also easy to crystallize when heated and softened. For fluoride glass optical fiber, this crystallization will be more serious, resulting in large interface loss of the optical fiber.
[0008] The suction injection method is a method of making optical fiber preform rods by using the suction force generated by the volume shrinkage of fluoride glass during the cooling process. When making the preform rod, the mold and the residual material cavity used to generate the shrinkage suction force are assembled, and the residual material cavity and the mold need to be preheated in advance. The molten cladding glass liquid is poured into the mold, and then the core glass liquid is poured on the cladding glass liquid. As the glass liquid cools, the volume of the glass liquid in the mold and the residual material cavity below shrinks. Since the temperature of the interface where the glass liquid contacts the mold is low and the viscosity is high, and the temperature in the center is high and the viscosity is low, the process of the cladding glass liquid flowing downward due to the volume shrinkage of the glass liquid in the residual material cavity mainly occurs in the center of the liquid column, thus forming a core-cladding structure. The biggest advantage of the suction injection method is that, unlike the tube-rod method, the casing and core rod need to be processed, so there is no problem of increased core-cladding interface loss caused by the tube-rod method. The suction injection method can obtain excellent core-cladding interface quality. However, the disadvantages of this method are also very obvious. First, the timing and temperature of glass liquid pouring are difficult to accurately control, and the stability and consistency are poor; second, the core material of suction injection is usually conical, and it is difficult to obtain a preform with uniform core diameter; in addition, the pouring method used by the suction injection method determines that it is difficult to produce high-quality glass optical fiber preforms with excellent optical uniformity.
[0009] The spin casting method is a method of making optical fiber preform rods by using the centrifugal force generated by the high-speed rotation of the mold. First, the cladding glass liquid is poured into the mold and starts to rotate at high speed. After the cladding glass solidifies, the mold is opened and the fiber core is poured to form an optical fiber preform rod. This method uses centrifugal force to evenly distribute the glass liquid and eliminate bubbles and inclusions. No additional processing is required, which avoids the problem of glass cracking caused by mechanical drilling required for the tube-rod method. In addition, the inner wall of the cladding tube is smooth and does not cause external pollution. Cladding glass tubes with different outer diameters and inner diameters can be easily prepared by changing the size of the mold or changing the volume of glass liquid poured into the mold. However, the optical fiber preform rods made by the spin casting method are very prone to more bubble defects at the core-cladding interface.
[0010] Chinese patent CN201510478413.5 discloses a double crucible method for preparing optical fiber preform based on laminar flow effect. The method uses inner and outer double crucibles to melt glass materials, controls the leakage injection rate by the piston downward speed, and controls the viscosity of the glass liquid and the leakage injection rate to control the Reynolds number of the leakage injection process to ensure that the leakage injection process is laminar. Its biggest advantage is that it is different from the tube and rod method, which requires the processing of sleeves and core rods, and it is also different from the suction injection method, which is difficult to obtain a preform with uniform core layer diameter. The double crucible laminar leakage injection method can obtain excellent core cladding interface quality and constant core diameter. However, when fluoride glass is melted, precipitates and bubbles with high adhesion will inevitably appear at the bottom of the crucible. This is because fluoride glass is highly sensitive to air moisture and ZrF4 hydrate forms non-stoichiometric zirconium oxide fluoride at high temperature. The use of double crucible laminar leakage injection method will cause precipitates and bubbles to be distributed inside the preform through the laminar flow effect.
[0011] In summary, among the existing methods for preparing fluoride glass optical fiber preforms, the tube-rod method is difficult to process, has many defects on the inner and outer surfaces, and is easily contaminated by the external environment; the suction injection method has poor stability and consistency, the core shape is conical, and it is difficult to obtain a preform with a uniform core diameter; the rotary casting method is prone to bubble defects at the core-cladding interface; and the double crucible method is inevitably affected by the sediment at the bottom of the crucible and the bubbles with high adhesion.
[0012] Therefore, it is necessary to design a method and device for preparing fluoride glass optical fiber preform by tube suction method to solve the above problems. Summary of the invention
[0013] The object of the present invention is to provide a method and device for preparing a fluoride glass optical fiber preform by a tube suction method, so as to solve the above-mentioned problems and achieve the purpose of preparing a fluoride glass optical fiber preform with good core-cladding interface quality, less crucible impurity contamination, uniform core diameter and simple preparation process.
[0014] To achieve the above object, the present invention provides the following scheme: a method for preparing a fluoride glass optical fiber preform by a tube suction method, comprising the following steps:
[0015] S1, heating and melting the glass raw materials of the outer cladding, inner cladding and core;
[0016] S2, preparing the outer layer by suction;
[0017] S3, preparing an inner cladding by absorbing inside the outer cladding;
[0018] S4, preparing the fiber core by absorbing inside the inner cladding;
[0019] S5. Annealing the outer cladding, inner cladding and core to obtain a preformed rod product.
[0020] Preferably, in S1, the glass raw materials of the outer cladding, the inner cladding and the core are respectively placed in a platinum crucible, and the platinum crucible is placed in a furnace at 700° C.-900° C. and kept warm for 1 h-2 h to melt all the glass raw materials.
[0021] Preferably, in S2, the platinum crucible containing the molten raw material is taken out of the furnace and placed on a mobile platform, and the temperature of the molten raw material is monitored by infrared temperature measurement. When the temperature of the molten raw material drops to 450°C-550°C, the quartz tube is inserted into the molten raw material of the outer cladding, and the molten raw material is sucked by negative pressure. After the suction is completed, the pressure is maintained for 5s-30s, the negative pressure is released, and the excess raw material is discharged to complete the preparation of the outer cladding.
[0022] Preferably, in S3, the platinum crucible containing the molten raw material of the inner cladding is moved to the bottom of the quartz tube by a mobile platform, and the quartz tube with the outer cladding is inserted into the molten raw material of the inner cladding, and the molten raw material is sucked by negative pressure. After the suction is completed, the pressure is maintained for 5s-10s, the negative pressure is released, and the excess raw material is discharged to complete the preparation of the inner cladding.
[0023] Preferably, in S4, the platinum crucible containing the core molten raw material is moved to the bottom of the quartz tube by a mobile platform, and the quartz tube with an outer cladding and an inner cladding is inserted into the core molten raw material. The molten raw material is sucked by negative pressure, and the pressure is maintained for 10s-30s after the suction is completed. After the core raw material is solidified, the negative pressure is released.
[0024] Preferably, in S5, the quartz tube with the outer cladding, the inner cladding and the core is placed in an annealing furnace for annealing. The annealing temperature is 10°C-20°C higher than the glass transition temperature. The annealing insulation time is 2h-4h. After the insulation is completed, the temperature is lowered to room temperature at a rate of 10°C / h to obtain a preformed rod product.
[0025] Preferably, a single-clad preform product can also be produced.
[0026] A device used in a method for preparing a fluoride glass optical fiber preform rod by a tube suction method comprises a moving platform, a platinum crucible is placed on the top of the moving platform, a lifting column is arranged on one side of the moving platform, the lifting column is fixedly connected to a valve body through a bracket, the valve body is fixedly connected to a quartz tube, the quartz tube is located above the platinum crucible, the valve body is also fixedly connected to two hoses, one of the hoses is fixedly connected to a suction device, and the other hose is fixedly connected to a venting valve through a quick interface.
[0027] Compared with the prior art, the present invention has the following advantages and technical effects:
[0028] 1. Good quality of core-cladding interface: The inner wall of the prepared cladding tube is a surface naturally formed by glass liquid, and there is no defect or pollution caused by optical processing; in addition, the fiber core is smoothly absorbed from bottom to top, and there is no need for optical processing of the core rod, so that a core-cladding interface with excellent quality can be obtained, avoiding the negative impact of defects, pollution and crystallization on the core-cladding interface in the tube-rod method on optical fiber drawing, and greatly reducing the interface loss of optical fiber.
[0029] 2. Less impurity pollution: Fluoride glass is easy to volatilize when it is melted, and a large amount of particulate impurities often adhere to the inner wall of the crucible. If the glass liquid is directly poured out of the crucible, it will inevitably cause pollution to the glass liquid. In the operation process of the present invention, the quartz glass tube is directly inserted into the cladding or core glass liquid, and the glass liquid inside the crucible is taken, which can completely avoid the pollution of the glass liquid by impurities on the inner wall of the crucible and reduce the impurity scattering loss of the optical fiber.
[0030] 3. Uniform core diameter: Although the suction injection method can also obtain a good core-package interface, the obtained core shape presents a conical structure, and it is impossible to obtain a long optical fiber with a uniform core diameter. The optical fiber preform obtained by the present invention has good core diameter uniformity.
[0031] 4. Simple preparation process: Due to the large difference in thermal expansion coefficients between fluoride glass and quartz, the preform rod and the quartz tube will shrink to varying degrees after cooling, causing the preform rod to separate naturally from the inner wall of the quartz tube. The outer surface of the obtained preform rod is smooth and does not require polishing, and the overall preparation process is simple. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those of ordinary skill in the art, other drawings can be obtained based on these drawings without creative labor:
[0033] Figure 1 It is a schematic diagram of the structure of the device of the present invention;
[0034] Figure 2 A flow chart of preparing a double-clad preform rod according to the present invention;
[0035] Figure 3 The present invention is a flow chart for preparing a single-clad preform rod.
[0036] Among them, 1. Mobile platform; 2. Platinum crucible; 3. Quartz tube; 4. Bracket; 5. Valve body; 6. Lifting column; 7. Quick connector; 8. Air release valve; 9. Hose; 10. Extractor. DETAILED DESCRIPTION
[0037] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0039] Reference Figures 1 to 3 As shown, the present invention provides a method for preparing a fluoride glass optical fiber preform by a tube suction method, comprising the following steps
[0040] S1, heating and melting the glass raw materials of the outer cladding, inner cladding and core;
[0041] S2, preparing the outer layer by suction;
[0042] S3, preparing an inner cladding by absorbing inside the outer cladding;
[0043] S4, preparing the fiber core by absorbing inside the inner cladding;
[0044] S5. Annealing the outer cladding, inner cladding and core to obtain a preformed rod product.
[0045] To further optimize the solution, in S1, the glass raw materials for the outer cladding, inner cladding and core are respectively placed in a platinum crucible 2, and the platinum crucible 2 is placed in a furnace at 700°C-900°C and kept warm for 1h-2h to melt all the glass raw materials.
[0046] To further optimize the solution, in S2, the platinum crucible 2 containing the molten raw material is taken out of the furnace and placed on the mobile platform 1. The temperature of the molten raw material is monitored by infrared temperature measurement. When the temperature of the molten raw material drops to 450°C-550°C, the quartz tube 3 is inserted into the molten raw material of the outer cladding, and the molten raw material is absorbed by negative pressure. After the absorption is completed, the pressure is maintained for 5s-30s, the negative pressure is released, the excess raw material is discharged, and the preparation of the outer cladding is completed.
[0047] The quartz tube 3 is a mold for preparing the preformed rod, and different diameters and lengths can be used to prepare preformed rods of different sizes.
[0048] To further optimize the solution, in S3, the platinum crucible 2 containing the molten raw material of the inner cladding is moved to the bottom of the quartz tube 3 by the mobile platform 1, and the quartz tube 3 with the outer cladding is inserted into the molten raw material of the inner cladding, and the molten raw material is sucked by negative pressure. After the suction is completed, the pressure is maintained for 5s-10s, the negative pressure is released, and the excess raw material is discharged to complete the preparation of the inner cladding.
[0049] To further optimize the solution, in S4, the platinum crucible 2 containing the core molten raw material is moved to the bottom of the quartz tube 3 by the mobile platform 1, and the quartz tube 3 with the outer cladding and the inner cladding is inserted into the core molten raw material. The molten raw material is sucked by negative pressure, and the pressure is maintained for 10s-30s after the suction is completed. After the core raw material is solidified, the negative pressure is released.
[0050] The thickness of the cladding glass is controlled by controlling the pressure holding time after the molten raw material is sucked.
[0051] To further optimize the solution, in S5, the quartz tube 3 with the outer cladding, inner cladding and core is placed in an annealing furnace for annealing. The annealing temperature is 10°C-20°C higher than the glass transition temperature. The annealing insulation time is 2h-4h. After the insulation is completed, the temperature is lowered to room temperature at a rate of 10°C / h to obtain a preformed rod product.
[0052] Further optimization of the solution can also produce single-clad preform rod products.
[0053] When preparing a single-clad preform rod, only one cladding raw material melt and one core raw material melt need to be prepared. Step S3 can be omitted, and step S4 can be changed to preparing the core by absorbing inside the outer cladding. Step S5 can be changed to annealing the outer cladding and the core to obtain a finished single-clad preform rod.
[0054] The number of platinum crucibles 2 is 3 or 2. When the number of platinum crucibles 2 is 3, they are used to prepare double-clad preform rods. When the number of platinum crucibles 2 is 2, they are used to prepare single-clad preform rods. Different platinum crucibles 2 are used to hold different core and cladding raw material melts.
[0055] A device used in a method for preparing a fluoride glass optical fiber preform by a tube suction method comprises a moving platform 1, a platinum crucible 2 is placed on the top of the moving platform 1, a lifting column 6 is arranged on one side of the moving platform 1, the lifting column 6 is fixedly connected to a valve body 5 through a bracket 4, the valve body 5 is fixedly connected to a quartz tube 3, the quartz tube 3 is located above the platinum crucible 2, the valve body 5 is also fixedly connected to two hoses 9, one of the hoses 9 is fixedly connected to an absorber 10, and the other hose 9 is fixedly connected to an air release valve 8 through a quick interface 7.
[0056] The mobile platform 1 has a programmable moving function, which can drive the placed platinum crucible 2 to move; the quartz tube 3 is assembled on the valve body 5 and sealed by an O-ring; the bracket 4 is installed on the lifting column 6, and the lifting column 6 has a programmable lifting function, which can drive the valve body 5 and the quartz tube 3 to rise and fall and extend into the platinum crucible 2; the venting valve 8 and the absorber 10 are connected to the valve body 5 by a quick interface 7 and a hose 9 respectively.
[0057] The air release valve 8 has a program control function, and the negative pressure in the quartz tube 3 is maintained or released through program control.
[0058] The suction device 10 has a program control function, and can realize program control to suck or discharge the glass liquid by moving the piston to generate negative pressure.
[0059] The manufacturing process of the present invention includes: starting a high-temperature furnace, melting the cladding and core glass in a plurality of platinum crucibles 2 respectively. After the core and cladding glass liquids are melted, they are placed on a mobile platform 1 to monitor the temperature, and when the temperature is appropriate, the glass liquid is sucked into a quartz tube 3 to form a preform. The suction temperature is determined by the viscosity of the glass liquid, and the cladding thickness is controlled by the holding time. The cladding thickness is controlled by controlling the viscosity of the glass liquid and the holding time, and the number of cladding layers is controlled by the number of suction times. After annealing is completed, the quartz tube 3 is taken out to obtain the desired optical fiber preform.
[0060] The piston movement of the aspirator 10 generates negative pressure to absorb the glass liquid. After the glass liquid cools to a certain degree, the excess glass liquid is discharged to form a cladding tube. In this process, the required cladding thickness can be prepared by controlling the temperature of the glass liquid and the pressure holding time after absorption. The bubble-free good interface between the cladding and the core is achieved by the good wettability of the glass surface at high temperature. In addition, the automatic demoulding of the preform can be achieved by the difference in thermal expansion between the quartz tube 3 and the fluoride glass.
[0061] Example 1: A fluorine-zirconium-based double-clad fluoride glass optical fiber preform
[0062] 1. Put the fluorine zirconium-based outer cladding, inner cladding and core glass into two 100ml and one 75ml platinum crucibles 2 respectively, put the platinum crucible 2 into a silicon carbon rod furnace and melt it at 700℃ for 1 hour to completely melt the glass raw materials into liquid state, then stir with platinum blade slurry for 30 minutes at a stirring speed of 60rpm to keep the glass liquid in the platinum crucible 2 at 700℃ for standby use.
[0063] 2. According to the target optical fiber size, select a quartz tube 3 with an inner diameter of 15 cm and a length of 20 cm, insert the quartz tube 3 into the tenon of the valve body 5, and complete the fixation of the quartz tube 3.
[0064] 3. Take out the outer cladding, inner cladding and core glass liquid at intervals of 1 minute and 30 seconds respectively, place them on the mobile platform 1, use infrared temperature measurement to monitor the temperature of the glass liquid, start the program after the temperature of the outer cladding glass liquid drops to 480°C, insert the quartz tube 3 into the outer cladding glass liquid, and absorb the glass liquid until the liquid level is slightly higher than the required preform rod length.
[0065] 4. After the absorption is completed, lift the quartz tube 3 out of the liquid surface, maintain the pressure for 30 seconds, release the negative pressure, discharge the excess glass liquid, and complete the preparation of the outer cladding.
[0066] 5. Execute the program to align the quartz tube 3 with the inner cladding glass liquid, insert the quartz tube 3 with the outer cladding tube into the inner cladding glass liquid, and absorb the inner cladding glass liquid until the liquid level is slightly higher than the outer cladding length.
[0067] 6. After the absorption is completed, lift the quartz tube 3 out of the liquid surface, maintain the pressure for 10 seconds after the absorption is completed, release the negative pressure, discharge the excess glass liquid, and complete the preparation of the inner cladding.
[0068] 7. Execute the program to align the quartz tube 3 with the core glass liquid, insert the quartz tube 3 with the cladding tube into the core glass liquid, and draw the core glass liquid until the liquid level is slightly higher than the inner cladding length.
[0069] 8. After the absorption is completed, lift the quartz tube 3 out of the liquid surface and maintain the pressure for 30 seconds. After the core glass liquid solidifies, release the negative pressure, remove the quartz tube 3, and immediately put it into the precision annealing furnace for annealing. Set the annealing starting temperature to 250°C, keep it at this temperature for 3 hours, and then cool it to room temperature at a rate of 10°C / h.
[0070] 9. After annealing, the fluoride glass rod is taken out from the quartz tube 3 to obtain a fluorine zirconium-based glass optical fiber preform rod with a double cladding structure.
[0071] Example 2: A fluorine zirconium-based single-clad fluoride glass optical fiber preform
[0072] 1. Put the fluorine zirconium-based outer coating and core glass into two 100ml platinum crucibles 2 respectively, put the platinum crucible 2 into a silicon carbon rod furnace and melt it at 700℃ for 1 hour to completely melt the glass raw materials into liquid state, then stir with platinum blade slurry for 30 minutes at a stirring speed of 60rpm to keep the glass liquid in the platinum crucible 2 at 700℃ for standby use.
[0073] 2. According to the target optical fiber size, select a quartz tube 3 with an inner diameter of 10 cm and a length of 20 cm, insert the quartz tube 3 into the tenon of the valve body 5, and complete the fixation of the quartz tube 3.
[0074] 3. Take out the outer cladding and core glass liquid after an interval of 1 minute, place them on the mobile platform 1, use infrared temperature measurement to monitor the temperature of the glass liquid, start the program after the temperature of the outer cladding glass liquid drops to 450°C, insert the quartz tube 3 into the outer cladding glass liquid, and absorb the glass liquid until the liquid level is slightly higher than the required preform rod length.
[0075] 4. After the absorption is completed, lift the quartz tube 3 out of the liquid surface, maintain the pressure for 10 seconds, release the negative pressure, discharge the excess glass liquid, and complete the preparation of the outer cladding.
[0076] 5. Execute the program to align the quartz tube 3 with the core glass liquid, insert the quartz tube 3 with the cladding tube into the core glass liquid, and draw the core glass liquid until the liquid level is slightly higher than the outer cladding length.
[0077] 6. After the absorption is completed, lift the quartz tube 3 out of the liquid surface and maintain the pressure for 10 seconds. After the core glass liquid solidifies, release the negative pressure, remove the quartz tube 3, and immediately put it into the precision annealing furnace for annealing. The annealing starting temperature is set to 250℃. First, keep it at this temperature for 2 hours, and then cool it to room temperature at a rate of 10℃ / h.
[0078] 7. After annealing, the fluoride glass rod is taken out from the quartz tube 3 to obtain a fluorine zirconium-based glass optical fiber preform rod with a single cladding structure.
[0079] Example 3: A fluorine-indium-based double-clad fluoride glass optical fiber preform
[0080] 1. Put the fluorine-indium-based outer cladding, inner cladding and core glass into two 100ml and one 75ml platinum crucibles 2 respectively, put the platinum crucible 2 into a silicon carbon rod furnace and melt it at 900℃ for 1 hour to completely melt the glass raw materials into liquid state, then stir with platinum blade slurry for 30 minutes at a stirring speed of 60rpm to keep the glass liquid in the platinum crucible 2 at 800℃ for standby use.
[0081] 2. According to the target optical fiber size, select a quartz tube 3 with an inner diameter of 12 cm and a length of 20 cm, insert the quartz tube 3 into the tenon of the valve body 5, and complete the fixation of the quartz tube 3.
[0082] 3. Take out the outer cladding, inner cladding and core glass liquids at intervals of 1.5 minutes and 30 seconds respectively, and place them on the mobile platform 1. Use infrared temperature measurement to monitor the temperature of the glass liquid. After the temperature of the outer cladding glass liquid drops to 550°C, start the program, insert the quartz tube 3 into the outer cladding glass liquid, and absorb the glass liquid until the liquid level is slightly higher than the required preform rod length.
[0083] 4. After the absorption is completed, lift the quartz tube 3 out of the liquid surface, maintain it for 30 seconds, release the negative pressure, discharge the excess glass liquid, and complete the preparation of the outer cladding.
[0084] 5. Execute the program to place the quartz tube 3 against the inner cladding glass liquid, insert the quartz tube 3 with the outer cladding tube into the inner cladding glass liquid, and absorb the inner cladding glass liquid until the liquid level is slightly higher than the outer cladding length.
[0085] 6. After the absorption is completed, lift the quartz tube 3 out of the liquid surface, maintain the pressure for 5 seconds after the absorption is completed, release the negative pressure, discharge the excess glass liquid, and complete the preparation of the inner cladding.
[0086] 7. Execute the program to align the quartz tube 3 with the core glass liquid, insert the quartz tube 3 with the cladding tube into the core glass liquid, and draw the core glass liquid until the liquid level is slightly higher than the inner cladding length.
[0087] 8. After the absorption is completed, lift the quartz tube 3 out of the liquid surface and maintain the pressure for 30 seconds. After the core glass liquid solidifies, release the negative pressure, remove the quartz tube 3, and immediately put it into the precision annealing furnace for annealing. The annealing starting temperature is set to 230°C. First, keep it at this temperature for 4 hours, and then cool it to room temperature at a rate of 10°C / h.
[0088] 9. After the annealing is completed, the fluoride glass rod is taken out from the quartz tube 3 to obtain a fluorine-indium-based glass optical fiber preform rod with a double cladding structure.
[0089] In the description of the present invention, it should be understood that the terms "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside" and "outside" etc., indicating orientations or positional relationships, are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.
[0090] The embodiments described above are only descriptions of the preferred embodiments of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should fall within the protection scope of the present invention.
Claims
1. A method for preparing a fluoride glass optical fiber preform by a tube suction method, characterized in that: The following steps are included S1, heating and melting the glass raw materials of the outer cladding, inner cladding and core; S2, sucking and preparing the outer layer; S3, preparing an inner cladding by absorbing inside the outer cladding; S4, preparing the fiber core by absorbing inside the inner cladding; S5. Annealing the outer cladding, inner cladding and core to obtain a preformed rod product.
2. The method for preparing a fluoride glass optical fiber preform by a tube suction method according to claim 1, characterized in that: In S1, the glass raw materials of the outer cladding, inner cladding and core are respectively placed in a platinum crucible (2), and the platinum crucible (2) is placed in a melting furnace at 700° C.-900° C. and kept warm for 1 h-2 h to melt all the glass raw materials.
3. The method for preparing a fluoride glass optical fiber preform by a pipetting method according to claim 2, characterized in that: In S2, the platinum crucible (2) containing the molten raw material is taken out of the furnace and placed on the mobile platform (1). The temperature of the molten raw material is monitored by infrared temperature measurement. When the temperature of the molten raw material drops to 450°C-550°C, the quartz tube (3) is inserted into the molten raw material of the outer cladding layer, and the molten raw material is sucked by negative pressure. After the suction is completed, the pressure is maintained for 5s-30s, the negative pressure is released, and the excess raw material is discharged to complete the preparation of the outer cladding layer.
4. The method for preparing a fluoride glass optical fiber preform by a pipetting method according to claim 3, characterized in that: In S3, the platinum crucible (2) containing the molten raw material of the inner cladding is moved to the bottom of the quartz tube (3) by means of the mobile platform (1), and the quartz tube (3) with the outer cladding is inserted into the molten raw material of the inner cladding, and the molten raw material is sucked by negative pressure. After the suction is completed, the pressure is maintained for 5s-10s, and the negative pressure is released to discharge the excess raw material, thereby completing the preparation of the inner cladding.
5. The method for preparing a fluoride glass optical fiber preform by a pipetting method according to claim 4, characterized in that: In S4, the platinum crucible (2) containing the core molten raw material is moved to the bottom of the quartz tube (3) by the mobile platform (1), and the quartz tube (3) with the outer cladding and the inner cladding is inserted into the core molten raw material. The molten raw material is sucked by negative pressure. After the suction is completed, the pressure is maintained for 10s-30s. After the core raw material is solidified, the negative pressure is released.
6. The method for preparing a fluoride glass optical fiber preform by a pipetting method according to claim 5, characterized in that: In S5, the quartz tube (3) with the outer cladding, the inner cladding and the fiber core is placed in an annealing furnace for annealing. The annealing temperature is 10°C-20°C higher than the glass transition temperature. The annealing insulation time is 2h-4h. After the insulation is completed, the temperature is lowered to room temperature at a rate of 10°C / h to obtain a preformed rod product.
7. The method for preparing a fluoride glass optical fiber preform by a tube suction method according to claim 1, characterized in that: It is also possible to produce a single-clad preform product.
8. A device used in the method for preparing a fluoride glass optical fiber preform by a pipette suction method according to any one of claims 1 to 7, characterized in that: The invention comprises a mobile platform (1), a platinum crucible (2) is placed on the top of the mobile platform (1), a lifting column (6) is arranged on one side of the mobile platform (1), the lifting column (6) is fixedly connected to a valve body (5) through a bracket (4), the valve body (5) is fixedly connected to a quartz tube (3), the quartz tube (3) is located above the platinum crucible (2), and the valve body (5) is also fixedly connected to two hoses (9), one of the hoses (9) is fixedly connected to a suction device (10), and the other hose (9) is fixedly connected to a venting valve (8) through a quick interface (7).
Citation Information
Patent Citations
Making device and method for soft glass optical fiber preform
CN105060700A
Automatic material suction device and material suction method thereof
CN114604636A
Device and method for preparing fluoride optical fiber preform
CN115893827A
Double-clad fluoride gain fiber and preparation method thereof
CN116774348A
Rare earth ions doped oxyfluoride microcrystalline glass optical fiber and preparing method thereof
CN1544964A