Preparation method of antibacterial glass bottle for cosmetic packaging

By using nanozeolite-loaded silver-zinc composite antibacterial agent and alternate leaf white laminate oil in cosmetic glass bottles, combined with heat treatment and surface protective layer technology, the problem of glass bottles being susceptible to bacterial infection is solved, and the lasting antibacterial effect and products are achieved Safety and durability.

CN118993538APending Publication Date: 2024-11-22HENAN FANGYU BIOTECHNOLOGY CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411199981.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Glass bottles in cosmetic packaging are susceptible to bacterial infections and cannot effectively protect the cosmetics in the packaging, affecting product quality and user experience.

Method used

Antibacterial glass bottles were prepared by nanozeolite-loaded silver-zinc composite antibacterial agent and alternate leaf white melaleuca oil as antibacterial additives, combined with heat treatment and surface protective film technology. The method includes raw material pretreatment, melt forming, annealing treatment and the formation of surface protective layers to ensure uniform distribution and long-lasting effect of antibacterial agents.

Benefits of technology

It significantly improves the antibacterial effect of glass bottles, extends the service life of cosmetics, ensures the safety and durability of the product, and does not affect the processing performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005017598740000071
    Figure BDA0005017598740000071
  • Figure BDA0005017598740000072
    Figure BDA0005017598740000072
Patent Text Reader

Abstract

The invention relates to the technical field of daily chemical packaging, in particular to a preparation method of an antibacterial glass bottle for cosmetic packaging, which comprises the following steps: step 1, raw material pretreatment: crushing blocky raw materials quartz sand, sodium carbonate, limestone, dolomite and feldspar, drying and removing impurities; step 2, adding the additive and the antibacterial agent, and uniformly mixing; 3, melting: heating and melting the mixed material obtained in the step 2 at the temperature of 1500-1600 DEG C to obtain liquid glass; 4, molding: putting the liquid glass into a mold, and molding to obtain a glass bottle; 5, heat treatment, wherein the glass bottle obtained in the step 4 is annealed, and a finished product is obtained. The antibacterial agent comprises a nano zeolite silver-loaded zinc composite antibacterial agent. The glass bottle disclosed by the invention has the advantages of difficulty in generating bacterial drug resistance, slow release, good sterilization effect, lasting sterilization and bacteriostasis effects, harmlessness to a human body, no irritation to skin, small powder particle size, uniform distribution, large specific surface area and no influence on processing performance and other performance of a material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of daily chemical packaging, and in particular to a method for preparing an antibacterial glass bottle for cosmetic packaging. Background Art

[0002] Antimicrobial agents are essential for human survival, development and environmental protection. With the rapid development of the cosmetics industry, glass bottles are easy to process, have good printing adaptability, and have a beautiful and classy appearance. They are favored by many cosmetics manufacturers and are widely used in the packaging of cleansing products, skin care products, and beauty and hairdressing products. At present, the packaging bottles commonly used in cosmetic packaging have the following problems: they can be infected by bacteria, cannot effectively protect the cosmetics in the packaging bottles, affect the quality of cosmetics, cause discomfort to consumers, and greatly affect the user experience. Summary of the invention

[0003] The object of the present invention is to provide a method for preparing a glass bottle for cosmetics with better antibacterial effect and longer-lasting antibacterial effect.

[0004] Based on the above purpose, the present invention adopts the following technical solutions:

[0005] A method for preparing an antibacterial glass bottle for cosmetic packaging comprises the following steps:

[0006] Step 1, raw material pretreatment: crush the blocky raw materials of quartz sand, soda ash, limestone, dolomite and feldspar, dry them and remove impurities (remove iron)

[0007] Step 2, adding additives and antimicrobial agents and mixing evenly;

[0008] Step 3, melting: heating and melting the mixed material obtained in step 2 at a temperature of 1500-1600° C. to obtain liquid glass;

[0009] Step 4, molding: putting liquid glass into a mold to mold and make a glass bottle;

[0010] Step 5, heat treatment: annealing the glass bottle obtained in step 4 to obtain a finished product;

[0011] The antibacterial agent comprises a nano-zeolite-supported silver-zinc composite antibacterial agent.

[0012] Preferably, the composite antibacterial agent contains 0.1-0.3% by mass of AgO, 0.5-0.8% by mass of ZnO, and the rest is nano zeolite.

[0013] Preferably, the particle size of the nano-zeolite-loaded silver-zinc composite antibacterial agent particles is 25-55 nanometers.

[0014] Preferably, the antibacterial agent also includes Melaleuca alternifolia oil.

[0015] Preferably, in step 5, the annealing temperature is 500-550° C., the temperature is lowered to 100-150° C. for 3-5 hours, and then lowered to room temperature.

[0016] Preferably, before the heat treatment in step 5, the surface of the glass bottle is heat-coated, specifically: when the glass bottle is cooled to 500-600° C., a metal coating agent is sprayed on the surface of the container to form a protective film with a thickness of 0.1-0.3 mm.

[0017] Preferably, the metal coating agent is a mixture of tin oxide and titanium oxide, and the weight ratio of the tin oxide to the titanium oxide is 1:1-3.

[0018] Preferably, after the heat treatment in step 5, the glass bottle is cold-coated, wherein the cold coating is as follows: when the glass bottle is cooled to 20-60° C., a polymer emulsion is sprayed into a mist and attached to the surface of the glass bottle to form a protective layer with wear resistance and lubricity.

[0019] Preferably, the polymer emulsion is an acrylic resin emulsion.

[0020] Preferably, in step 1 and step 2, the weight portions of the raw materials and additives are: 18-25 parts of quartz sand, 8-14 parts of soda ash, 15-25 parts of limestone, 14-26 parts of dolomite, 15-20 parts of feldspar, 2-3 parts of CaO, 2-5 parts of MgO, 1-3 parts of P2O3, 1-3 parts of Na2O, 2-5 parts of cryolite, 10-18 parts of composite antibacterial agent, and 3-5 parts of Melaleuca alternifolia oil.

[0021] Silica sand or borax introduces silicon oxide or boron oxide, the main components of glass, which can be melted into the main body of glass during combustion and determine the main properties of glass. Sodium oxide, which can form fusible complex salts with acidic oxides such as silica sand during calcination, plays a role in fluxing and makes glass easier to shape.

[0022] Limestone introduces calcium oxide, the main component of glass, to enhance the chemical stability and mechanical strength of glass, improve the transparency of glass, reduce thermal expansion and improve water resistance, but too much content will cause glass crystal folding and reduce heat resistance. Feldspar, as a raw material for introducing aluminum oxide, can control the melting temperature and also improve durability. In addition, feldspar can also provide potassium oxide components to improve the thermal expansion performance of glass. The addition of cryolite, as an emulsifier, can form particles of 0.1-1.0μm, which are suspended in the glass, making the glass opaque and turning the glass into a milky white translucent body.

[0023] The surface state, composition and structure of glass bottles are very different from their internal composition and structure. The surface properties of glass bottles have a significant impact on their main properties. The chemical stability of glass actually depends on the chemical stability of its surface. The mechanical strength and impact resistance of glass are also largely determined by the morphology and structure of the glass surface. Therefore, the surface treatment of glass is one of the important technical means to manufacture high-strength and lightweight glass containers. The purpose of glass bottle surface treatment is to change the chemical stability of the container surface and eliminate the damage to the glass surface, so as to achieve the purpose of strengthening.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] The preparation method of the antibacterial glass bottle for cosmetic packaging provided by the present invention adopts nano-zeolite silver-zinc composite antibacterial agent as an antibacterial additive, which is added to the glass bottle raw material. The metallic silver has strong bactericidal and antibacterial ability and high safety, and the bactericidal property of silver ions is stronger than that of elemental silver. The silver ions are loaded on inorganic mineral materials with good adsorption and ion exchange properties, which not only have a certain slow-release effect, but also can give good performance to the carrier material used for the antibacterial agent. The nano-level zeolite has good adsorption, screening, cation exchange and catalytic properties, and has high purity and strong selective exchange ability for silver ions. The nano-zeolite silver-zinc antibacterial agent with the nano-zeolite as a carrier is not easy to produce bacterial resistance, is slowly released, has good sterilization effect, has a lasting bactericidal and antibacterial effect, is harmless to the human body, has no irritation to the skin, is a safe and non-toxic product, and has a small powder particle size, uniform distribution, large specific surface area, and has no effect on the processing performance and other properties of the material. At the same time, Melaleuca alternifolia oil is added as an antibacterial agent, which cooperates with the nano-zeolite antibacterial agent to further improve the antibacterial effect, ensure that the cosmetics contained in the antibacterial glass bottle are not contaminated, and extend its service life.

[0026] Furthermore, the present invention heat-coates the glass bottle after it is formed before heat treatment, sprays the metal coating agent on the surface of the container to form a protective film, enhances the surface strength by about 30%, and enables the bottle to withstand long-term water flushing and washing. After the heat treatment of the glass bottle, cold coating is performed again, spraying the polymer emulsion into mist, adhering to the surface of the glass bottle, forming a protective layer with wear resistance and lubricity. The two protective layers make the glass bottle more durable. DETAILED DESCRIPTION

[0027] In the description of the present embodiment, it should be understood that the terms "first" and "second" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features, that is, include one or more of the features. In the description of the present invention, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined. When a feature "includes or contains" one or some of the features it covers, unless otherwise specifically described, this indicates that other features are not excluded and other features may be further included.

[0028] In the description of the present embodiment, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0029] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme of the present invention is described in detail below, but the following embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other implementation methods obtained by those skilled in the art without making creative work belong to the scope of protection of the present invention.

[0030] Example 1

[0031] A method for preparing an antibacterial glass bottle for cosmetic packaging comprises the following steps:

[0032] Step 1, raw material pretreatment: crush 22 parts of block raw materials of quartz sand, 11 parts of soda ash, 20 parts of limestone, 20 parts of dolomite, and 17 parts of feldspar by weight, and dry them, remove impurities, and remove iron;

[0033] Step 2, adding additives CaO 2.5 parts, MgO 4 parts, P2O3 2 parts, Na2O 2 parts, cryolite 4 parts, composite antibacterial agent 10 parts, Melaleuca alternifolia oil 3 parts by weight, and mixing evenly;

[0034] Step 3, melting: heating and melting the mixed material obtained in step 2 at a temperature of 1550° C. to obtain liquid glass;

[0035] Step 4, molding: putting liquid glass into a mold to mold and make a glass bottle;

[0036] Step 5, heat treatment: annealing the glass bottle obtained in step 4 at a temperature of 520°C, cooling the temperature to 130°C for 4 hours, and then cooling the temperature to room temperature to obtain a finished product;

[0037] The antibacterial agent comprises a nano-zeolite silver-zinc composite antibacterial agent, which contains 0.2% by mass of AgO, 0.6% by mass of ZnO, and the rest is nano-zeolite, and the particle size of the nano-zeolite silver-zinc composite antibacterial agent is 35-38 nanometers.

[0038] Step 5 Before the heat treatment, the surface of the glass bottle is heat-coated, specifically: when the glass bottle is cooled to 600°C, a metal coating agent is sprayed on the surface of the container to form a protective film with a thickness of 0.3 mm. The metal coating agent is a mixture of tin oxide and titanium oxide, and the weight ratio of tin oxide to titanium oxide is 1:2.

[0039] Step 5 After the heat treatment, the glass bottle is cold-coated, wherein when the glass bottle is cooled to 60° C., a polymer emulsion is sprayed in a mist form and attached to the surface of the glass bottle to form a protective layer with wear resistance and lubricity. The polymer emulsion is an acrylic resin emulsion.

[0040] Example 2

[0041] A method for preparing an antibacterial glass bottle for cosmetic packaging comprises the following steps:

[0042] Step 1, raw material pretreatment: crush 18 parts of block raw materials of quartz sand, 14 parts of soda ash, 15 parts of limestone, 26 parts of dolomite, and 20 parts of feldspar by weight, and dry them, remove impurities, and remove iron;

[0043] Step 2, adding additives CaO 3 parts, MgO 2 parts, P2O3 1 part, Na2O 3 parts, cryolite 2 parts, composite antibacterial agent 14 parts, Melaleuca alternifolia oil 4 parts by weight, and mixing evenly;

[0044] Step 3, melting: heating and melting the mixed material obtained in step 2 at a temperature of 1500° C. to obtain liquid glass;

[0045] Step 4, molding: putting liquid glass into a mold to mold and make a glass bottle;

[0046] Step 5, heat treatment: annealing the glass bottle obtained in step 4 at a temperature of 500°C, cooling it to 100°C for 3 hours, and then cooling it to room temperature to obtain a finished product;

[0047] The antibacterial agent comprises a nano-zeolite silver-zinc composite antibacterial agent, which contains 0.1% by mass of AgO, 0.8% by mass of ZnO, and the rest is nano-zeolite, and the particle size of the nano-zeolite silver-zinc composite antibacterial agent is 25-28 nanometers.

[0048] Step 5 Before the heat treatment, the surface of the glass bottle is heat-coated, specifically: when the glass bottle is cooled to 500°C, a metal coating agent is sprayed on the surface of the container to form a protective film with a thickness of 0.1 mm. The metal coating agent is a mixture of tin oxide and titanium oxide, and the weight ratio of tin oxide to titanium oxide is 1:3.

[0049] Step 5 After the heat treatment, the glass bottle is cold-coated, wherein when the glass bottle is cooled to 20° C., a polymer emulsion is sprayed in a mist form and attached to the surface of the glass bottle to form a protective layer with wear resistance and lubricity. The polymer emulsion is an acrylic resin emulsion.

[0050] Example 3

[0051] A method for preparing an antibacterial glass bottle for cosmetic packaging comprises the following steps:

[0052] Step 1, raw material pretreatment: crush 25 parts of block raw materials of quartz sand, 8 parts of soda ash, 25 parts of limestone, 14 parts of dolomite, and 15 parts of feldspar by weight, and dry them, remove impurities, and remove iron;

[0053] Step 2, adding additives CaO 2 parts, MgO 5 parts, P2O3 3 parts, Na2O 1 part, cryolite 5 parts, composite antibacterial agent 18 parts, Melaleuca alternifolia oil 5 parts by weight, and mixing evenly;

[0054] Step 3, melting: heating and melting the mixed material obtained in step 2 at a temperature of 1600° C. to obtain liquid glass;

[0055] Step 4, molding: putting liquid glass into a mold to mold and make a glass bottle;

[0056] Step 5, heat treatment: annealing the glass bottle obtained in step 4 at a temperature of 550°C, cooling the temperature to 150°C for 5 hours, and then cooling the temperature to room temperature to obtain a finished product;

[0057] The antibacterial agent comprises a nano-zeolite silver-zinc composite antibacterial agent, which contains 0.3% by mass of AgO, 0.5% by mass of ZnO, and the rest is nano-zeolite, and the particle size of the nano-zeolite silver-zinc composite antibacterial agent is 50-55 nanometers.

[0058] Step 5 Before the heat treatment, the surface of the glass bottle is heat-coated, specifically: when the glass bottle is cooled to 550°C, a metal coating agent is sprayed on the surface of the container to form a protective film with a thickness of 0.2 mm. The metal coating agent is a mixture of tin oxide and titanium oxide, and the weight ratio of tin oxide to titanium oxide is 1:1.

[0059] Step 5 After the heat treatment, the glass bottle is cold-coated, wherein when the glass bottle is cooled to 40° C., a polymer emulsion is sprayed in a mist form and attached to the surface of the glass bottle to form a protective layer with wear resistance and lubricity. The polymer emulsion is an acrylic resin emulsion.

[0060] The glass bottle of Example 1 of the present invention was used to hold the hydrosol, and various tests were carried out two years later. The specific results are as follows:

[0061] Table 1. Microbial detection in hydrosols

[0062]

[0063] Table 2. Detection of heavy metal content in hydrosol

[0064]

[0065] As can be seen from the above table, the antibacterial glass bottle of the present invention is not easy to produce bacterial resistance by adding the nano-zeolite silver-zinc composite antibacterial agent, and has a slow release, good sterilization effect, and a lasting bactericidal and antibacterial effect. At the same time, the addition of Melaleuca alternifolia oil as an antibacterial agent, which cooperates with the nano-zeolite antibacterial agent, further improves the antibacterial effect, ensures that the cosmetics contained in the antibacterial glass bottle are not contaminated, and prolongs its service life.

[0066] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A method for preparing an antibacterial glass bottle for cosmetic packaging, characterized in that: The following steps are involved: Step 1, raw material pretreatment: crush the blocky raw materials of quartz sand, soda ash, limestone, dolomite and feldspar, dry them and remove impurities (remove iron) Step 2, adding additives and antimicrobial agents and mixing evenly; Step 3, melting: heating and melting the mixed material obtained in step 2 at a temperature of 1500-1600° C. to obtain liquid glass; Step 4, molding: putting liquid glass into a mold to mold and make a glass bottle; Step 5, heat treatment: annealing the glass bottle obtained in step 4 to obtain a finished product; The antibacterial agent comprises a nano-zeolite-supported silver-zinc composite antibacterial agent.

2. The method for preparing the antibacterial glass bottle for cosmetic packaging according to claim 1, characterized in that: The composite antibacterial agent contains 0.1-0.3% by mass of AgO, 0.5-0.8% by mass of ZnO, and the rest is nano zeolite.

3. The method for preparing the antibacterial glass bottle for cosmetic packaging according to claim 1, characterized in that: The particle size of the nano-zeolite-supported silver-zinc composite antibacterial agent particles is 25-55 nanometers.

4. The method for preparing the antibacterial glass bottle for cosmetic packaging according to claim 1, characterized in that: The antimicrobial agents also include Melaleuca alternifolia oil.

5. The method for preparing the antibacterial glass bottle for cosmetic packaging according to claim 1, characterized in that: In the step 5, the annealing temperature is 500-550° C., the temperature is lowered to 100-150° C. for 3-5 hours, and then the temperature is lowered to room temperature.

6. The method for preparing the antibacterial glass bottle for cosmetic packaging according to claim 1, characterized in that: Step 5 Before the heat treatment, the surface of the glass bottle is heat-coated. Specifically, when the glass bottle is cooled to 500-600° C., a metal coating agent is sprayed on the surface of the container to form a protective film with a thickness of 0.1-0.3 mm.

7. The method for preparing the antibacterial glass bottle for cosmetic packaging according to claim 6, characterized in that: The metal coating agent is a mixture of tin oxide and titanium oxide, and the weight ratio of the tin oxide to the titanium oxide is 1:1-3.

8. The method for preparing the antibacterial glass bottle for cosmetic packaging according to claim 1, characterized in that: After the heat treatment in step 5, the glass bottle is cold-coated. The cold coating is as follows: when the glass bottle is cooled to 20-60° C., a polymer emulsion is sprayed into mist and attached to the surface of the glass bottle to form a protective layer with wear resistance and lubricity.

9. The method for preparing the antibacterial glass bottle for cosmetic packaging according to claim 8, characterized in that: The polymer emulsion is an acrylic resin emulsion.

10. The method for preparing an antibacterial glass bottle for cosmetic packaging according to claim 1, characterized in that: In step 1 and step 2, the weight proportions of the raw materials and additives are: 18-25 parts of quartz sand, 8-14 parts of soda ash, 15-25 parts of limestone, 14-26 parts of dolomite, 15-20 parts of feldspar, 2-3 parts of CaO, 2-5 parts of MgO, 1-3 parts of P2O3, 1-3 parts of Na2O, 2-5 parts of cryolite, 10-18 parts of composite antibacterial agent, and 3-5 parts of Melaleuca alternifolia oil.

Citation Information

Patent Citations

  • Cold-end spraying agent for glass product and method for making same

    CN101041559A

  • Medical glass bottle formula and preparation method thereof

    CN107586019A

  • Anti-bacterial bottle

    JP1997118373A