Heat-insulating self-cleaning transparent coating and preparation method thereof

By preparing an indium-doped tin oxide and zwitterionic polymer composite coating on glass, the problems of insufficient pollutant adsorption and heat insulation performance of glass windows are solved, achieving self-cleaning and heat insulation effects, and improving transparency and ease of cleaning.

CN118993571APending Publication Date: 2024-11-22天辰(天津)生物科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411107386.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing glass windows suffer from the problems of pollutant adsorption and penetration, affecting their appearance and practicality. They also lack sufficient heat insulation and self-cleaning performance, making cleaning difficult and posing safety hazards, especially on the exterior of high-rise buildings.

Method used

A transparent coating using an indium-doped tin oxide layer combined with a zwitterionic polymer layer is formed by growing indium-doped tin oxide seeds on a glass slide, combined with hydrothermal reaction and ultrasonic treatment, to create a uniform nanoparticle coating. The zwitterionic polymer enhances hydrophilicity and electrostatic interaction, achieving a self-cleaning effect.

Benefits of technology

It improves the heat insulation performance and self-cleaning ability of the glass surface, reduces the adhesion of pollutants, increases light transmittance, and simplifies the cleaning process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004991205990000071
    Figure BDA0004991205990000071
  • Figure BDA0004991205990000081
    Figure BDA0004991205990000081
Patent Text Reader

Abstract

The invention discloses a heat-insulating self-cleaning transparent coating and a preparation method thereof, and relates to the technical field of material science and surface engineering. According to the preparation method, oxalic acid is used for assisting a hydrothermal growth solution, generated indium hydroxide and tin hydroxide nucleate and grow on indium-doped tin oxide seeds, uniform and ordered nano-particles are obtained on a glass substrate, the coating achieves the heat insulation performance, and through 3-ethyoxyl catechol, 1, 3-propane sultone is grafted, so that the heat insulation performance of the coating is improved. The zwitter-ion polymer is formed by the zwitter-ion polymer and polyethyleneimine, gaps of particles are filled with the zwitter-ion polymer through ultrasound, the zwitter-ion polymer is combined with water molecules through electrostatic and hydrogen bond interaction, a stable and compact hydration layer structure is formed, the affinity of pollutants and the coating is reduced, and then oil stains are easily removed through continuous water. And the long-acting self-cleaning effect is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of material science and surface engineering, and in particular to a heat-insulating self-cleaning transparent coating and a preparation method thereof. Background Art

[0002] In recent years, with the rapid development of economic level and the progress of human society, environmental problems have become more and more prominent. The generation of industrial waste, the discharge of domestic waste and the dust in the air have brought a large number of pollutants and bacteria. Due to the effects of static electricity, capillary and other factors, pollutants are easily adsorbed and penetrated into the surface of materials, which not only affects the appearance and practicality of the materials, but also threatens people's health. At the same time, the surface of materials contaminated by dust and bacteria requires a lot of manpower and financial resources to clean and maintain; and with global warming, greenhouse gas emissions are becoming more and more serious, and the proportion of building energy consumption in the total social energy consumption is increasing. Glass windows, as lighting channels and energy exchange channels for high-rise buildings, cars, ceilings, etc., have a great impact on building energy consumption. In addition, the glass windows on the periphery of high-rise buildings also have problems such as difficulty in cleaning, especially in cities in desert areas. Traditional glass windows have poor selection ability for sunlight, not only visible light is easy to pass through, but also radiation caused by sunlight enters the room, and the heat insulation ability is not good. In addition, there are two problems in the cleaning of high-altitude glass: the difficulty coefficient is large and the risk coefficient is high; therefore, it is particularly necessary to invent a heat-insulating self-cleaning transparent coating. Summary of the invention

[0003] The object of the present invention is to provide a heat-insulating self-cleaning transparent coating and a preparation method thereof, so as to solve the problems existing in the prior art.

[0004] In order to solve the above technical problems, the present invention provides the following technical solution: a heat-insulating and self-cleaning transparent coating, wherein the heat-insulating and self-cleaning transparent coating is made of an indium-doped tin oxide layer and a composite zwitterionic polymer layer.

[0005] Furthermore, a method for preparing a heat-insulating self-cleaning transparent coating comprises the following preparation steps:

[0006] (1) Pre-treating a glass sheet, and then coating the glass sheet with an indium-doped tin oxide precursor solution by Czochralski coating, drying at 50-70° C. for 2-4 hours, repeating the coating step 3-6 times, and finally annealing at 220-260° C. for 8-15 minutes to obtain a glass sheet coated with indium-doped tin oxide seeds;

[0007] (2) immersing the glass sheet covered with indium-doped tin oxide seeds in a growth solution, subjecting it to a hydrothermal reaction, washing it with deionized water for 3 to 8 times, and drying it at 50 to 80° C. for 2.5 to 5 hours to obtain a glass sheet covered with indium-doped tin oxide;

[0008] (3) Mix polyethyleneimine and deionized water, stir at 300-600 rpm for 10-30 min, add 3-ethoxycatechol, raise the temperature to 55-70° C. under nitrogen atmosphere, stir at 100-200 rpm for 100-200 min, add 1,3-propane sultone, continue stirring for 10-15 h, and then adjust the solution pH to 7.8-8.5 with sodium hydroxide solution to obtain a zwitterionic polymer;

[0009] (4) The zwitterionic polymer is mixed at 15 to 30 g / m 2 The glass sheet covered with indium-doped tin oxide is placed upside down, and after ultrasonic treatment, it is cured at 30-60° C. for 6-10 hours to obtain a heat-insulating and self-cleaning transparent coating.

[0010] Furthermore, the glass pretreatment method of step (1) is as follows: the glass sheet is immersed in a 5wt% sodium hydroxide aqueous solution for 4 hours, then rinsed with deionized water for 3 to 6 times, immersed in a 0.5wt% potassium dichromate aqueous solution for 24 hours, then ultrasonically washed with deionized water at 21kHz for 10 to 30 minutes, then washed with anhydrous ethanol for 3 to 6 times, and dried at 50 to 80°C for 1 to 3 hours.

[0011] Furthermore, the preparation method of the indium-doped tin oxide precursor solution in step (1) is as follows: tin tetrachloride pentahydrate, hexamethylenetetramine, indium chloride, and deionized water are mixed in a mass ratio of 1-5:1.5:3-6:1000, and stirred at 100-300 rpm for 25-50 min.

[0012] Furthermore, in step (1), the downward speed of the coating pulling process is 0.15 to 0.2 mm / s, the upward speed is 0.05 to 0.1 mm / s, and the residence time is 8 to 15 min.

[0013] Furthermore, the preparation method of the growth liquid in step (2) is as follows: tin tetrachloride pentahydrate, hexamethylenetetramine, indium chloride, and deionized water are mixed in a mass ratio of 1-5:1.5:3-6:1000, stirred at 100-300 rpm for 25-50 min, and ethylene glycol in an amount of 0.3 times the mass of hexamethylenetetramine is added, and mixed to obtain the product.

[0014] Furthermore, the conditions of the hydrothermal reaction in step (2) are: temperature of 60-90° C. and time of 24 h.

[0015] Furthermore, the molecular weight of the polyethyleneimine in step (3) is 10,000.

[0016] Furthermore, in step (3), the mass ratio of polyethyleneimine, deionized water, 3-ethoxycatechol and 1,3-propane sultone is 2-4:300-500:0.1-0.5:0.8-1.4.

[0017] Furthermore, the frequency of the ultrasound in step (4) is 21 to 25 kHz and the time is 10 to 30 minutes.

[0018] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0019] The invention uses tin tetrachloride pentahydrate and indium chloride to grow indium-doped tin oxide seeds on a glass substrate, then uses oxalic acid to assist hydrothermal growth liquid, so that indium hydroxide and tin hydroxide are nucleated and grown on the indium-doped tin oxide seeds, and indium oxide and tin oxide are generated after dehydroxylation, thereby improving the stability of the coating, wherein ethylene glycol controls the growth of particles, and in the hot water reaction, ethylene glycol surrounds the initially formed nucleus, inhibits a specific crystal face, and promotes the growth of other faces, so that the obtained crystals no longer grow excessively along a certain direction, and the shape changes from a long strip of log to a regular square, thereby obtaining uniform and ordered nanoparticles, and having a strong reflective ability for infrared light of thermal radiation, so that the coating realizes heat insulation performance, and then, 3-ethoxycatechol is grafted with 1,3-propane sultone and polyethylene The ethyleneimine forms a zwitterionic polymer, which is coated on the substrate by reverse coating. After ultrasound, it fills the gaps between the particles, so that the obtained coating is smooth and bubble-free, and the light transmittance of the coating is enhanced. The zwitterionic polymer combines with water molecules through electrostatic and hydrogen bond interactions to enhance the hydrophilicity of the coating. The oxygen on the ketone group in 1,3-propane sultone and the hydrogen ion on the amino group at the β position of polyethyleneimine form a five-membered ring structure through intramolecular hydrogen bonds, which increases the proportion of strong hydrogen bonds in the matrix. The ethoxy group in 3-ethoxycatechol protects the functional groups in the matrix, making the strong hydrogen bonds more stable, and cooperates with the electrostatic effect to enhance the interaction between it and the water molecules, thereby forming a stable and dense hydration layer structure, reducing the affinity of pollutants to the coating, and then the oil stains are easily removed by continuous water, achieving a long-lasting self-cleaning effect. DETAILED DESCRIPTION

[0020] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of the heat-insulating self-cleaning transparent coating prepared in the following examples are as follows:

[0022] Heat insulation: Take the embodiment and comparative example of the same size, place an infrared lamp with a power of 250W 50 cm above them to simulate light, and use corrugated boards around them to isolate air circulation. Record the temperature on both sides of the glass until the temperature stabilizes and no longer rises, and record the temperature difference on both sides.

[0023] Self-cleaning: Take the embodiment and the comparative example of the same size, drop a mixture consisting of hydrophobic pollutant silicone oil and carbon powder on the surface of the coated glass slide, slowly drip deionized water, and record the residual degree of pollutants on the glass slide; place it outdoors for 100 days, and then test the residual degree of pollutants on the glass slide again.

[0024] Transparency: Take the embodiment and comparative example of the same size and refer to GB / T12997 to test their transmittance in the visible light range.

[0025] Example 1

[0026] (1) Tin tetrachloride pentahydrate, hexamethylenetetramine, indium chloride, and deionized water were mixed in a mass ratio of 1:1.5:3:1000, and stirred at 100 rpm for 25 min to obtain an indium-doped tin oxide precursor solution; a glass sheet was pretreated by first soaking it in a 5 wt % sodium hydroxide aqueous solution for 4 h, then rinsing it with deionized water for 3 times, soaking it in a 0.5 wt % potassium dichromate aqueous solution for 24 h, and then ultrasonically washing it with deionized water at 21 kHz for 10 min, then washing it with anhydrous ethanol for 3 times, drying it at 50° C. for 1 h, and then coating the indium-doped tin oxide precursor solution on it by pulling and coating, with a downward speed of 0.15 mm / s, an upward speed of 0.05 mm / s, a residence time of 8 min, and drying it at 50° C. for 2 h. The coating step was repeated 3 times, and finally annealing was performed at 220° C. for 8 min to obtain a glass sheet covered with indium-doped tin oxide seeds;

[0027] (2) Tin tetrachloride pentahydrate, hexamethylenetetramine, indium chloride, and deionized water were mixed in a mass ratio of 1:1.5:3:1000, stirred at 100 rpm for 25 min, and ethylene glycol with a mass of 0.3 times that of hexamethylenetetramine was added and mixed to obtain a growth solution; a glass sheet coated with indium-doped tin oxide seeds was immersed in the growth solution, heated to 60° C., subjected to a hydrothermal reaction for 24 h, washed with deionized water three times, and dried at 50° C. for 2.5 h to obtain a glass sheet coated with indium-doped tin oxide;

[0028] (3) Mixing polyethyleneimine with a molecular weight of 10,000 and deionized water, stirring at 300 rpm for 10 min, adding 3-ethoxycatechol, heating to 55° C. under a nitrogen atmosphere, stirring at 100 rpm for 100 min, adding 1,3-propane sultone, and continuing to stir for 10 h, and then adjusting the solution pH to 7.8 with sodium hydroxide solution to obtain a zwitterionic polymer; the mass ratio of polyethyleneimine with a molecular weight of 10,000, deionized water, 3-ethoxycatechol, and 1,3-propane sultone is 2:300:0.1:0.8;

[0029] (4) The zwitterionic polymer was added at 15 g / m 2 The glass sheet covered with indium-doped tin oxide was inverted and ultrasonically treated at a frequency of 21 kHz for 10 min and cured at 30°C for 6 h to obtain a heat-insulating and self-cleaning transparent coating.

[0030] Example 2

[0031] (1) Tin tetrachloride pentahydrate, hexamethylenetetramine, indium chloride, and deionized water were mixed in a mass ratio of 3:1.5:4.5:1000, and stirred at 200 rpm for 40 min to obtain an indium-doped tin oxide precursor solution; a glass sheet was pretreated by first soaking it in a 5 wt % sodium hydroxide aqueous solution for 4 h, then rinsing it with deionized water for 5 times, soaking it in a 0.5 wt % potassium dichromate aqueous solution for 24 h, and then ultrasonically washing it with deionized water at 21 kHz for 20 min, then washing it with anhydrous ethanol for 5 times, drying it at 60° C. for 2 h, and then coating the indium-doped tin oxide precursor solution on it by pulling and coating, with a downward speed of 0.18 mm / s, an upward speed of 0.09 mm / s, a residence time of 11 min, and drying it at 60° C. for 3 h. The coating step was repeated 5 times, and finally annealing was performed at 240° C. for 12 min to obtain a glass sheet covered with indium-doped tin oxide seeds;

[0032] (2) Tin tetrachloride pentahydrate, hexamethylenetetramine, indium chloride, and deionized water were mixed in a mass ratio of 3:1.5:4.5:1000, stirred at 200 rpm for 33 min, and ethylene glycol with a mass of 0.3 times that of hexamethylenetetramine was added and mixed to obtain a growth solution; a glass sheet coated with indium-doped tin oxide seeds was immersed in the growth solution, heated to 75° C., subjected to a hydrothermal reaction for 24 h, washed with deionized water 5 times, and dried at 65° C. for 3.5 h to obtain a glass sheet coated with indium-doped tin oxide;

[0033] (3) Mixing polyethyleneimine with a molecular weight of 10,000 and deionized water, stirring at 400 rpm for 20 min, adding 3-ethoxycatechol, heating to 63° C. under a nitrogen atmosphere, stirring at 150 rpm for 150 min, adding 1,3-propane sultone, and continuing to stir for 12 h, and then adjusting the solution pH to 8.2 with sodium hydroxide solution to obtain a zwitterionic polymer; the mass ratio of polyethyleneimine with a molecular weight of 10,000, deionized water, 3-ethoxycatechol, and 1,3-propane sultone is 3:400:0.3:1.1;

[0034] (4) The zwitterionic polymer was added at 22 g / m 2 The glass sheet covered with indium-doped tin oxide was inverted and ultrasonically treated at a frequency of 22 kHz for 20 min and cured at 45°C for 8 h to obtain a heat-insulating and self-cleaning transparent coating.

[0035] Example 3

[0036] (1) Tin tetrachloride pentahydrate, hexamethylenetetramine, indium chloride, and deionized water were mixed in a mass ratio of 5:1.5:6:1000, and stirred at 300 rpm for 50 min to obtain an indium-doped tin oxide precursor solution; a glass sheet was pretreated by first soaking it in a 5 wt % sodium hydroxide aqueous solution for 4 h, then rinsing it with deionized water for 6 times, soaking it in a 0.5 wt % potassium dichromate aqueous solution for 24 h, and then ultrasonically washing it with deionized water at 21 kHz for 30 min, then washing it with anhydrous ethanol for 6 times, drying it at 80° C. for 3 h, and then coating the indium-doped tin oxide precursor solution on it by pulling and coating, with a downward speed of 0.2 mm / s, an upward speed of 0.1 mm / s, a residence time of 15 min, and drying it at 70° C. for 4 h. The coating step was repeated 6 times, and finally annealing was performed at 260° C. for 15 min to obtain a glass sheet covered with indium-doped tin oxide seeds;

[0037] (2) Tin tetrachloride pentahydrate, hexamethylenetetramine, indium chloride, and deionized water were mixed in a mass ratio of 5:1.5:6:1000, stirred at 300 rpm for 50 min, and ethylene glycol with a mass of 0.3 times that of hexamethylenetetramine was added and mixed to obtain a growth solution; a glass sheet coated with indium-doped tin oxide seeds was immersed in the growth solution, heated to 90° C., subjected to a hydrothermal reaction for 24 h, washed with deionized water 8 times, and dried at 80° C. for 5 h to obtain a glass sheet coated with indium-doped tin oxide;

[0038] (3) Mixing polyethyleneimine with a molecular weight of 10,000 and deionized water, stirring at 600 rpm for 30 min, adding 3-ethoxycatechol, heating to 70° C. under a nitrogen atmosphere, stirring at 200 rpm for 200 min, adding 1,3-propane sultone, and continuing to stir for 15 h, and then adjusting the solution pH to 8.5 with sodium hydroxide solution to obtain a zwitterionic polymer; the mass ratio of polyethyleneimine with a molecular weight of 10,000, deionized water, 3-ethoxycatechol, and 1,3-propane sultone is 4:500:0.5:1.4;

[0039] (4) The zwitterionic polymer was added at 30 g / m 2 The glass sheet covered with indium-doped tin oxide was inverted and ultrasonically treated at a frequency of 25 kHz for 30 min and cured at 60° C. for 10 h to obtain a heat-insulating and self-cleaning transparent coating.

[0040] Comparative Example 1

[0041] The difference between Comparative Example 1 and Example 2 is that step (2) is different. Step (2) is changed to: immerse the glass sheet covered with indium-doped tin oxide seeds in an indium-doped tin oxide precursor solution, heat to 75°C, undergo hydrothermal reaction for 24 hours, wash with deionized water 5 times, and dry at 65°C for 3.5 hours to obtain a glass sheet covered with indium-doped tin oxide; the remaining steps are the same as Example 2.

[0042] Comparative Example 2

[0043] The difference between Comparative Example 2 and Example 2 is that there is no step (1) and step (2), and step (4) is changed to: the glass sheet is pretreated by soaking it in a 5wt% sodium hydroxide aqueous solution for 4 hours, then rinsing it with deionized water for 5 times, soaking it in a 0.5wt% potassium dichromate aqueous solution for 24 hours, then ultrasonically washing it with deionized water at 21kHz for 20 minutes, then washing it with anhydrous ethanol for 5 times, drying it at 60°C for 2 hours, and then rinsing it with a zwitterionic polymer at 22g / m 2 Place the mixture upside down on a glass sheet and cure it at 45° C. for 8 hours to obtain a heat-insulating, self-cleaning transparent coating. The remaining steps are the same as those in Example 2.

[0044] Comparative Example 3

[0045] The difference between Comparative Example 3 and Example 2 is that step (3) is different. Step (3) is changed to: polyethyleneimine with a molecular weight of 10,000 and deionized water are mixed, stirred at 400 rpm for 20 min, 1,3-propane sultone is added, stirred at 150 rpm for 12 h, and then the pH of the solution is adjusted to 8.2 with sodium hydroxide solution to obtain a zwitterionic polymer; the mass ratio of polyethyleneimine with a molecular weight of 10,000, deionized water, and 1,3-propane sultone is 3:400:1.1; the remaining steps are the same as Example 2.

[0046] Comparative Example 4

[0047] The difference between Comparative Example 4 and Example 2 is that step (3) is different. Step (3) is changed to: polyethyleneimine with a molecular weight of 10,000 and deionized water are mixed, stirred at 400 rpm for 20 min, 3-ethoxycatechol is added, and the temperature is raised to 63° C. under a nitrogen atmosphere, and stirred at 150 rpm for 150 min. The pH of the solution is adjusted to 8.2 with a sodium hydroxide solution to obtain a zwitterionic polymer; the mass ratio of polyethyleneimine with a molecular weight of 10,000, deionized water, and 3-ethoxycatechol is 3:400:0.3; the remaining steps are the same as in Example 2.

[0048] Comparative Example 5

[0049] The difference between Comparative Example 5 and Example 2 is that step (4) is different. Step (4) is changed to: the zwitterionic polymer is mixed at 22 g / m 2 The coating was inverted onto a glass sheet covered with indium-doped tin oxide and cured at 45° C. for 8 h to obtain a heat-insulating, self-cleaning, transparent coating. The remaining steps were the same as in Example 2.

[0050] Comparative Example 6

[0051] The difference between Comparative Example 6 and Example 2 is that step (3) and step (4) are omitted; the remaining steps are the same as those of Example 2.

[0052] Effect example

[0053] Table 1 below shows the performance analysis results of the heat-insulating and self-cleaning transparent coatings of Examples 1 to 3 of the present invention and Comparative Examples 1 to 6.

[0054] Table 1

[0055]

[0056]

[0057] From the comparison of the experimental results of the embodiment and the comparative example in Table 1, it can be found that the present invention uses tin tetrachloride pentahydrate and indium chloride to grow indium-doped tin oxide seeds on a glass substrate, and then uses oxalic acid to assist the hydrothermal growth liquid to make the generated indium hydroxide and tin hydroxide nucleate and grow on the indium-doped tin oxide seeds, wherein ethylene glycol controls the growth of the particles and promotes the growth of other surfaces, so that the obtained crystals no longer grow excessively along a certain direction, and the shape changes from the long strip of log to a regular square, thereby obtaining uniform and orderly nanoparticles, and having a strong reflective ability for the infrared light of thermal radiation, so that the coating achieves thermal insulation performance, and then, through 3-ethoxycatechol, 1,3-propane sultone is grafted, and polyethylene glycol is used to form a nanoparticle. Amines form zwitterionic polymers, which are coated on the substrate by reverse coating. After ultrasound, they fill the gaps between the particles, so that the obtained coating is smooth and bubble-free, and the light transmittance of the coating is enhanced. The oxygen on the ketone group in 1,3-propane sultone and the hydrogen ion on the amino group at the β position of polyethylene imine form a five-membered ring structure through intramolecular hydrogen bonds, which increases the proportion of strong hydrogen bonds in the matrix. The ethoxy group in 3-ethoxycatechol protects the functional groups in the matrix, making the strong hydrogen bonds more stable, and cooperates with electrostatic effects to enhance the interaction between it and water molecules, thereby forming a stable and dense hydration layer structure, reducing the affinity of pollutants to the coating, and then the oil stains are easily removed by continuous water, achieving a long-lasting self-cleaning effect.

[0058] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A heat-insulating self-cleaning transparent coating, characterized in that: The heat-insulating and self-cleaning transparent coating is prepared by combining an indium-doped tin oxide layer with a zwitterionic polymer layer.

2. A method for preparing a heat-insulating self-cleaning transparent coating, characterized in that: The method comprises the following preparation steps: (1) Pre-treating a glass sheet, and then coating the glass sheet with an indium-doped tin oxide precursor solution by Czochralski coating, drying at 50-70° C. for 2-4 hours, repeating the coating step 3-6 times, and finally annealing at 220-260° C. for 8-15 minutes to obtain a glass sheet coated with indium-doped tin oxide seeds; (2) immersing the glass sheet covered with indium-doped tin oxide seeds in a growth solution, subjecting it to a hydrothermal reaction, washing it with deionized water for 3 to 8 times, and drying it at 50 to 80° C. for 2.5 to 5 hours to obtain a glass sheet covered with indium-doped tin oxide; (3) Mix polyethyleneimine and deionized water, stir at 300-600 rpm for 10-30 min, add 3-ethoxycatechol, raise the temperature to 55-70° C. under nitrogen atmosphere, stir at 100-200 rpm for 100-200 min, add 1,3-propane sultone, continue stirring for 10-15 h, and then adjust the solution pH to 7.8-8.5 with sodium hydroxide solution to obtain a zwitterionic polymer; (4) The zwitterionic polymer is mixed at 15 to 30 g / m 2 The glass sheet covered with indium-doped tin oxide is placed upside down, and after ultrasonic treatment, it is cured at 30-60° C. for 6-10 hours to obtain a heat-insulating and self-cleaning transparent coating.

3. The method for preparing a heat-insulating self-cleaning transparent coating according to claim 2, characterized in that: The glass pretreatment method of step (1) is as follows: the glass sheet is immersed in a 5wt% sodium hydroxide aqueous solution for 4 hours, then rinsed with deionized water for 3 to 6 times, immersed in a 0.5wt% potassium dichromate aqueous solution for 24 hours, then ultrasonically washed with deionized water at 21kHz for 10 to 30 minutes, then washed with anhydrous ethanol for 3 to 6 times, and dried at 50 to 80°C for 1 to 3 hours.

4. The method for preparing a heat-insulating self-cleaning transparent coating according to claim 2, characterized in that: The preparation method of the indium-doped tin oxide precursor solution in step (1) is as follows: tin tetrachloride pentahydrate, hexamethylenetetramine, indium chloride, and deionized water are mixed in a mass ratio of 1-5:1.5:3-6:1000, and stirred at 100-300 rpm for 25-50 min to obtain the product.

5. The method for preparing a heat-insulating self-cleaning transparent coating according to claim 2, characterized in that: In step (1), the downward speed of the coating pulling process is 0.15 to 0.2 mm / s, the upward speed is 0.05 to 0.1 mm / s, and the residence time is 8 to 15 min.

6. The method for preparing a heat-insulating self-cleaning transparent coating according to claim 2, characterized in that: The preparation method of the growth solution in step (2) is as follows: tin tetrachloride pentahydrate, hexamethylenetetramine, indium chloride and deionized water are mixed in a mass ratio of 1-5:1.5:3-6:1000, stirred at 100-300 rpm for 25-50 min, and ethylene glycol in an amount of 0.3 times the mass of hexamethylenetetramine is added, and mixed to obtain the solution.

7. The method for preparing a heat-insulating self-cleaning transparent coating according to claim 2, characterized in that: The conditions of the hydrothermal reaction in step (2) are: temperature of 60-90° C. and time of 24 h.

8. The method for preparing a heat-insulating self-cleaning transparent coating according to claim 2, characterized in that: The molecular weight of the polyethyleneimine in step (3) is 10,000.

9. The method for preparing a heat-insulating self-cleaning transparent coating according to claim 2, characterized in that: The mass ratio of the polyethyleneimine, deionized water, 3-ethoxycatechol and 1,3-propane sultone in step (3) is 2-4:300-500:0.1-0.5:0.8-1.

4.