Fluidized solidified soil as well as preparation method and application construction method thereof

By mixing rock weathered soil or pore-formed slag with curing agent to form fluid solidified soil, it is used for foundation pit construction, and the problems of high cost of slag treatment and environmental pollution are solved, and high-strength and low-pollution bite pile support are achieved Protection effect.

CN118993685APending Publication Date: 2024-11-22SHENZHEN HONGYEJI GEOTECHNICAL TECH CO LTD
View PDF 0 Cites 5 Cited by

Patent Information

Application Number
CN202411100954.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The cost of transporting and disposal of slag generated during foundation pit construction is high and polluted the environment. The concrete of the existing bite pile support material is high and the environmental pollution is serious.

Method used

Flow-state solidified soil is used to mix rock weathered soil or pore-formed slag with curing agents such as cement, slag powder, fly ash, silicon powder and water glass to form fluid-state solidified soil with high strength and anti-seepage properties. It is poured into the plain pile position, and after curing, it is solidified to form a bite pile.

Benefits of technology

It significantly reduces the cost of slag treatment, realizes the resource utilization of slag, and provides a green construction plan. The strength of the fluid solidified soil is higher than that of traditional concrete, with significant anti-seepage effect, and is suitable for foundation pit support construction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993685A_ABST
    Figure CN118993685A_ABST
Patent Text Reader

Abstract

The invention provides flow-state solidified soil as well as a preparation method and an application construction method thereof, and relates to the technical field of civil engineering. The flow-state solidified soil comprises rock weathered soil and / or pore-forming muck and further comprises a curing agent, and the curing agent comprises cement, superfine slag powder, fly ash, silicon powder, a water reducing agent and water glass. Rock weathered soil or field pore-forming muck is used as a main material of flow-state solidified soil, and the main material is solidified through cement, superfine slag powder and fly ash; various rock weathered soil or field pore-forming muck generated by excavation of a foundation pit is adopted as a main component, engineering muck generated in urban construction can be consumed on a large scale, a new thought is provided for treatment and solving of the engineering muck, and the engineering muck can be recycled and utilized in a green and pollution-free mode; the strength of the poured flow-state solidified soil is higher than that of concrete and is higher than that of a traditional concrete plain pile.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of civil engineering, and in particular to a fluidized solidified soil and a preparation method and an application construction method thereof. Background Art

[0002] In recent years, with the adjustment of national strategies, the coastal areas have developed rapidly. In the process of rapid urban construction and development, high-rise buildings have sprung up, requiring a large amount of foundation pit support construction. Interlocking pile support is an extremely common form of foundation pit support. Because it adopts interlocking piles and interlocking piles, interlocking piles have both the function of retaining soil and preventing seepage.

[0003] The concrete used for casting interlocking piles is mostly composed of cement, crushed stone, medium-coarse sand, etc., which has a high cost. In addition, a large amount of granite weathered soil and other types of rock weathered soil or on-site bored soil will be generated during the foundation pit construction process before the interlocking pile support. These need to be transported and disposed of, which is costly and pollutes the environment. Summary of the invention

[0004] The problem solved by the invention is how to solve the problem of high cost and environmental pollution when the slag generated during the foundation pit construction is transported and discarded.

[0005] In order to solve the above problems, the present invention provides a fluidized solidified soil and a preparation method and an application construction method thereof.

[0006] In a first aspect, the present invention provides a fluidized solidified soil, including rock weathered soil and / or porous slag soil, and also includes a curing agent, and the curing agent includes cement, slag powder, fly ash, silica fume, water reducing agent and water glass.

[0007] Optionally, the curing agent includes, by weight, 12-30 parts of cement, 35-75 parts of slag powder, 6-16 parts of fly ash, 13-21 parts of silica fume, 0.05-10 parts of water reducing agent and 2-10 parts of water glass.

[0008] Optionally, the fluidized solidified soil also includes water, and the rock weathered soil and / or porous slag soil are mixed in the water to obtain slag mud. By weight, the fluidized solidified soil includes 70-85 parts of slag mud and 15-30 parts of curing agent.

[0009] Optionally, the fluidized solidified soil also includes waste mud, and rock weathered soil and / or porous slag are mixed in the waste mud to obtain slag mud, the weight of rock weathered soil and / or porous slag accounts for 16%-25% of the waste mud. By weight, the fluidized solidified soil includes 70-85 parts of slag mud and 15-30 parts of curing agent.

[0010] Optionally, the rock-weathered soil is granite-weathered soil.

[0011] Optionally, the modulus of the water glass is 2.6-3.0.

[0012] Optionally, the specific gravity of the fluidized solidified soil is 1.25-1.4.

[0013] In a second aspect, the present invention provides a method for preparing the fluidized solidified soil as described in any one of the above items, comprising the following steps:

[0014] S1: rock weathered soil or porous slag soil is mixed with water or waste mud to obtain slag mud;

[0015] S2: adding cement, slag powder, fly ash and silica fume to the slag slurry, stirring and mixing for 30-45 minutes to obtain a mixed slurry;

[0016] S3: adding a water reducing agent to the mixed slurry of step S2, stirring for 15-30 minutes to obtain a water reducing slurry;

[0017] S4: Add water glass to the water-reducing slurry of step S3, and stir for 3-5 minutes to obtain fluidized solidified soil.

[0018] Optionally, in step S2, slag powder and fly ash are mixed in advance to obtain premixed powder, cement, premixed powder and silica powder are added to the slag slurry, and stirred for 30-45 minutes. The specific surface area of ​​the premixed powder is ≥400m 2 / kg.

[0019] In a third aspect, the present invention provides an application construction method of the fluidized solidified soil as described in any of the above items, comprising the following steps: pouring the fluidized solidified soil into the pile position, and curing and hardening the fluidized solidified soil to form an interlocking pile after curing.

[0020] The beneficial effects of the fluidized solidified soil and its preparation method and application construction method of the present invention are as follows: by using rock weathered soil or on-site pore-forming slag as the main material of the fluidized solidified soil, cement, slag powder and fly ash are used for solidification treatment, and silicon powder and water reducing agent are used to improve its strength, impermeability, wear resistance and other properties. Through the mutual coordination of various components, the solidification effect of the fluidized solidified soil can be significantly improved. The water glass used can greatly increase the anti-seepage effect of the fluidized solidified soil after pouring, and can reach 10 -7cm / s level, which ensures its normal performance and meets the construction requirements of interlocking piles; various types of rock weathered soil or on-site pore-forming slag produced by foundation pit excavation are used as the main components, which can absorb the engineering slag produced in urban construction on a large scale, providing a new idea for the treatment and solution of engineering slag, so that it can be resourced and used green and pollution-free; the strength of fluidized solidified soil after pouring is greater than that of concrete, and the strength can reach 15Mpa in 28 days, which is higher than that of traditional concrete piles, and its elastic modulus is not less than 22000N / mm 2 , the effect is better than traditional plain piles. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 Flow chart of the method for preparing fluidized solidified soil of this embodiment. DETAILED DESCRIPTION

[0022] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. Although certain embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be interpreted as being limited to the embodiments described herein. On the contrary, these embodiments are provided to provide a more thorough and complete understanding of the present invention. It should be understood that the drawings and embodiments of the present invention are only for exemplary purposes and are not intended to limit the scope of protection of the present invention.

[0023] Unless otherwise defined, all technical and scientific terms used in this application have the same meanings as those commonly understood by those skilled in the art to which this application belongs; the terms used in the specification of this application are only for the purpose of describing specific implementation methods and are not intended to limit this application;

[0024] The term "including" and its variations used in this article are open inclusions, that is, "including but not limited to"; the term "based on" is "based at least in part on"; the term "one embodiment" means "at least one embodiment"; the term "another embodiment" means "at least one other embodiment"; the term "some embodiments" means "at least some embodiments"; the term "optionally" means "optional embodiments". The relevant definitions of other terms will be given in the following description. It should be noted that the concepts of "first" and "second" mentioned in the present invention are used to distinguish different objects, rather than to describe a specific order or a primary and secondary relationship. In addition, the terms "first" and "second" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of this application, unless otherwise specified, the meaning of "multiple" is two or more.

[0025] In view of the problems existing in the above-mentioned related technologies, this embodiment provides a fluidized solidified soil and a preparation method and an application construction method thereof.

[0026] A fluidized solidified soil provided in an embodiment of the present invention includes weathered rock soil and / or porous slag soil, and also includes a curing agent, and the curing agent includes cement, slag powder, fly ash, silica fume, water reducing agent and water glass.

[0027] In this embodiment, rock weathered soil or on-site pore-forming slag soil is used as the main material of the fluidized solidified soil, and cement, slag powder, and fly ash are used for solidification treatment, and silicon powder and water reducing agent are used to improve its strength, impermeability, wear resistance and other properties. Through the coordinated effect of each component, the solidification effect of the fluidized solidified soil can be significantly improved. The water glass used can greatly increase the anti-seepage effect of the fluidized solidified soil after pouring, and can reach 10 -7 cm / s level, which ensures its normal performance and meets the construction requirements of interlocking piles; various types of rock weathered soil or on-site pore-forming slag produced by foundation pit excavation are used as the main components, which can absorb the engineering slag produced in urban construction on a large scale, providing a new idea for the treatment and solution of engineering slag, so that it can be resourced and used green and pollution-free; the strength of fluidized solidified soil after pouring is greater than that of concrete, and the strength can reach 15Mpa in 28 days, which is higher than that of traditional concrete piles, and its elastic modulus is not less than 22000N / mm 2 , the effect is better than traditional plain piles.

[0028] Specifically, the weathered rock soil or porous slag formed during the foundation pit excavation project is used. The weathered rock soil or porous slag that is difficult to handle generated during the construction is collected, soaked and sieved at the construction site to screen out particles larger than 5 mm; ordinary Portland cement 42.5 is used as cement; the silicon powder is collected and treated by a special capture device during the high-temperature smelting of industrial silicon and ferrosilicon in an industrial electric furnace, and the smoke escaping with the exhaust gas is collected and treated by a special capture device, and the SiO2 content in the silicon powder is not less than 85%; the water reducer can be a naphthalene-based water reducer, which has the appearance of brown-yellow powder and a brown-brown viscous liquid.

[0029] Refer to the following formulas ① to ⑥. Silica powder and other ingredients build the overall "skeleton" framework based on hydration reactions. The main components of the built "skeleton" are hydrated calcium silicate (CSH) and some calcium aluminate (AFt). Rock weathered soil or porous slag belongs to clay, in which the soil particles are neutrally charged and the particle surface is negatively charged. Under the action of static gravity, the surface of rock weathered soil or porous slag will form an electric layer corresponding to a layer of charged and a layer of positively charged hydrated cations. The attracted cations will move in the opposite direction due to the molecular concentration gradient and thermal motion. During the cation adsorption and diffusion process, a hydrated cation layer in a diffused state will be formed on the surface of the rock weathered soil or porous slag. This state is the double electron layer of the rock weathered soil or porous slag. After the curing agent is added, subsequent reactions continue to produce ion exchange, hardening reaction, and carbonation reaction to fill the "skeleton" generated by a series of hydration reactions. The cations increase, and the high-charge Ca 2+ 、Al 3+ The cations replace the previous Na + The cations make the double layer thinner, thereby weakening the double layer, shortening the distance between clay particles, reducing the plasticity of the solidified soil and increasing its strength, thereby increasing the intensity of the reaction.

[0030] Formula ①: 2(3CaO·SiO2)+6H2O→3CaO·2SiO2·3H2O+3Ca(OH)2

[0031] Formula ②: 2(2CaO·SiO2)+4H2O→3CaO·2SiO2·3H2O+Ca(OH)2

[0032] Formula ③: 3CaO·Al2O3+6H2O→3CaO·Al2O3·6H2O

[0033] Formula ④: 3CaSO4+3CaO·Al2O3+32H2O→3CaO·Al2O3·3CaSO4·32H2O

[0034] (hardening reaction).

[0035] Formula ⑤SiO2+Ca(OH)2+n H2O→CaO·SiO2·(n+1)H2O

[0036] Formula ⑥Al2O3+Ca(OH)2+n H2O→CaO·Al2O3·(n+1)H2O

[0037] Optionally, the curing agent includes, by weight, 12-30 parts of cement, 35-75 parts of slag powder, 6-16 parts of fly ash, 13-21 parts of silica fume, 0.05-10 parts of water reducing agent and 2-10 parts of water glass.

[0038] Optionally, the fluidized solidified soil also includes water, and the rock weathered soil and / or porous slag soil are mixed in the water to obtain slag mud. By weight, the fluidized solidified soil includes 70-85 parts of slag mud and 15-30 parts of curing agent.

[0039] Optionally, the fluidized solidified soil also includes waste mud, and rock weathered soil and / or porous slag are mixed in the waste mud to obtain slag mud, the weight of rock weathered soil and / or porous slag accounts for 16%-25% of the waste mud. By weight, the fluidized solidified soil includes 70-85 parts of slag mud and 15-30 parts of curing agent.

[0040] In this optional embodiment, the raw materials are mixed and stirred according to the ratio to form a uniform slurry, which is then poured into the pile position and solidified and hardened after curing to form an interlocking pile.

[0041] Optionally, the rock-weathered soil is granite-weathered soil.

[0042] In this optional embodiment, the weathered granite soil belongs to clay, in which the soil particles are neutrally charged and the surface of the particles is negatively charged. Under the action of static gravity, the surface layer of the weathered granite soil will form an electric layer corresponding to a layer of charged and a layer of positively charged hydrated cations. The attracted cations will move in the opposite direction due to the molecular concentration gradient and thermal motion. In the process of cation adsorption and diffusion movement, a hydrated cation layer in a diffused state will be formed on the surface of the weathered granite soil. This state is the double electron layer of the weathered granite soil.

[0043] Optionally, the modulus of the water glass is 2.6-3.0.

[0044] In this optional embodiment, the appearance of the water glass is a colorless, slightly colored, translucent or transparent viscous liquid. When the modulus is controlled at 2.6-3.0, the bonding strength and compressive strength are relatively high.

[0045] Optionally, the specific gravity of the fluidized solidified soil is 1.25-1.4.

[0046] In this optional embodiment, the fluidized solidified soil with a specific gravity of 1.25-1.4 is convenient for transportation to the construction site by a pump tanker.

[0047] An embodiment of the present invention provides a method for preparing fluidized solidified soil as described in any one of the above items, comprising the following steps:

[0048] S1: rock weathered soil and / or pore-forming slag soil is mixed with water or waste mud to obtain slag soil mud;

[0049] S2: adding cement, slag powder, fly ash and silica fume to the slag slurry, stirring and mixing for 30-45 minutes to obtain a mixed slurry;

[0050] S3: adding a water reducing agent to the mixed slurry of step S2, stirring for 15-30 minutes to obtain a water reducing slurry;

[0051] S4: Add water glass to the water-reducing slurry of step S3, and stir for 3-5 minutes to obtain fluidized solidified soil.

[0052] Specifically, S1: at the construction site, the difficult-to-handle granite weathered soil or various types of rock weathered soil or on-site hole-forming slag generated during construction are collected and soaked, sieved to remove particles larger than 5 mm, and stored in a storage tank. There are two mixing methods: one is to directly mix the granite weathered soil or various types of rock weathered soil or on-site hole-forming slag with water into a muddy state, at which time the slag content accounts for about 70-85% of the total weight; the other is to add the granite weathered soil or various types of rock weathered soil or on-site hole-forming slag to the waste mud on site, at which time its weight accounts for 16%-25% of the waste mud, and stir it evenly for not less than 40 minutes to obtain slag mud for standby use.

[0053] S2: After the slag slurry is prepared, add the corresponding curing agent, including cement, slag powder, fly ash, silica powder and water, and stir for 30-45 minutes.

[0054] (3) The Nai series water reducer should be prepared in advance before the mixing process. After the cement and other curing agents are added and mixed, add the water reducer solution according to the mass ratio after an interval of 5-10 minutes. After adding water glass, stir for 15-30 minutes.

[0055] (4) Water glass is the last reagent to be added, and the water glass is prepared in advance before the stirring process. After the water reducer is stirred, the water glass solution is added according to the mass ratio at an interval of about 5-10 minutes. After adding the water glass, stir for 3-5 minutes to obtain fluidized solidified soil.

[0056] Optionally, in step S2, slag powder and fly ash are mixed in advance to obtain premixed powder, cement, premixed powder and silica powder are added to the slag slurry, and stirred for 30-45 minutes. The specific surface area of ​​the premixed powder is ≥400m 2 / kg.

[0057] In this optional embodiment, slag powder and fly ash are mixed in advance and then added to solidify the slag slurry.

[0058] An application construction method of the fluidized solidified soil as described in any one of the above items is provided in an embodiment of the present invention, comprising the following steps: pouring the fluidized solidified soil into the pile position, and curing and hardening the fluidized solidified soil to form an interlocking pile.

[0059] Specifically, the specific gravity of the fluidized solidified soil after configuration is between 1.25 and 1.4, which is convenient for transportation to the construction site by a pump tanker.

[0060] The application construction method of fluidized solidified soil comprises the following steps:

[0061] 1. Site leveling and machine positioning: Before the construction of interlocking piles, the site needs to be leveled, and the crawler crane is driven to the vicinity of the pile position origin on the leveled site. The center of the chassis hole of the pipe rolling machine is concentric with the center of the pile position, and the pipe rolling machine is lowered and fixed.

[0062] 2. Tube drilling: During the tube drilling process, casing drilling and soil extraction from the casing are performed simultaneously without interfering with each other, which improves work efficiency. It has been measured that this type of drilling construction method has greatly improved efficiency compared to traditional rotary drilling.

[0063] 3. Pre-casting sequence: After the hole is formed, the crane hook lifts the conduit with a wire rope and puts it into the hole so that the bottom of the conduit is about 300-500mm away from the bottom of the hole. Then the crane lifts the hopper and the workers connect the hopper to the conduit.

[0064] 4. Before pouring: The fluidized solidified soil should be mixed in a mixing tank truck before pouring to ensure its fluidity. Before pouring the fluidized solidified soil, the laboratory should test whether its slump and visual quality meet the requirements. Only if they meet the requirements can on-site pouring be carried out.

[0065] During pouring: continuous pouring is required and it should not be stopped for any reason. The fluidized solidified soil should be poured while the casing is pulled up with a tube rolling machine. When the casing of about 4 meters is pulled out, the pouring of fluidized solidified soil and the pulling of the tube should be stopped. The 4-meter casing and the 6-meter conduit should be removed, and the hopper should be removed first. While removing the casing and conduit, the casing and conduit should be held with the large and small hooks of the crane, and the workers should go to unload them. After unloading, the hopper and conduit are connected with the crane. Then continue to pour the fluidized solidified soil, but do not pull out the tube, until the required fluidized solidified soil is completely poured into the casing. At this time, the crane lifts the hopper and conduit and removes them.

[0066] 5. Pulling the pipe: Use the crane hook to hook the wire rope connected to the casing, and the pipe rolling machine starts to pull the pipe upwards. The hook is lifted upwards at the same time until the casing is completely pulled up. The crane puts the casing on the open space next to it and unloads it. At this point, it becomes a bite pile. Maintain the pile and construct it according to the actual situation on site. If hard bite construction is used on site, the maintenance time is 14 days or more. If soft bite construction is used on site, the maintenance time is about 3 days before the pile construction can be carried out.

[0067] In this embodiment, the pipe rolling machine is used to construct the interlocking piles, and there is no need for mud wall protection. It can ensure that the construction site is clean and tidy. At the same time, the work efficiency of the pipe rolling machine construction is greatly improved. The strength of the pipe rolling machine after pouring with fluidized solidified soil is greater than that of concrete. The strength after 28 days can reach 15Mpa level, which is higher than that of traditional concrete piles, and its elastic modulus is not less than 22000N / mm 2 , it has better effect than traditional plain piles, so it is suitable for promotion.

[0068] Although the present invention is disclosed as above, the protection scope of the present invention is not limited thereto. Those skilled in the art may make various changes and modifications without departing from the spirit and scope of the present invention, and these changes and modifications will fall within the protection scope of the present invention.

Claims

1. A fluidized solidified soil, characterized in that: The invention comprises weathered rock soil and / or porous slag soil, and also comprises a curing agent, wherein the curing agent comprises cement, slag powder, fly ash, silica powder, a water reducing agent and water glass.

2. The fluidized solidified soil according to claim 1, characterized in that: In parts by weight, the curing agent includes 12-30 parts of cement, 35-75 parts of slag powder, 6-16 parts of fly ash, 13-21 parts of silica fume, 0.05-10 parts of water reducing agent and 2-10 parts of water glass.

3. The fluidized solidified soil according to claim 1, characterized in that: The fluidized solidified soil also includes water. The rock weathered soil or the porous slag soil is mixed in the water to obtain slag mud. In terms of weight, the fluidized solidified soil includes 70-85 parts of the slag mud and 15-30 parts of the curing agent.

4. The fluidized solidified soil according to claim 1, characterized in that: The fluidized solidified soil also includes waste mud, the rock weathered soil and / or the porous slag soil are mixed in the waste mud to obtain slag mud, the weight of the rock weathered soil and / or the porous slag soil accounts for 16%-25% of the waste mud, and the fluidized solidified soil includes 70-85 parts of the slag mud and 15-30 parts of the curing agent in parts by weight.

5. The fluidized solidified soil according to claim 1, characterized in that: The rock weathered soil is granite weathered soil.

6. The fluidized solidified soil according to claim 1, characterized in that: The modulus of the water glass is 2.6-3.

0.

7. The fluidized solidified soil according to claim 1, characterized in that: The specific gravity of the fluidized solidified soil is 1.25-1.

4.

8. A method for preparing fluidized solidified soil according to any one of claims 1 to 7, characterized in that: The following steps are involved: S1: mixing rock weathered soil or porous slag soil with water or waste mud to obtain slag mud; S2: adding cement, slag powder, fly ash and silica fume to the slag slurry, stirring and mixing for 30-45 minutes to obtain mixed slurry; S3: adding a water reducing agent to the mixed slurry of step S2, stirring for 15-30 minutes to obtain a water reducing slurry; S4: Add water glass to the water-reducing slurry of step S3, and stir for 3-5 minutes to obtain fluidized solidified soil.

9. The method for preparing fluidized solidified soil according to claim 8, characterized in that: Step S2: slag powder and fly ash are mixed in advance to obtain premixed powder, cement, the premixed powder and silicon powder are added to the slag slurry, and stirred for 30-45 minutes. The specific surface area of ​​the premixed powder is ≥400m 2 / kg.

10. An application construction method of the fluidized solidified soil according to any one of claims 1 to 7, characterized in that: The following steps are involved: The fluidized solidified soil is poured into the pile position of the plain pile, and after curing, it is solidified and hardened to form the occlusal plain pile.

Citation Information

Cited By

  • Sewage pond closed curing treatment method

    CN120247127A

  • Premixed high-strength flow-state solidified soil and preparation method thereof

    CN120328979A

  • Premixed high-strength fluidized solidified soil and preparation method thereof

    CN120328979B

  • Construction method for curing sewage in sewage pond by on-site dry-method mixing and curing soil

    CN120398218A

  • Multi-source solid-waste-based fluid-state solidified soil as well as preparation method and application thereof