Preparation method of ultra-high molecular weight narrow distribution poly-alpha-olefin

By using catalytic systems of organoboron compounds, bisphenoloxy metal complexes and organoaluminum compounds, the problem of difficult to prepare high molecular weight narrow distribution polyα-olefins in the prior art is solved, and efficient monomer utilization and polymerization activity are achieved , suitable for drag reducing agents in crude oil transportation.

CN118994450APending Publication Date: 2024-11-22SHAANXI COAL & CHEM TECH INST +1

Patent Information

Application Number
CN202411090794.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The prior art is difficult to prepare polyα-olefins with a molecular weight of over one million and a narrow distribution at a lower monomer-catalyst ratio, resulting in low polymerization activity, poor controllability and low monomer utilization, affecting their crude oil transportation. Drag reduction effect.

Method used

A-catalyzed by a specific structure of bisphenoloxy metal complex (such as a complex with a structure of formula I or II) using a catalytic system comprising an organoboron compound, a bisphenoloxy metal complex and optionally an organoaluminum compound. Homopolymerization of olefins enables the obtainment of high molecular weight polyolefins at a lower monomer and catalyst ratio, avoid chain transfer and improve monomer utilization.

Benefits of technology

Polyα-olefins with molecular weight over one million and narrow distribution were successfully prepared, which improved the monomer utilization rate and polymerization activity, significantly improved the drag reduction performance of the polymer, and was suitable for drag reduction agents in crude oil transportation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004986504530000021
    Figure BDA0004986504530000021
  • Figure BDA0004986504530000031
    Figure BDA0004986504530000031
  • Figure BDA0004986504530000051
    Figure BDA0004986504530000051
Patent Text Reader

Abstract

The invention provides a preparation method of ultra-high molecular weight narrow-distribution poly-alpha-olefin, which comprises the following steps: initiating polymerization reaction of alpha-olefin or derivative monomers thereof in a reaction medium under a catalytic system to obtain a poly-alpha-olefin homopolymer; the catalytic system comprises an organic boron compound, a bisphenol oxygen metal complex and an optional organic aluminum compound. The invention also provides poly-alpha-olefin with ultra-high molecular weight and narrow distribution. According to the application, the bisphenol oxygen-based metal complex with the structure as shown in the formula I or the formula II, the organic boron compound and the organic aluminum compound form a catalytic system to catalyze homopolymerization of alpha-olefin monomers, polyolefin with the molecular weight of over millions can be obtained at a relatively low ratio of the monomers to the catalyst, chain transfer does not exist in the system, and the molecular weight of the polyolefin can be over 10 millions. Therefore, the preparation of ultra-high molecular weight polyolefin is facilitated, and the monomer utilization rate is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and in particular to a method for preparing ultra-high molecular weight narrow distribution poly-alpha-olefin. Background Art

[0002] Long-chain α-olefin homopolymers are mainly used as drag reducers in crude oil pipelines to reduce the flow resistance of crude oil, thereby achieving energy saving and increased transportation. The molecular weight of over one million is the primary condition for the use of polyalphaolefins as drag reducers.

[0003] In 1979, high molecular weight poly alpha olefin developed by ConocoPhillips was used as a drag reducer on long-distance crude oil pipelines in Alaska, USA, which greatly reduced transportation costs and achieved great success. After that, hundreds of offshore and onshore oil pipelines began to use oil drag reducers. Since the 1980s, my country has begun to develop oil drag reducers. In 2000, China Petroleum Pipeline Company conducted pilot production and field experiments of EP drag reducers. However, the active ingredient poly alpha olefin in domestic drag reducers has a low molecular weight and a wide molecular weight distribution, and the drag reduction effect is not good.

[0004] The catalytic system composed of TiCl4 / AlR3 catalyzes the polymerization of 1-hexene and usually obtains oligomers and low molecular weight polymers (J.Am.Chem.Soc.1958,80,6549–6551.). In comparison, although the polymerization of 1-hexene catalyzed by TiCl3 / AlEt2Cl can obtain poly-1-hexene with a molecular weight of over one million, the polymerization activity is low and the controllability is poor (Macromolecules 1970,3,206–214.). The three-way catalytic system composed of TiCl3 / AlR2Cl / electron donor usually catalyzes the polymerization at low temperature to obtain a polymer with excellent drag reduction performance. Low temperature causes the viscosity of the polymerization system to further increase, the diffusion of monomers becomes difficult, and the polymerization is difficult to achieve a high monomer conversion rate (US Patent No.5504132(1996).). Summary of the invention

[0005] In view of this, the present invention provides a method for preparing ultra-high molecular weight narrow distribution poly-α-olefins. The method provided by the present invention can obtain polyolefins with a molecular weight of over one million and a narrow distribution at a relatively low monomer to catalyst ratio, and the monomer utilization rate is high.

[0006] The present application provides a method for preparing ultra-high molecular weight narrow distribution poly-alpha-olefin, comprising:

[0007] Initiating polymerization of α-olefin or its derivative monomers in a reaction medium under a catalytic system to obtain poly-α-olefin;

[0008] The catalyst system comprises an organic boron compound, a bisphenoloxy metal complex and an optional organic aluminum compound;

[0009] The bisphenoloxy metal complex has a structure of Formula I or Formula II:

[0010]

[0011] wherein M is selected from titanium, zirconium or hafnium;

[0012] R1, R2, R3 and R4 are independently selected from hydrogen, an alkyl group containing 1 to 30 carbon atoms, a cycloalkyl group containing 3 to 30 carbon atoms, an aryl-substituted alkyl group containing 7 to 30 carbon atoms, a silyl-substituted alkyl group containing 1 to 30 carbon atoms, an aryl group having a carbon number greater than or equal to 6, or a halogen; at least two of R1, R2, R3 and R4 are different and at least one is a halogen;

[0013] X is selected from hydrogen, an alkyl group containing 1 to 30 carbon atoms, an aryl-substituted alkyl group containing 7 to 30 carbon atoms, a silyl-substituted alkyl group containing 1 to 30 carbon atoms, a halogen, or an alkoxy group containing 1 to 30 carbon atoms;

[0014] Y is selected from one of N, S or O;

[0015] n is selected from an integer of 0 to 4; when Y is N, R5 and R6 are selected from hydrogen, an alkyl group containing 1 to 10 carbon atoms, or an aryl group having a carbon number greater than or equal to 6; m is selected from an integer of 0 to 4.

[0016] The present application comprises a bisphenoloxy metal complex having a structure of formula I or II, an organic boron compound, and an optional organic aluminum compound to form a catalyst system, which catalyzes the homopolymerization of α-olefin monomers. At a relatively low monomer to catalyst ratio, polyolefins with a molecular weight of over one million can be obtained, indicating that there is no chain transfer in the system, and thus it is more conducive to the preparation of ultra-high molecular weight polyolefins with a higher monomer utilization rate.

[0017] The present application uses α-olefins or their derivative monomers as raw materials, and the carbon chain length of the α-olefins or their derivative monomers is 4 to 10, including but not limited to 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tetradecene, 1-hexadecene or 1-eicosene, etc., preferably 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene or 1-decene.

[0018] The catalytic system provided by the present application comprises an organic boron compound, a bisphenoloxy metal complex and an optional organic aluminum compound, wherein the bisphenoloxy metal complex has a structure of Formula I or Formula II:

[0019] The bisphenoloxy metal complex has a structure of Formula I or Formula II:

[0020]

[0021] wherein M is selected from titanium, zirconium or hafnium;

[0022] R1, R2, R3 and R4 are independently selected from hydrogen, an alkyl group containing 1 to 30 carbon atoms, a cycloalkyl group containing 3 to 30 carbon atoms, an aryl-substituted alkyl group containing 7 to 30 carbon atoms, a silyl-substituted alkyl group containing 1 to 30 carbon atoms, an aryl group having a carbon number greater than or equal to 6, or a halogen; at least two of R1, R2, R3 and R4 are different and at least one is a halogen;

[0023] X is selected from hydrogen, an alkyl group containing 1 to 30 carbon atoms, an aryl-substituted alkyl group containing 7 to 30 carbon atoms, a silyl-substituted alkyl group containing 1 to 30 carbon atoms, a halogen, or an alkoxy group containing 1 to 30 carbon atoms;

[0024] Y is selected from one of N, S or O;

[0025] n is selected from an integer of 0 to 4; when Y is N, R5 and R6 are selected from hydrogen, an alkyl group containing 1 to 10 carbon atoms, or an aryl group having a carbon number greater than or equal to 6; m is selected from an integer of 0 to 4.

[0026] Compared with R1 to R4 being all chlorine or bromine, the present application makes at least two of R1, R2, R3 and R4 different and at least one is a halogen, which can improve the utilization rate of α-olefin monomers and obtain polyolefins with a molecular weight of over one million at a relatively low monomer to catalyst ratio.

[0027] In some specific implementations, R1, R2, R3 and R4 are independently selected from hydrogen, alkyl groups containing 1 to 30 carbon atoms, cycloalkyl groups containing 3 to 30 carbon atoms, aryl-substituted alkyl groups containing 7 to 30 carbon atoms, silyl-substituted alkyl groups containing 1 to 30 carbon atoms, aryl groups having a carbon number greater than or equal to 6, or halogens, preferably selected from hydrogen, alkyl groups containing 1 to 10 carbon atoms, cycloalkyl groups containing 3 to 10 carbon atoms, aryl-substituted alkyl groups containing 7 to 10 carbon atoms, silyl-substituted alkyl groups containing 1 to 10 carbon atoms, phenyl, Cl or Br, more preferably selected from hydrogen, alkyl groups containing 1 to 7 carbon atoms, cycloalkyl groups containing 3 to 7 carbon atoms, aryl-substituted alkyl groups containing 7 to 10 carbon atoms, silyl-substituted alkyl groups containing 1 to 7 carbon atoms, phenyl, Cl or Br.

[0028] In some specific implementations, at least two of R1, R2, R3 and R4 are different. Specifically, R1 and R2 may be different, or R1 and R3 or R4 may be different, or R2 and R3 or R4 may be different. This application has no special restrictions on this.

[0029] In some specific implementations, at least one of R1, R2, R3 and R4 is a halogen, preferably, at least two of R1, R2, R3 and R4 are halogens, preferably, at least one of R1, R2, R3 and R4 is Cl or Br.

[0030] In the structure of Formula I or Formula II, X is selected from hydrogen, an alkyl group containing 1 to 30 carbon atoms, an aryl-substituted alkyl group containing 7 to 30 carbon atoms, a silyl-substituted alkyl group containing 1 to 30 carbon atoms, a halogen or an alkoxy group containing 1 to 30 carbon atoms, preferably selected from hydrogen, an alkyl group containing 1 to 10 carbon atoms, an aryl-substituted alkyl group containing 7 to 10 carbon atoms, a silyl-substituted alkyl group containing 1 to 10 carbon atoms, a halogen or an alkoxy group containing 1 to 10 carbon atoms, more preferably selected from hydrogen, an alkyl group containing 1 to 7 carbon atoms, an aryl-substituted alkyl group containing 7 to 10 carbon atoms, a silyl-substituted alkyl group containing 1 to 7 carbon atoms, Cl, Br or an alkoxy group containing 1 to 7 carbon atoms.

[0031] In the structure of Formula I or Formula II, Y is selected from N, S or O.

[0032] In the structure of formula I, n is selected from an integer of 0 to 4, such as 1, 2, 3 or 4; when Y is N, R5 and R6 are selected from hydrogen, an alkyl group containing 1 to 10 carbon atoms, such as methyl, ethyl, propyl, or an aryl group having a carbon number greater than or equal to 6. In the structure of formula II, when Y is N, R5 and R6 are selected from hydrogen, an alkyl group containing 1 to 10 carbon atoms, such as methyl, ethyl, propyl, or an aryl group having a carbon number greater than or equal to 6; m is selected from an integer of 0 to 4, such as 1, 2, 3 or 4.

[0033] Specifically, the bisphenoloxy metal complex has structures of Formula 1 to Formula 16:

[0034]

[0035]

[0036] The present application has no particular limitation on the source of the bisphenoloxy metal complex. When Y is N, it can be synthesized and prepared according to the method disclosed in Organometallics 2009, 28, 1391-1405. When Y is S, it can be synthesized and prepared according to the method disclosed in Inorg. Chem. 2007, 46, 8114-8116.

[0037] Taking Y as N as an example, the amine shown in a is condensed with the salicylaldehyde compound shown in b to form compound c, which is then selectively reduced with sodium borohydride to form compound d. Compound d reacts with a phenol derivative e to form compound f, which is then reacted with compound g to form a complex shown in formula (IN). The reaction process is as follows:

[0038]

[0039] Alternatively, the bisphenoloxy metal complex shown in formula (II-N) can also be prepared according to the following method:

[0040]

[0041] When Y is S, it can also be prepared by the following method: the phenol compound shown in e-2, the phenol compound shown in e-3 and the thiol compound shown in h undergo nucleophilic substitution reaction to generate the compound shown in f-2, and then react with the compound shown in g to generate the complex shown in formula (III). The reaction process is as follows:

[0042]

[0043] Similarly, when Y is O, it can also be prepared according to any of the above methods, which will not be described in detail in this application.

[0044] In some specific implementations, in the catalytic system, the organoboron compound is selected from an ionic compound formed by an organoboron anion and a cation, wherein the organoboron anion is selected from tetraphenylborate ([BPh4] - ), tetrakis(monofluorophenyl)borate, tetrakis(difluorophenyl)borate, tetrakis(trifluorophenyl)borate, tetrakis(tetrafluorophenyl)borate, tetrakis(pentafluorophenyl)borate ([B(C6F5)4] - ), tetrakis(tetrafluoromethylphenyl)borate, tetrakis(tolyl)borate, tetrakis(xylyl)borate, (triphenyl, pentafluorophenyl)borate, [tris(pentafluorophenyl), phenyl]borate or undecanoic acid-7,8-dicarbonundecaborate; the cation is selected from carbonium cation, oxonium cation, ammonium cation, phosphonium cation, cycloheptatrienyl cation or ferrocenium cation containing transition metal; wherein the carbonium cation preferably comprises a trisubstituted carbonium cation such as a triphenylcarbonium cation ([Ph3C] + ) and tri(substituted phenyl)carbonium cations such as tri(tolyl)carbonium cations; the ammonium cations preferably include trialkylammonium cations such as trimethylammonium cations, triethylammonium cations ([NEt3H] +), tripropylammonium cation and tributylammonium cation; N,N-dialkylanilinium cation such as N,N-dimethylanilinium cation ([PhNMe2H] + ), N,N-diethylanilinium cation and N,N-2,4,6-pentamethylanilinium cation; dialkylammonium cations such as diisopropylammonium cation and dicyclohexylammonium cation; the phosphonium cation preferably includes triarylphosphonium cations such as triphenylphosphonium cation, tri(tolyl)phosphonium cation or tri(xylyl)phosphonium cation. In some specific implementations, the organic boron salt compound is preferably selected from [Ph3C][B(C6F5)4], [PhNMe2H][BPh4], [NEt3H][BPh4] or [PhNMe2H][B(C6F5)4]; organic boron compounds having the same function as the organic boron salt compound, such as B(C6F5)3, can also be used.

[0045] In some specific implementations, the organoaluminum compound is selected from trimethylaluminum, triethylaluminum, tripropylaluminum, tributylaluminum, triisopropylaluminum, triisobutylaluminum, tripentylaluminum, trihexylaluminum, tricyclohexylaluminum, trioctylaluminum, triphenylaluminum, tri-p-tolylaluminum, tribenzylaluminum, ethyldibenzylaluminum, methylaluminoxane or ethyldi(p-tolyl)aluminum.

[0046] In some specific implementations, the molar ratio of the organoboron compound, the organoaluminum compound and the bisphenoloxy metal complex is (0.5-10): (2-3000): (10-1), preferably (1-8): (5-300): (8-2). Specifically, when the organoboron compound is an organoboron salt, the molar ratio of the organoboron compound to the bisphenoloxy metal complex is preferably (1-10): (10-1), more preferably (2-8): (8-2), and most preferably (3-6): (6-3); when the organoboron compound is an organoboron compound such as B(C6F5)3, the molar ratio of the organoboron compound to the bisphenoloxy metal complex is preferably (0.5-10): 1, more preferably (1-8): 1, more preferably (2-6): 1, and most preferably 1:1. In some specific implementations, the molar ratio of the organoaluminum compound to the bisphenoloxy metal complex is preferably (2-300):1, more preferably (2-250):1, more preferably (2-200):1, more preferably (2-150):1, more preferably (2-120):1, and most preferably (2-20):1.

[0047] In some specific implementations, the catalytic system further comprises a solvent, and the solvent is preferably selected from α-olefins. The present application has no particular limitation on the amount of the solvent, and those skilled in the art can select an appropriate amount of solvent according to the amount known in the art and actual conditions to ensure the polymerization reaction proceeds.

[0048] In some specific implementations, the molar ratio of the α-olefin monomer to the bisphenoloxy metal complex is 10000 to 25000: 1, preferably 12000 to 20000: 1, and more preferably 13000 to 18000: 1. The present application can obtain polyolefins with a molecular weight of over one million at a relatively low monomer to catalyst ratio, and has a high monomer utilization rate.

[0049] In some specific implementations, the reaction medium is selected from one or more of aliphatic saturated hydrocarbons, aromatic hydrocarbons, α-olefins, aromatic halides and cycloalkanes, including but not limited to hexane, cyclohexane, benzene, toluene, xylene, chlorobenzene, dichlorobenzene, bromobenzene and α-olefins, etc., and can be one or more thereof. The present application has no particular restrictions on the amount of the reaction medium, and those skilled in the art can select an appropriate amount of the reaction medium according to actual conditions to ensure that the polymerization reaction can proceed.

[0050] The present application mixes α-olefin or its derivative monomer, catalytic system and reaction medium to carry out polymerization reaction. When α-olefin or its derivative monomer is also the reaction medium, no other reaction medium needs to be added. When α-olefin or its derivative monomer is also the reaction medium, in some specific implementations, the present application preferably dissolves the organoaluminum compound in the α-olefin or its derivative monomer to obtain an organoaluminum compound solution; dissolves the bisphenoloxy metal complex in the α-olefin or its derivative monomer to obtain a complex solution; dissolves the organoboron compound in the α-olefin or its derivative monomer to obtain an organoboron compound solution; and mixes the organoaluminum solution, the complex solution and the organoboron compound solution to carry out polymerization reaction. In some specific implementations, the temperature of the polymerization reaction is -20°C to 150°C, preferably -10 to 120°C, more preferably 10 to 90°C, more preferably 20 to 70°C, more preferably 20 to 50°C, and most preferably 20 to 30°C. The present application does not particularly limit the time of the polymerization reaction, which is selected according to the amount of catalyst used and the size of the reaction system. In some specific implementations, the polymerization reaction time is 1 minute to 10 days, preferably 10 minutes to 8 days, and more preferably 30 minutes to 7 days. Specifically, when the polymerization reaction is carried out in an intermittent reactor, the reaction time is 1 minute to 10 hours, preferably 10 minutes to 8 hours; when the polymerization reaction is carried out in a continuous reactor, the reaction time is 1 day to 10 days, preferably 2 days to 8 days.

[0051] After the reaction is completed, methanol hydrochloric acid solution is preferably added to terminate the reaction, and after the reaction is terminated, ethanol is preferably added to separate the polymer, and then dried to obtain poly-α-olefin. In some specific implementations, the drying method is preferably vacuum drying; the drying temperature is preferably 30-50°C, more preferably 35-45°C, and most preferably 40°C.

[0052] After the polymer is obtained, it is tested. The experimental results show that the number average molecular weight of the ultra-high molecular weight narrow distribution poly-α-olefin prepared by the method provided in the present application is greater than 1.0×10 6 ; Molecular weight distribution <2.5; Tacticity not higher than 90%. Based on this, the present application provides a poly-α-olefin with ultra-high molecular weight and narrow distribution that meets the above parameters. In some specific implementations, the number average molecular weight of the poly-α-olefin is preferably 1.0×10 6 ~4.0×10 6 , more preferably 1.2×10 6 ~4.0×10 6 , more preferably 1.2×10 6 ~3.0×10 6 ; The molecular weight distribution is preferably 1.0 to 2.0, more preferably 1.0 to 1.7, and most preferably 1.0 to 1.5; the stereoregularity is preferably 20% to 90%, more preferably 30% to 90%, and most preferably 40% to 90%.

[0053] This application uses α-olefins or α-olefin derivative monomers of different lengths and a catalyst system of a specific structure. At a relatively low ratio of monomer to catalyst, polyolefins with a molecular weight of over one million and a narrow molecular weight distribution can be obtained, which can be used as a crude oil drag reducer material, significantly improving the utilization rate of α-olefin or its derivative monomers. Experimental results show that when the ratio of monomer to catalyst is 13000:1, the above catalyst system can be used to catalyze the polymerization of α-olefins with carbon numbers ranging from 6 to 16, and polyolefins with a number average molecular weight of over one million can be obtained. The molecular weight distribution of the obtained polymer is relatively narrow, and the conversion rate of the monomer is higher than 70%. BRIEF DESCRIPTION OF THE DRAWINGS

[0054] Figure 1 This is a sample photo of the poly-α-olefin prepared in Example 3 of the present application;

[0055] Figure 2 The poly α-olefin sample prepared in Example 17 of the present invention 13 C NMR spectrum;

[0056] Figure 3 This is a GPC curve diagram of the poly-α-olefin sample prepared in Example 17 of the present invention;

[0057] Figure 4 The poly α-olefin sample prepared in Example 18 of the present invention 13 C NMR spectrum;

[0058] Figure 5 This is the GPC curve of the poly-α-olefin sample prepared in Example 19 of the present invention. DETAILED DESCRIPTION

[0059] It should be understood that the expression "one or more of..." includes each of the items recited after the expression individually and in various different combinations of two or more of the recited items, unless otherwise understood from the context and usage. The expression "and / or" in combination with three or more recited items should be understood to have the same meaning, unless otherwise understood from the context.

[0060] The use of the terms "comprising", "having" or "containing", including their grammatical synonyms, should generally be understood as open and non-restrictive, for example not excluding other unrecited elements or steps, unless otherwise specifically stated or otherwise understood from the context.

[0061] It should be understood that the order of steps or the order in which certain actions are performed is not important as long as the present invention remains operable. In addition, two or more steps or actions may be performed simultaneously.

[0062] The use of any and all examples or exemplary language, such as "for example" or "including", herein is intended only to better illustrate the invention and does not limit the scope of the invention unless otherwise claimed. No language in this specification should be construed as indicating that any non-claimed element is essential to the practice of the invention.

[0063] In addition, the numerical ranges and parameters used to define the present invention are approximate values, and the relevant values ​​in the specific embodiments have been presented as accurately as possible. However, any numerical value inherently inevitably contains standard deviations due to individual test methods. Therefore, unless otherwise expressly stated, it should be understood that all ranges, quantities, values ​​and percentages used in this disclosure are modified by "about". Here, "about" generally means that the actual value is within plus or minus 10%, 5%, 1% or 0.5% of a specific value or range.

[0064] The present application provides a method for preparing ultra-high molecular weight narrow distribution poly-alpha-olefin, comprising:

[0065] Initiating a polymerization reaction of α-olefin or its derivative monomer in a reaction medium under a catalytic system to obtain a poly-α-olefin homopolymer;

[0066] The catalytic system comprises an organic boron compound, an organic aluminum compound and a bisphenoloxy metal complex;

[0067] The bisphenoloxy metal complex has a structure of Formula I or Formula II:

[0068]

[0069]

[0070] wherein M is selected from titanium, zirconium or hafnium;

[0071] R1, R2, R3 and R4 are independently selected from hydrogen, an alkyl group containing 1 to 30 carbon atoms, a cycloalkyl group containing 3 to 30 carbon atoms, an aryl-substituted alkyl group containing 7 to 30 carbon atoms, a silyl-substituted alkyl group containing 1 to 30 carbon atoms, an aryl group having a carbon number greater than or equal to 6, or a halogen; at least two of R1, R2, R3 and R4 are different and at least one is a halogen;

[0072] X is selected from hydrogen, an alkyl group containing 1 to 30 carbon atoms, an aryl-substituted alkyl group containing 7 to 30 carbon atoms, a silyl-substituted alkyl group containing 1 to 30 carbon atoms, a halogen, or an alkoxy group containing 1 to 30 carbon atoms;

[0073] Y is selected from one of N, S or O;

[0074] n is selected from an integer of 0 to 4; when Y is N, R5 and R6 are selected from hydrogen, an alkyl group containing 1 to 10 carbon atoms, or an aryl group having a carbon number greater than or equal to 6; m is selected from an integer of 0 to 4.

[0075] The present application forms a catalytic system with a bisphenoloxy metal complex having a structure of Formula I or Formula II, an organic boron compound, and an organic aluminum compound to catalyze the homopolymerization of α-olefin monomers. Polyolefins with a molecular weight of over one million can be obtained at a relatively low monomer to catalyst ratio, indicating that there is no chain transfer in the system, which is more conducive to the preparation of ultra-high molecular weight polyolefins and has a higher monomer utilization rate.

[0076] The preparation method of the ultra-high molecular weight narrow distribution poly-α-olefin provided in the present application is further described below in conjunction with examples.

[0077] The complexes used in the following Examples 1 to 11 and 15 to 16 of the present invention were synthesized and prepared according to the method disclosed in Organometallics 2009, 28, 1391–1405. The complexes used in Examples 12 to 14 were synthesized and prepared according to the method disclosed in Inorg. Chem. 2007, 46, 8114-8116.

[0078] The complexes used in the following Examples 1 to 6 and 15-16 of the present invention are all prepared by the following method, and the specific process is as follows:

[0079] The amine shown in a is condensed with the salicylaldehyde compound shown in b to form compound c, which is then selectively reduced with sodium borohydride to form compound d. Compound d reacts with a phenol derivative e to form compound f, which is then reacted with compound g to generate a complex shown in formula (I). The substituents in each complex are shown in Table 1.

[0080]

[0081] The complexes used in the following Examples 7 to 11 of the present invention are prepared by the following method. The substituents in each complex are shown in Table 1.

[0082]

[0083] The complexes used in the following Examples 12 to 14 of the present invention are prepared by the following method, and the specific process is as follows:

[0084] The phenol compound shown in e-2, the phenol compound shown in e-3 and the thiol compound shown in h undergo nucleophilic substitution reaction to generate the compound shown in formula f-2, which then reacts with the compound shown in formula g to generate the complex shown in formula (III). The substituents in each complex are shown in Table 1.

[0085]

[0086] The substituents in each complex are shown in Table 1.

[0087] Table 1 Complex structures and raw materials for preparation

[0088]

[0089]

[0090] Example 1

[0091] In a glove box, weigh the complex of formula 1 (7.0 mg, 10 μmol) into a 50 mL cillin bottle, add 1-hexene (10.08 g, 0.12 mol) to fully dissolve the catalyst; weigh tri(pentafluorophenyl)borane B(C6F5)3 (5.2 mg, 10 μmol), add 1-hexene (0.84 g, 0.01 mol) to dissolve B(C6F5)3; under stirring, quickly add B(C6F5)3 solution to the complex solution, and the polymerization reaction begins. After 18 hours of reaction, immediately add 20 mL of methanol hydrochloric acid solution to terminate the reaction. Then add a large amount of ethanol to separate the copolymer, and vacuum dry the copolymer at 40°C until the polymer weight does not change.

[0092] Example 2

[0093] In a glove box, weigh the complex of formula 2 (7.1 mg, 10 μmol) into a 50 mL cillin bottle, add 1-hexene (10.08 g, 0.12 mol) to fully dissolve the catalyst; weigh tri(pentafluorophenyl)borane B(C6F5)3 (5.2 mg, 10 μmol), add 1-hexene (0.84 g, 0.01 mol) to dissolve B(C6F5)3; under stirring, quickly add B(C6F5)3 solution to the complex solution, and the polymerization reaction begins. After 18 hours of reaction, immediately add 20 mL of methanol hydrochloric acid solution to terminate the reaction. Then add a large amount of ethanol to separate the copolymer, and vacuum dry the copolymer at 40°C until the polymer weight does not change.

[0094] Example 3

[0095] In the glove box, weigh the complex of formula 3 (6.4 mg, 10 μmol) into a 50 mL vial, add 1-hexene (10.08 g, 0.12 mol) and Al i Bu3 (40μL, 0.5M, 20μmol) was added to fully dissolve the catalyst; tri(pentafluorophenyl)borane B(C6F5)3 (5.2mg, 10μmol) was weighed, 1-hexene (0.84g, 0.01mol) was added to dissolve B(C6F5)3; under stirring, the B(C6F5)3 solution was quickly added to the complex solution, and the polymerization reaction began. After 18h of reaction, 20mL of methanol-hydrochloric acid solution was immediately added to terminate the reaction. Then a large amount of ethanol was added to separate the copolymer, and the copolymer was vacuum dried at 40°C until the polymer weight did not change.

[0096] See also Figure 1 , Figure 1 This is a sample photo of the poly-α-olefin prepared in Example 3 of the present application.

[0097] Example 4

[0098] In a glove box, weigh the complex of formula 4 (8.0 mg, 10 μmol) into a 50 mL cillin bottle, add 1-hexene (10.08 g, 0.12 mol) to fully dissolve the catalyst; weigh tri(pentafluorophenyl)borane B(C6F5)3 (5.2 mg, 10 μmol), add 1-hexene (0.84 g, 0.01 mol) to dissolve B(C6F5)3; under stirring, quickly add B(C6F5)3 solution to the complex solution, and the polymerization reaction begins. After 18 hours of reaction, immediately add 20 mL of methanol hydrochloric acid solution to terminate the reaction. Then add a large amount of ethanol to separate the copolymer, and vacuum dry the copolymer at 40°C until the polymer weight does not change.

[0099] Example 5

[0100] In a glove box, weigh the complex of formula 5 (7.6 mg, 10 μmol) into a 50 mL vial, add 1-hexene (10.08 g, 0.12 mol) and Al i Bu3 (40μL, 0.5M, 20μmol) was added to fully dissolve the catalyst; tri(pentafluorophenyl)borane B(C6F5)3 (5.2mg, 10μmol) was weighed, 1-hexene (0.84g, 0.01mol) was added to dissolve B(C6F5)3; under stirring, the B(C6F5)3 solution was quickly added to the complex solution, and the polymerization reaction began. After 18h of reaction, 20mL of methanol-hydrochloric acid solution was immediately added to terminate the reaction. Then a large amount of ethanol was added to separate the copolymer, and the copolymer was vacuum dried at 40°C until the weight of the polymer did not change.

[0101] Example 6

[0102] In a glove box, weigh the complex of formula 6 (6.6 mg, 10 μmol) into a 50 mL cillin bottle, add 1-hexene (10.08 g, 0.12 mol) to fully dissolve the catalyst; weigh tri(pentafluorophenyl)borane B(C6F5)3 (5.2 mg, 10 μmol), add 1-hexene (0.84 g, 0.01 mol) to dissolve B(C6F5)3; under stirring, quickly add B(C6F5)3 solution to the complex solution, and the polymerization reaction begins. After 18 hours of reaction, immediately add 20 mL of methanol hydrochloric acid solution to terminate the reaction. Then add a large amount of ethanol to separate the copolymer, and vacuum dry the copolymer at 40°C until the weight of the polymer does not change.

[0103] Example 7

[0104] In a glove box, weigh the complex of formula 7 (7.7 mg, 10 μmol) into a 50 mL cillin bottle, add 1-hexene (10.08 g, 0.12 mol) to fully dissolve the catalyst; weigh tri(pentafluorophenyl)borane B(C6F5)3 (5.2 mg, 10 μmol), add 1-hexene (0.84 g, 0.01 mol) to dissolve B(C6F5)3; under stirring, quickly add B(C6F5)3 solution to the complex solution, and the polymerization reaction begins. After 18 hours of reaction, immediately add 20 mL of methanol hydrochloric acid solution to terminate the reaction. Then add a large amount of ethanol to separate the copolymer, and vacuum dry the copolymer at 40°C until the polymer weight does not change.

[0105] Example 8

[0106] In a glove box, weigh the complex of formula 8 (6.4 mg, 10 μmol) into a 50 mL cillin bottle, add 1-hexene (10.08 g, 0.12 mol) to fully dissolve the catalyst; weigh tri(pentafluorophenyl)borane B(C6F5)3 (5.2 mg, 10 μmol), add 1-hexene (0.84 g, 0.01 mol) to dissolve B(C6F5)3; under stirring, quickly add B(C6F5)3 solution to the complex solution, and the polymerization reaction begins. After 18 hours of reaction, immediately add 20 mL of methanol hydrochloric acid solution to terminate the reaction. Then add a large amount of ethanol to separate the copolymer, and vacuum dry the copolymer at 40°C until the polymer weight does not change.

[0107] Example 9

[0108] In a glove box, weigh the complex of formula 9 (8.4 mg, 10 μmol) into a 50 mL cillin bottle, add 1-hexene (10.08 g, 0.12 mol) to fully dissolve the catalyst; weigh tri(pentafluorophenyl)borane B(C6F5)3 (5.2 mg, 10 μmol), add 1-hexene (0.84 g, 0.01 mol) to dissolve B(C6F5)3; under stirring, quickly add the B(C6F5)3 solution to the complex solution, and the polymerization reaction begins. After 18 hours of reaction, immediately add 20 mL of methanol hydrochloric acid solution to terminate the reaction. Then add a large amount of ethanol to separate the copolymer, and vacuum dry the copolymer at 40°C until the polymer weight does not change.

[0109] Example 10

[0110] In a glove box, weigh the complex of formula 10 (6.6 mg, 10 μmol) into a 50 mL vial, add 1-hexene (10.08 g, 0.12 mol) and Al i Bu3 (40μL, 0.5M, 20μmol) was added to fully dissolve the catalyst; tri(pentafluorophenyl)borane B(C6F5)3 (5.2mg, 10μmol) was weighed, 1-hexene (0.84g, 0.01mol) was added to dissolve B(C6F5)3; under stirring, the B(C6F5)3 solution was quickly added to the complex solution, and the polymerization reaction began. After 18h of reaction, 20mL of methanol-hydrochloric acid solution was immediately added to terminate the reaction. Then a large amount of ethanol was added to separate the copolymer, and the copolymer was vacuum dried at 40°C until the polymer weight did not change.

[0111] Embodiment 11

[0112] In a glove box, weigh the complex of formula 11 (7.8 mg, 10 μmol) into a 50 mL vial, add 1-hexene (10.08 g, 0.12 mol) and Al i Bu3 (40μL, 0.5M, 20μmol) was added to fully dissolve the catalyst; tri(pentafluorophenyl)borane B(C6F5)3 (5.2mg, 10μmol) was weighed, 1-hexene (0.84g, 0.01mol) was added to dissolve B(C6F5)3; under stirring, the B(C6F5)3 solution was quickly added to the complex solution, and the polymerization reaction began. After 18h of reaction, 20mL of methanol-hydrochloric acid solution was immediately added to terminate the reaction. Then a large amount of ethanol was added to separate the copolymer, and the copolymer was vacuum dried at 40°C until the polymer weight did not change.

[0113] Example 12

[0114] In a glove box, weigh the complex of formula 12 (7.8 mg, 10 μmol) into a 50 mL cillin bottle, add 1-hexene (10.08 g, 0.12 mol) to fully dissolve the catalyst; weigh tri(pentafluorophenyl)borane B(C6F5)3 (5.2 mg, 10 μmol), add 1-hexene (0.84 g, 0.01 mol) to dissolve B(C6F5)3; under stirring, quickly add the B(C6F5)3 solution to the complex solution, and the polymerization reaction begins. After 18 hours of reaction, immediately add 20 mL of methanol hydrochloric acid solution to terminate the reaction. Then add a large amount of ethanol to separate the copolymer, and vacuum dry the copolymer at 40°C until the polymer weight does not change.

[0115] Embodiment 13

[0116] In a glove box, weigh the complex of formula 13 (7.8 mg, 10 μmol) into a 50 mL vial, add 1-hexene (10.08 g, 0.12 mol) and Al i Bu3 (40μL, 0.5M, 20μmol) was added to fully dissolve the catalyst; tri(pentafluorophenyl)borane B(C6F5)3 (5.2mg, 10μmol) was weighed, 1-hexene (0.84g, 0.01mol) was added to dissolve B(C6F5)3; under stirring, the B(C6F5)3 solution was quickly added to the complex solution, and the polymerization reaction began. After 18h of reaction, 20mL of methanol-hydrochloric acid solution was immediately added to terminate the reaction. Then a large amount of ethanol was added to separate the copolymer, and the copolymer was vacuum dried at 40°C until the weight of the polymer did not change.

[0117] Embodiment 14

[0118] In a glove box, weigh the complex of formula 14 (6.3 mg, 10 μmol) into a 50 mL vial, add 1-hexene (10.08 g, 0.12 mol) and Al i Bu3 (40μL, 0.5M, 20μmol) was added to fully dissolve the catalyst; tri(pentafluorophenyl)borane B(C6F5)3 (5.2mg, 10μmol) was weighed, 1-hexene (0.84g, 0.01mol) was added to dissolve B(C6F5)3; under stirring, the B(C6F5)3 solution was quickly added to the complex solution, and the polymerization reaction began. After 18h of reaction, 20mL of methanol-hydrochloric acid solution was immediately added to terminate the reaction. Then a large amount of ethanol was added to separate the copolymer, and the copolymer was vacuum dried at 40°C until the weight of the polymer did not change.

[0119] Embodiment 15

[0120] In a glove box, weigh the complex of formula 15 (7.0 mg, 10 μmol) into a 50 mL cillin bottle, add 1-hexene (10.08 g, 0.12 mol) to fully dissolve the catalyst; weigh tri(pentafluorophenyl)borane B(C6F5)3 (5.2 mg, 10 μmol), add 1-hexene (0.84 g, 0.01 mol) to dissolve B(C6F5)3; under stirring, quickly add the B(C6F5)3 solution to the complex solution, and the polymerization reaction begins. After 18 hours of reaction, immediately add 20 mL of methanol hydrochloric acid solution to terminate the reaction. Then add a large amount of ethanol to separate the copolymer, and vacuum dry the copolymer at 40°C until the polymer weight does not change.

[0121] Example 16

[0122] In a glove box, weigh the complex of formula 16 (7.3 mg, 10 μmol) into a 50 mL cillin bottle, add 1-hexene (10.08 g, 0.12 mol) to fully dissolve the catalyst; weigh tri(pentafluorophenyl)borane B(C6F5)3 (5.2 mg, 10 μmol), add 1-hexene (0.84 g, 0.01 mol) to dissolve B(C6F5)3; under stirring, quickly add the B(C6F5)3 solution to the complex solution, and the polymerization reaction begins. After 18 hours of reaction, immediately add 20 mL of methanol hydrochloric acid solution to terminate the reaction. Then add a large amount of ethanol to separate the copolymer, and vacuum dry the copolymer at 40°C until the weight of the polymer does not change.

[0123] Embodiment 17

[0124] In a glove box, weigh the complex of formula 2 (7.1 mg, 10 μmol) into a 50 mL cillin bottle, add 1-hexene (10.08 g, 0.12 mol) to fully dissolve the catalyst; weigh tri(pentafluorophenyl)borane B(C6F5)3 (5.2 mg, 10 μmol), add 1-hexene (0.84 g, 0.01 mol) to dissolve B(C6F5)3; under stirring, quickly add B(C6F5)3 solution to the complex solution, and the polymerization reaction begins. After 18 hours of reaction, immediately add 20 mL of methanol hydrochloric acid solution to terminate the reaction. Then add a large amount of ethanol to separate the copolymer, and vacuum dry the copolymer at 40°C until the polymer weight does not change.

[0125] The polymer was characterized and the results are shown in Figure 2 and Figure 3 ,in, Figure 2 The poly α-olefin sample prepared in Example 17 of the present invention 13 C NMR spectrum, Figure 3 This is the GPC curve of the poly-α-olefin sample prepared in Example 17 of the present invention.

[0126] Embodiment 18

[0127] In a glove box, weigh the complex of formula 4 (8.0 mg, 10 μmol) into a 50 mL cillin bottle, add 1-octene (10.08 g, 0.09 mol) to fully dissolve the catalyst; weigh tri(pentafluorophenyl)borane B(C6F5)3 (5.2 mg, 10 μmol), add 1-octene (1.12 g, 0.01 mol) to dissolve B(C6F5)3; under stirring, quickly add B(C6F5)3 solution to the complex solution, and the polymerization reaction begins. After 18 hours of reaction, immediately add 20 mL of methanol hydrochloric acid solution to terminate the reaction. Then add a large amount of ethanol to separate the copolymer, and vacuum dry the copolymer at 40°C until the weight of the polymer does not change.

[0128] The polymer was characterized and the results are shown in Figure 4 , Figure 4 The poly α-olefin sample prepared in Example 18 of the present invention 13 C NMR spectrum.

[0129] Embodiment 19

[0130] In a glove box, weigh the complex of formula 2 (7.1 mg, 10 μmol) into a 50 mL cillin bottle, add 1-octene (10.08 g, 0.09 mol) to fully dissolve the catalyst; weigh tri(pentafluorophenyl)borane B(C6F5)3 (5.2 mg, 10 μmol), add 1-octene (1.12 g, 0.01 mol) to dissolve B(C6F5)3; under stirring, quickly add B(C6F5)3 solution to the complex solution, and the polymerization reaction begins. After 18 hours of reaction, immediately add 20 mL of methanol hydrochloric acid solution to terminate the reaction. Then add a large amount of ethanol to separate the copolymer, and vacuum dry the copolymer at 40°C until the polymer weight does not change.

[0131] The polymer was characterized and the results are shown in Figure 5 , Figure 5 This is the GPC curve of the poly-α-olefin sample prepared in Example 19 of the present invention.

[0132] Embodiment 20

[0133] In the glove box, weigh the complex of formula 2 (7.1 mg, 10 μmol) into a 50 mL vial, add 1-nonene (23.94 g, 0.19 mol) and Al i Bu3 (40 μL, 20 μmol) was added to fully dissolve the catalyst; tri(pentafluorophenyl)borane B(C6F5)3 (5.2 mg, 10 μmol) was weighed, 1-nonene (1.26 g, 0.01 mol) was added to dissolve B(C6F5)3; under stirring, the B(C6F5)3 solution was quickly added to the complex solution, and the polymerization reaction began. After 18 hours of reaction, 20 mL of methanol-hydrochloric acid solution was immediately added to terminate the reaction. Then a large amount of ethanol was added to separate the copolymer, and the copolymer was vacuum dried at 40°C until the weight of the polymer did not change.

[0134] Embodiment 21

[0135] In a glove box, weigh the complex of formula 2 (7.1 mg, 10 μmol) into a 50 mL vial, add 1-decene (26.60 g, 0.19 mol) and Al iBu3 (40 μL, 20 μmol) was added to fully dissolve the catalyst; tri(pentafluorophenyl)borane B(C6F5)3 (5.2 mg, 10 μmol) was weighed, 1-decene (1.40 g, 0.01 mol) was added to dissolve B(C6F5)3; under stirring, the B(C6F5)3 solution was quickly added to the complex solution, and the polymerization reaction began. After 18 hours of reaction, 20 mL of methanol-hydrochloric acid solution was immediately added to terminate the reaction. Then a large amount of ethanol was added to separate the copolymer, and the copolymer was vacuum dried at 40°C until the weight of the polymer did not change.

[0136] Embodiment 22

[0137] In a glove box, weigh the complex of formula 2 (7.1 mg, 10 μmol) into a 50 mL vial, add 1-dodecene (31.92 g, 0.19 mol) and Al i Bu3 (40 μL, 20 μmol) was added to fully dissolve the catalyst; tri(pentafluorophenyl)borane B(C6F5)3 (5.2 mg, 10 μmol) was weighed, 1-dodecene (1.68 g, 0.01 mol) was added to dissolve B(C6F5)3; under stirring, the B(C6F5)3 solution was quickly added to the complex solution, and the polymerization reaction began. After 18 hours of reaction, 20 mL of methanol-hydrochloric acid solution was immediately added to terminate the reaction. Then a large amount of ethanol was added to separate the copolymer, and the copolymer was vacuum dried at 40°C until the weight of the polymer did not change.

[0138] Embodiment 23

[0139] In a glove box, weigh the complex of formula 2 (7.1 mg, 10 μmol) into a 50 mL vial, add 1-tetradecene (37.24 g, 0.19 mol) and Al i Bu3 (40 μL, 20 μmol) was added to fully dissolve the catalyst; tri(pentafluorophenyl)borane B(C6F5)3 (5.2 mg, 10 μmol) was weighed, 1-tetradecene (1.96 g, 0.01 mol) was added to dissolve B(C6F5)3; under stirring, the B(C6F5)3 solution was quickly added to the complex solution, and the polymerization reaction began. After 18 hours of reaction, 20 mL of methanol-hydrochloric acid solution was immediately added to terminate the reaction. Then a large amount of ethanol was added to separate the copolymer, and the copolymer was vacuum dried at 40°C until the weight of the polymer did not change.

[0140] Embodiment 24

[0141] In a glove box, weigh the complex of formula 2 (7.1 mg, 10 μmol) into a 50 mL vial, add 1-hexadecene (42.56 g, 0.19 mol) and Ali Bu3 (40 μL, 20 μmol) was added to fully dissolve the catalyst; tri(pentafluorophenyl)borane B(C6F5)3 (5.2 mg, 10 μmol) was weighed, 1-hexadecene (2.24 g, 0.01 mol) was added to dissolve B(C6F5)3; under stirring, the B(C6F5)3 solution was quickly added to the complex solution, and the polymerization reaction began. After 18 hours of reaction, 20 mL of methanol-hydrochloric acid solution was immediately added to terminate the reaction. Then a large amount of ethanol was added to separate the copolymer, and the copolymer was vacuum dried at 40°C until the weight of the polymer did not change.

[0142] Embodiment 25

[0143] In a glove box, weigh the complex of formula 2 (7.1 mg, 10 μmol) into a 50 mL cillin bottle, add 1-octene (15.68 g, 0.14 mol) to fully dissolve the catalyst; weigh tri(pentafluorophenyl)borane B(C6F5)3 (5.2 mg, 10 μmol), add 1-octene (1.12 g, 0.01 mol) to dissolve B(C6F5)3; under stirring, quickly add B(C6F5)3 solution to the complex solution, and the polymerization reaction begins. After 18 hours of reaction, immediately add 20 mL of methanol hydrochloric acid solution to terminate the reaction. Then add a large amount of ethanol to separate the copolymer, and vacuum dry the copolymer at 40°C until the polymer weight does not change.

[0144] Embodiment 26

[0145] In a glove box, weigh the complex of formula 4 (8.0 mg, 10 μmol) into a 50 mL cillin bottle, add 1-octene (2.24 g, 0.02 mol) to fully dissolve the catalyst; weigh tri(pentafluorophenyl)borane B(C6F5)3 (5.2 mg, 10 μmol), add 1-octene (1.12 g, 0.01 mol) to dissolve B(C6F5)3; under stirring, quickly add B(C6F5)3 solution to the complex solution, and the polymerization reaction begins. After 18 hours of reaction, immediately add 20 mL of methanol hydrochloric acid solution to terminate the reaction. Then add a large amount of ethanol to separate the copolymer, and vacuum dry the copolymer at 40°C until the polymer weight does not change.

[0146] Embodiment 27

[0147] In a glove box, weigh the complex of formula 4 (8.0 mg, 10 μmol) into a 50 mL cillin bottle, add 1-octene (4.48 g, 0.04 mol) to fully dissolve the catalyst; weigh tri(pentafluorophenyl)borane B(C6F5)3 (5.2 mg, 10 μmol), add 1-octene (1.12 g, 0.01 mol) to dissolve B(C6F5)3; under stirring, quickly add B(C6F5)3 solution to the complex solution, and the polymerization reaction begins. After 18 hours of reaction, immediately add 20 mL of methanol hydrochloric acid solution to terminate the reaction. Then add a large amount of ethanol to separate the copolymer, and vacuum dry the copolymer at 40°C until the weight of the polymer does not change.

[0148] Embodiment 28

[0149] In a glove box, weigh the complex of formula 4 (8.0 mg, 10 μmol) into a 50 mL cillin bottle, add 1-octene (6.72 g, 0.06 mol) to fully dissolve the catalyst; weigh tri(pentafluorophenyl)borane B(C6F5)3 (5.2 mg, 10 μmol), add 1-octene (1.12 g, 0.01 mol) to dissolve B(C6F5)3; under stirring, quickly add B(C6F5)3 solution to the complex solution, and the polymerization reaction begins. After 18 hours of reaction, immediately add 20 mL of methanol hydrochloric acid solution to terminate the reaction. Then add a large amount of ethanol to separate the copolymer, and vacuum dry the copolymer at 40°C until the polymer weight does not change.

[0150] Embodiment 29

[0151] In a glove box, weigh the complex of formula 4 (8.0 mg, 10 μmol) into a 50 mL cillin bottle, add 1-octene (10.08 g, 0.09 mol) to fully dissolve the catalyst; weigh tri(pentafluorophenyl)borane B(C6F5)3 (5.2 mg, 10 μmol), add 1-octene (1.12 g, 0.01 mol) to dissolve B(C6F5)3; under stirring, quickly add B(C6F5)3 solution to the complex solution, and the polymerization reaction begins. After 18 hours of reaction, immediately add 20 mL of methanol hydrochloric acid solution to terminate the reaction. Then add a large amount of ethanol to separate the copolymer, and vacuum dry the copolymer at 40°C until the weight of the polymer does not change.

[0152] Embodiment 30

[0153] In a glove box, weigh the complex of formula 4 (8.0 mg, 10 μmol) into a 50 mL cillin bottle, add 1-octene (12.32 g, 0.11 mol) to fully dissolve the catalyst; weigh tri(pentafluorophenyl)borane B(C6F5)3 (5.2 mg, 10 μmol), add 1-octene (1.12 g, 0.01 mol) to dissolve B(C6F5)3; under stirring, quickly add B(C6F5)3 solution to the complex solution, and the polymerization reaction begins. After 18 hours of reaction, immediately add 20 mL of methanol hydrochloric acid solution to terminate the reaction. Then add a large amount of ethanol to separate the copolymer, and vacuum dry the copolymer at 40°C until the weight of the polymer does not change.

[0154] Embodiment 31

[0155] In a glove box, weigh the complex of formula 4 (8.0 mg, 10 μmol) into a 50 mL cillin bottle, add 1-octene (15.68 g, 0.14 mol) to fully dissolve the catalyst; weigh tri(pentafluorophenyl)borane B(C6F5)3 (5.2 mg, 10 μmol), add 1-octene (1.12 g, 0.01 mol) to dissolve B(C6F5)3; under stirring, quickly add B(C6F5)3 solution to the complex solution, and the polymerization reaction begins. After 18 hours of reaction, immediately add 20 mL of methanol hydrochloric acid solution to terminate the reaction. Then add a large amount of ethanol to separate the copolymer, and vacuum dry the copolymer at 40°C until the polymer weight does not change.

[0156] Embodiment 32

[0157] In a glove box, weigh the complex of formula 4 (8.0 mg, 10 μmol) into a 50 mL cillin bottle, add 1-octene (21.28 g, 0.19 mol) to fully dissolve the catalyst; weigh tri(pentafluorophenyl)borane B(C6F5)3 (5.2 mg, 10 μmol), add 1-octene (1.12 g, 0.01 mol) to dissolve B(C6F5)3; under stirring, quickly add B(C6F5)3 solution to the complex solution, and the polymerization reaction begins. After 18 hours of reaction, immediately add 20 mL of methanol hydrochloric acid solution to terminate the reaction. Then add a large amount of ethanol to separate the copolymer, and vacuum dry the copolymer at 40°C until the polymer weight does not change.

[0158] Test example

[0159] 1. Determination of molecular weight and molecular weight distribution of α-olefin homopolymer

[0160] Homopolymer number average molecular weight (M n) and molecular weight distribution (PDI): the number average molecular weight (M n ) and molecular weight distribution (PDI) were determined by gel permeation chromatography (GPC) at 40°C using THF as the mobile phase with polystyrene as the standard.

[0161] 2. Determination of stereoregularity of α-olefin homopolymer

[0162] The stereoregularity of the homopolymer was determined in CDCl3 at 25 °C. 13 C NMR spectrum was obtained.

[0163] The test results of the homopolymers prepared in Examples 1 to 16 are shown in Table 2:

[0164] Table 2 Performance test results of homopolymers prepared in Examples 1 to 16 of the present invention a

[0165]

[0166]

[0167] Polymerization conditions: 25°C, catalyst 10 μmol, polymerization time 18 hours, [1-hexene]: [Cat.] = 13000: 1; b Al i Bu3=20μmol;

[0168] As shown in Table 2, when the ratio of monomer to catalyst is 13000:1, the catalytic system can catalyze the polymerization of 1-hexene and obtain polyhexene with a number average molecular weight higher than 1 million. This ratio is much lower than the monomer-catalyst ratio (35000:1) used in the literature (Organometallics 2005, 24, 200-202.) for preparing polyhexene with a molecular weight higher than 1 million, indicating that compared with the system in the literature, the chain transfer of this system is not obvious, and it is more conducive to the preparation of ultra-high molecular weight poly-α-olefins.

[0169] The test results of the copolymers prepared in Examples 17 to 25 are shown in Table 3:

[0170] Table 3 Performance test results of homopolymers prepared in Examples 17 to 25 of the present invention a

[0171]

[0172]

[0173] Polymerization conditions: 25°C, catalyst 2: 10 μmol, polymerization time 18 hours; b Catalyst 4: 10 μmol;c Al i Bu3=20μmol;

[0174] As shown in Table 3, the catalytic system can catalyze the polymerization of α-olefins with carbon numbers ranging from 6 to 16 to obtain polyolefins with a number average molecular weight of over one million, and the molecular weight distribution of the obtained polymers is relatively narrow. In addition, the conversion rates of the monomers are all higher than 70%, indicating that the steric hindrance of the monomers has no obvious effect on the polymerization of α-olefins catalyzed by the catalytic system.

[0175] The test results of the copolymers prepared in Examples 26 to 32 are shown in Table 4:

[0176] Table 4 Performance test results of homopolymers prepared in Examples 26 to 32 of the present invention a

[0177]

[0178] Polymerization conditions: 25°C, catalyst 4:10 μmol, polymerization time 18 hours, Mon = 1-octene;

[0179] The catalytic system composed of complex 4 catalyzes the polymerization of octene at different monomer to catalyst ratios. As the monomer to catalyst ratio increases, the number average molecular weight of the resulting polymer increases linearly, indicating that the polymerization has good controllability. The number average molecular weight of the resulting polymer is close to the theoretical molecular weight, indicating that the catalytic system has a high catalyst efficiency. When the monomer to catalyst ratio is higher than 10000:1, the number average molecular weight of the resulting polyoctene exceeds 1 million, further indicating that there is no chain transfer in the polymerization system.

[0180] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing an ultrahigh molecular weight narrow distribution poly-alpha-olefin, comprising: Initiating polymerization of α-olefin or its derivative monomers in a reaction medium under a catalytic system to obtain poly-α-olefin; The catalytic system comprises an organic boron compound, a bisphenoloxy metal complex and an optional organic aluminum compound; The bisphenoloxy metal complex has a structure of Formula I or Formula II: wherein M is selected from titanium, zirconium or hafnium; R1, R2, R3 and R4 are independently selected from hydrogen, an alkyl group containing 1 to 30 carbon atoms, a cycloalkyl group containing 3 to 30 carbon atoms, an aryl-substituted alkyl group containing 7 to 30 carbon atoms, a silyl-substituted alkyl group containing 1 to 30 carbon atoms, an aryl group having a carbon number greater than or equal to 6, or a halogen; at least two of R1, R2, R3 and R4 are different and at least one is a halogen; X is selected from hydrogen, an alkyl group containing 1 to 30 carbon atoms, an aryl-substituted alkyl group containing 7 to 30 carbon atoms, a silyl-substituted alkyl group containing 1 to 30 carbon atoms, a halogen, or an alkoxy group containing 1 to 30 carbon atoms; Y is selected from one of N, S or O; n is selected from an integer of 0 to 4; when Y is N, R5 and R6 are selected from hydrogen, an alkyl group containing 1 to 10 carbon atoms, or an aryl group having a carbon number greater than or equal to 6; m is selected from an integer of 0 to 4.

2. The preparation method according to claim 1, characterized in that: The bisphenoloxy metal complex has structures of Formula 1 to Formula 16:

3. The preparation method according to claim 1 or 2, characterized in that: In the catalytic system, the organic boron compound is selected from an ionic compound formed by an organic boron anion and a cation, and the organic boron anion is selected from tetraphenylborate, tetrakis(monofluorophenyl)borate, tetrakis(difluorophenyl)borate, tetrakis(trifluorophenyl)borate, tetrakis(tetrafluorophenyl)borate, tetrakis(pentafluorophenyl)borate, tetrakis(tetrafluoromethylphenyl)borate, tetrakis(tolyl)borate, tetrakis(xylyl)borate, (triphenyl, pentafluorophenyl)borate, [tris(pentafluorophenyl), phenyl]borate or undecyl-7,8-dicarbonundecaborate; the cation is selected from carbonium cation, oxonium cation, ammonium cation, phosphonium cation, cycloheptatrienyl cation or ferrocenium cation containing a transition metal; The organoaluminum compound is selected from trimethylaluminum, triethylaluminum, tripropylaluminum, tributylaluminum, triisopropylaluminum, triisobutylaluminum, tripentylaluminum, trihexylaluminum, tricyclohexylaluminum, trioctylaluminum, triphenylaluminum, tri-p-tolylaluminum, tribenzylaluminum, ethyldibenzylaluminum, methylaluminoxane or ethyldi(p-tolyl)aluminum.

4. The preparation method according to claim 3, characterized in that: The molar ratio of the organic boron compound, the organic aluminum compound and the bisphenoloxy metal complex is (0.5-10): (2-3000): (10-1).

5. The preparation method according to claim 4, characterized in that: The molar ratio of the α-olefin or its derivative monomer to the bisphenoloxy metal complex is 10000-25000:

1.

6. The preparation method according to claim 5, characterized in that: The α-olefin or its derivative monomer is selected from 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tetradecene, 1-hexadecene or 1-eicosene.

7. The preparation method according to claim 6, characterized in that: The polymerization reaction temperature is -20°C to 150°C, and the polymerization reaction time is 1 minute to 10 days.

8. The preparation method according to claim 7, characterized in that: The reaction medium is selected from one or more of aliphatic saturated hydrocarbons, aromatic hydrocarbons, α-olefins, aromatic halides and cycloalkanes.

9. An ultra-high molecular weight narrow distribution poly-α-olefin, whose number average molecular weight is greater than 1.0×10 6 ; Molecular weight distribution <2.5; Stereotacticity not higher than 95%.

10. The poly-α-olefin according to claim 9, having a number average molecular weight of 1.0×10 6 ~4.0×10 6 ; Molecular weight distribution is 1.0-2.0; Stereotacticity is not higher than 90%.

Citation Information

Patent Citations

  • Solvent free oil soluble drag reducing polymer suspension

    US5504132A

Cited By

  • Ethylene / alpha-olefin gradient copolymer and preparation method thereof

    CN119708316A