Preparation method of alkali-induced tackifying hydrogel
By adjusting the pH value and components in the hydrogel, an alkali-induced viscosity-enhancing hydrogel was prepared, which solved the adhesion and hysteresis of the hydrogel in the primary cell and improved its electrochemical cycle. Stability and output efficiency.
Patent Information
- Application Number
- CN202411108185.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-22
AI Technical Summary
The application of hydrogels in primary batteries is affected by problems such as low interface adhesion, high interface impedance, ineffective ion transport, uneven deposition and high hysteresis, which affects its long-term stability and output efficiency.
By adjusting the combination of methylcellulose, acrylamide, silk protein, photoinitiator and crosslinking agent at different pH values, the pH of the hydrogel is adjusted to increase viscosity and reduce hysteresis, An alkali-tassification hydrogel was prepared.
The adhesion of the hydrogel is adjusted and low hysteresis is achieved, the output efficiency and application life of the electrochemical cycle are improved, and the strong adhesion between the hydrogel and the electrode sheet is solved and the debonding on demand is solved. question.
Smart Images

Figure CN118994487A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of hydrogel material preparation, in particular to a method for preparing an alkali-induced viscosity-increasing hydrogel. Background Art
[0002] Green, sustainable and stable energy supply is of great significance to human life. Batteries are one of the main sources of electrical energy in many fields such as soft robots, artificial intelligence, and smart devices, so more and more researchers have begun to pay attention to the development of batteries. In recent decades, hydrogels have gradually been used as quasi-solid electrolyte materials. Despite the great progress made in this conductive material, there is still a gap between the practical value of hydrogels and the expected performance of electrolytes.
[0003] Since the output power of batteries using neutral electrolytes is insufficient, acidic or alkaline electrolytes are widely accepted in order to obtain satisfactory output power. Hydrogels are gradually used as electrolytes for alkaline batteries, such as zinc-air batteries and zinc-manganese batteries. Related work mainly focuses on improving the energy supply efficiency and the intrinsic flexibility of electrolytes. However, low interfacial adhesion still hinders the development of hydrogel electrolytes in primary batteries, especially the rigid adhesion of hydrogels leads to low interfacial bonding strength, high interfacial impedance, ineffective ion transport, uneven deposition, negative electrode metal shedding, dendrite growth during electrochemical cycling, and even battery failure. In addition, the fatigue irreversible deformation caused by high hysteresis seriously affects its long-term stability and availability, becoming a fatal defect for most hydrogel electrolytes to achieve continuous and stable energy output. So far, there is still a lack of an effective means to synergistically solve these problems. Therefore, it is urgent to develop an integrated strategy for the one-step preparation of hydrogel electrolytes to achieve the key indicator goals of controllable adhesion and low hysteresis for alkaline batteries.
[0004] Therefore, the present invention provides a method for preparing a hydrogel with adjustable adhesion. Summary of the invention
[0005] In view of the shortcomings of the prior art, the present invention provides a method for preparing an alkali-induced viscosity-enhancing hydrogel, which solves the problems of unadjustable adhesion and hysteresis performance, and poor long-term stability and output efficiency of traditional hydrogels.
[0006] To achieve the above objectives, the present invention is implemented by the following technical scheme: a method for preparing an alkali-induced viscosity-increasing hydrogel, comprising the following steps:
[0007] S1. Dissolve methyl cellulose and acrylamide in deionized water and stir at 40-70°C for 20-50 minutes;
[0008] S2. Slowly pour the silk protein into the rapidly stirred mixed solution and set aside;
[0009] S3, adding the photoinitiator and the cross-linking agent to the mixed solution, and stirring magnetically for 5-20 minutes;
[0010] S4, adding different sodium hydroxide or hydrochloric acid solutions dropwise into the solution in step 3, stirring evenly, measuring the pH value of the solution with a pH meter, and recording;
[0011] S5. Rapidly place the solution in step S4 under a 70-150W ultraviolet lamp for 2-5 minutes to obtain an alkali-induced thickening hydrogel.
[0012] Preferably, in step S1, the methyl cellulose and acrylamide include the following components by weight: 2-6 g acrylamide and 0.2-0.6 g methyl cellulose.
[0013] Preferably, the amount of deionized water in step S1 is 12-16 ml.
[0014] Preferably, the silk protein in step S2 comprises the following components by weight: 0.7-1.5 g silk protein.
[0015] Preferably, the photoinitiator and the cross-linking agent in step S3 include the following components by weight ratio: 0.02-0.06 g of photoinitiator and 0.01-0.05 g of cross-linking agent.
[0016] Preferably, the concentration of the sodium hydroxide or hydrochloric acid solution in step S4 is 2-6 mol / L.
[0017] Preferably, the photoinitiator in step S3 is 2959, and the cross-linking agent in step S3 is N,N'-methylenebisacrylamide.
[0018] Preferably, the step S4 specifically includes the following steps:
[0019] S4.1. Divide the solution obtained in step S3 into several portions, each of which is about 1-2 mL;
[0020] S4.2. Prepare sodium hydroxide or hydrochloric acid solutions of different concentrations;
[0021] S4.3, adding a sodium hydroxide or hydrochloric acid solution of a certain concentration dropwise to a portion of the solution of step S4.1, stirring while adding dropwise, until the desired pH value is reached, and measuring and recording the pH value of the solution using a pH meter while adding dropwise;
[0022] S4.4, by adjusting the pH value of the mixed solution, when the pH value is between 4 and 11, the viscosity of the hydrogel changes accordingly; when the pH value is between 6.5 and 12, the hysteresis energy changes accordingly;
[0023] S4.5, repeating steps S4.3 and S4.4, treating different portions of the solution in step S4.1 for each concentration of sodium hydroxide or hydrochloric acid solution, until the pH values of all solutions are measured and recorded;
[0024] S4.6. Set all treated solutions aside and let stand for 8-10 minutes;
[0025] S4.7. Use a pH meter to measure and record the pH value of each solution again;
[0026] S4.8. Label the solution after treatment with each concentration of sodium hydroxide or hydrochloric acid solution.
[0027] The present invention provides a method for preparing an alkali-induced viscosity-increasing hydrogel, which has the following beneficial effects:
[0028] 1. The present invention can easily control the interfacial viscosity of the hydrogel before polymerization by changing the pH value of the prepolymer solution. When the pH value is adjusted from 4 to 11, the viscosity increases by 3.44 times, and the maximum viscosity reaches 15.48 kPa. This method allows the adhesion of the hydrogel to be adjusted according to specific application requirements.
[0029] 2. The present invention adjusts the pH value so that the prepared hydrogel can meet the requirements of strong adhesion and on-demand debonding, and has multifunctional application potential. The hydrogel is particularly suitable for solid electrolytes and solves the problems of strong adhesion and on-demand debonding between the hydrogel electrolyte and the electrode sheet.
[0030] 3. The hydrogel prepared by the method of the present invention can maintain a stable output efficiency during the electrochemical cycle, reducing fatigue and irreversible deformation caused by high hysteresis, thereby improving the application life and stability of the hydrogel in the fields of batteries and the like. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 It is a flow chart of the present invention. DETAILED DESCRIPTION
[0032] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] Please see attached Figure 1 The present invention provides a method for preparing an alkali-induced thickening hydrogel, comprising the following steps:
[0034] S1. Dissolve methyl cellulose and acrylamide in deionized water and stir at 40-70°C for 20-50 minutes;
[0035] S2. Slowly pour the silk protein into the rapidly stirred mixed solution and set aside;
[0036] S3, adding the photoinitiator and the cross-linking agent to the mixed solution, and stirring magnetically for 5-20 minutes;
[0037] S4, adding different sodium hydroxide or hydrochloric acid solutions dropwise into the solution in step 3, stirring evenly, measuring the pH value of the solution with a pH meter, and recording;
[0038] S5. Rapidly place the solution in step S4 under a 70-150W ultraviolet lamp for 2-5 minutes to obtain an alkali-induced thickening hydrogel.
[0039] In step S1, the methyl cellulose and acrylamide are mixed by weight and include the following components: 2-6 g acrylamide and 0.2-0.6 g methyl cellulose.
[0040] In step S1, the amount of deionized water is 12-16 ml.
[0041] In step S2, the silk protein comprises the following components by weight: 0.7-1.5 g of silk protein.
[0042] In step S3, the photoinitiator and the crosslinking agent include the following components by weight ratio: 0.02-0.06 g of photoinitiator and 0.01-0.05 g of crosslinking agent.
[0043] In step S4, the concentration of the sodium hydroxide or hydrochloric acid solution is 2-6 mol / L.
[0044] The photoinitiator in step S3 is 2959, and the cross-linking agent in step S3 is N,N'-methylenebisacrylamide.
[0045] The S4 step specifically includes the following steps:
[0046] S4.1. Divide the solution obtained in step S3 into several portions, each of which is about 1-2 mL;
[0047] S4.2. Prepare sodium hydroxide or hydrochloric acid solutions of different concentrations;
[0048] S4.3, adding a sodium hydroxide or hydrochloric acid solution of a certain concentration dropwise to a portion of the solution of step S4.1, stirring while adding dropwise, until the desired pH value is reached, and measuring and recording the pH value of the solution using a pH meter while adding dropwise;
[0049] S4.4, by adjusting the pH value of the mixed solution, when the pH value is between 4 and 11, the viscosity of the hydrogel changes accordingly; when the pH value is between 6.5 and 12, the hysteresis energy changes accordingly;
[0050] S4.5, repeating steps S4.3 and S4.4, treating different portions of the solution in step S4.1 for each concentration of sodium hydroxide or hydrochloric acid solution, until the pH values of all solutions are measured and recorded;
[0051] S4.6. Set all treated solutions aside and let stand for 8-10 minutes;
[0052] S4.7. Use a pH meter to measure and record the pH value of each solution again;
[0053] S4.8. Label the solution after treatment with each concentration of sodium hydroxide or hydrochloric acid solution.
[0054] Embodiment 1:
[0055] Implementation steps:
[0056] S1: Dissolve 4 g acrylamide and 0.4 g methylcellulose in 14 mL deionized water and stir at 60 °C for 30 min;
[0057] S2: slowly pour 1.0 g of silk protein into the rapidly stirred mixed solution and set aside;
[0058] S3: 0.04 g of photoinitiator 2959 and 0.03 g of cross-linker N,N'-methylenebisacrylamide were added to the above mixed solution and magnetically stirred for 10 minutes;
[0059] S4:
[0060] S4.1: Divide the solution obtained in step S3 into several portions, each portion is about 1.5 mL;
[0061] S4.2: Prepare 4 mol / L sodium hydroxide or hydrochloric acid solution;
[0062] S4.3: Add 4 mol / L sodium hydroxide or hydrochloric acid solution dropwise to a portion of the solution in step S4.1, stirring while adding, until the pH value reaches 7, and measure and record the pH value of the solution using a pH meter while adding;
[0063] S4.4: By adjusting the pH value of the mixed solution, when the pH value is between 4 and 11, the viscosity of the hydrogel changes accordingly; when the pH value is between 6.5 and 12, the hysteresis energy changes accordingly;
[0064] S4.5: Repeat steps S4.3 and S4.4, treating different portions of the solution in step S4.1 for each concentration of sodium hydroxide or hydrochloric acid solution, until the pH values of all solutions are measured and recorded;
[0065] S4.6: Set all treated solutions aside for 10 minutes;
[0066] S4.7: Use a pH meter to measure and record the pH of each solution again.
[0067] S4.8: Label the solution after treatment with each concentration of sodium hydroxide or hydrochloric acid solution;
[0068] S5: The solution in step S4 is quickly placed under a 100 W ultraviolet lamp for 3 minutes to obtain an alkali-induced thickening hydrogel.
[0069] Summary: In this example, a hydrogel with medium viscosity and low hysteresis was obtained by adjusting the pH value of the solution to 7.
[0070] Embodiment 2:
[0071] Implementation steps:
[0072] S1: Dissolve 4 g acrylamide and 0.4 g methylcellulose in 14 mL deionized water and stir at 60 °C for 30 min;
[0073] S2: slowly pour 1.0 g of silk protein into the rapidly stirred mixed solution and set aside;
[0074] S3: 0.04 g of photoinitiator 2959 and 0.03 g of cross-linker N,N'-methylenebisacrylamide were added to the above mixed solution and magnetically stirred for 10 minutes;
[0075] S4:
[0076] S4.1: Divide the solution obtained in step S3 into several portions, each portion is about 1.5 mL;
[0077] S4.2: Prepare 5 mol / L sodium hydroxide or hydrochloric acid solution;
[0078] S4.3: Add 5 mol / L sodium hydroxide or hydrochloric acid solution dropwise to a portion of the solution in step S4.1, stirring while adding, until the pH value reaches 8, and measure and record the pH value of the solution using a pH meter while adding;
[0079] S4.4: By adjusting the pH value of the mixed solution, when the pH value is between 4 and 11, the viscosity of the hydrogel changes accordingly; when the pH value is between 6.5 and 12, the hysteresis energy changes accordingly;
[0080] S4.5: Repeat steps S4.3 and S4.4, treating different portions of the solution in step S4.1 for each concentration of sodium hydroxide or hydrochloric acid solution, until the pH values of all solutions are measured and recorded;
[0081] S4.6: Set all treated solutions aside for 10 minutes;
[0082] S4.7: Use a pH meter to measure and record the pH of each solution again.
[0083] S4.8: Label the solution after treatment with each concentration of sodium hydroxide or hydrochloric acid solution;
[0084] S5: The solution in step S4 is quickly placed under a 100 W ultraviolet lamp for 3 minutes to obtain an alkali-induced thickening hydrogel.
[0085] Summary: Based on Example 1, this example further increases the viscosity of the hydrogel by adjusting the pH value of the solution to 8.
[0086] Embodiment three:
[0087] Implementation steps:
[0088] S1: Dissolve 4 g acrylamide and 0.4 g methylcellulose in 14 mL deionized water and stir at 60 °C for 30 min;
[0089] S2: slowly pour 1.0 g of silk protein into the rapidly stirred mixed solution and set aside;
[0090] S3: 0.04 g of photoinitiator 2959 and 0.03 g of cross-linker N,N'-methylenebisacrylamide were added to the above mixed solution and magnetically stirred for 10 minutes;
[0091] S4:
[0092] S4.1: Divide the solution obtained in step S3 into several portions, each portion is about 1.5 mL;
[0093] S4.2: Prepare 6 mol / L sodium hydroxide or hydrochloric acid solution;
[0094] S4.3: Add 6 mol / L sodium hydroxide or hydrochloric acid solution dropwise to a portion of the solution in step S4.1, stirring while adding, until the pH value reaches 9, and measure and record the pH value of the solution using a pH meter while adding;
[0095] S4.4: By adjusting the pH value of the mixed solution, when the pH value is between 4 and 11, the viscosity of the hydrogel changes accordingly; when the pH value is between 6.5 and 12, the hysteresis energy changes accordingly;
[0096] S4.5: Repeat steps S4.3 and S4.4, treating different portions of the solution in step S4.1 for each concentration of sodium hydroxide or hydrochloric acid solution, until the pH values of all solutions are measured and recorded;
[0097] S4.6: Set all treated solutions aside for 10 minutes;
[0098] S4.7: Use a pH meter to measure and record the pH of each solution again.
[0099] S4.8: Label the solution after treatment with each concentration of sodium hydroxide or hydrochloric acid solution;
[0100] S5: The solution in step S4 is quickly placed under a 100 W ultraviolet lamp for 3 minutes to obtain an alkali-induced thickening hydrogel.
[0101] Summary: Based on Example 2, this example further optimizes the performance of the hydrogel by adjusting the pH value of the solution to 9.
[0102] Embodiment 4:
[0103] Implementation steps:
[0104] S1: Dissolve 4 g acrylamide and 0.4 g methylcellulose in 14 mL deionized water and stir at 60 °C for 30 min;
[0105] S2: slowly pour 1.0 g of silk protein into the rapidly stirred mixed solution and set aside;
[0106] S3: 0.04 g of photoinitiator 2959 and 0.03 g of cross-linker N,N'-methylenebisacrylamide were added to the above mixed solution and magnetically stirred for 10 minutes;
[0107] S4:
[0108] S4.1: Divide the solution obtained in step S3 into several portions, each portion is about 1.5 mL;
[0109] S4.2: Prepare 6 mol / L sodium hydroxide or hydrochloric acid solution;
[0110] S4.3: Add 6 mol / L sodium hydroxide or hydrochloric acid solution dropwise to a portion of the solution in step S4.1, stirring while adding, until the pH value reaches 10, and measure and record the pH value of the solution using a pH meter while adding;
[0111] S4.4: By adjusting the pH value of the mixed solution, when the pH value is between 4 and 11, the viscosity of the hydrogel changes accordingly; when the pH value is between 6.5 and 12, the hysteresis energy changes accordingly;
[0112] S4.5: Repeat steps S4.3 and S4.4, treating different portions of the solution in step S4.1 for each concentration of sodium hydroxide or hydrochloric acid solution, until the pH values of all solutions are measured and recorded;
[0113] S4.6: Set all treated solutions aside for 10 minutes;
[0114] S4.7: Use a pH meter to measure and record the pH of each solution again.
[0115] S4.8: Label the solution after treatment with each concentration of sodium hydroxide or hydrochloric acid solution;
[0116] S5: The solution in step S4 is quickly placed under a 100 W ultraviolet lamp for 3 minutes to obtain an alkali-induced thickening hydrogel.
[0117] Summary: Based on Example 3, this example further improves the adhesion performance and hysteresis energy control of the hydrogel by adjusting the pH value of the solution to 10.
[0118] Embodiment five:
[0119] Implementation steps:
[0120] S1: Dissolve 4 g acrylamide and 0.4 g methylcellulose in 14 mL deionized water and stir at 60 °C for 30 min;
[0121] S2: slowly pour 1.0 g of silk protein into the rapidly stirred mixed solution and set aside;
[0122] S3: 0.04 g of photoinitiator 2959 and 0.03 g of cross-linker N,N'-methylenebisacrylamide were added to the above mixed solution and magnetically stirred for 10 minutes;
[0123] S4:
[0124] S4.1: Divide the solution obtained in step S3 into several portions, each portion is about 1.5 mL;
[0125] S4.2: Prepare 6 mol / L sodium hydroxide or hydrochloric acid solution;
[0126] S4.3: Add 6 mol / L sodium hydroxide or hydrochloric acid solution dropwise to a portion of the solution in step S4.1, stirring while adding, until the pH value reaches 11, and measure and record the pH value of the solution using a pH meter while adding;
[0127] S4.4: By adjusting the pH value of the mixed solution, when the pH value is between 4 and 11, the viscosity of the hydrogel changes accordingly; when the pH value is between 6.5 and 12, the hysteresis energy changes accordingly;
[0128] S4.5: Repeat steps S4.3 and S4.4, treating different portions of the solution in step S4.1 for each concentration of sodium hydroxide or hydrochloric acid solution, until the pH values of all solutions are measured and recorded;
[0129] S4.6: Set all treated solutions aside for 10 minutes;
[0130] S4.7: Use a pH meter to measure and record the pH of each solution again.
[0131] S4.8: Label the solution after treatment with each concentration of sodium hydroxide or hydrochloric acid solution;
[0132] S5: The solution in step S4 is quickly placed under a 100 W ultraviolet lamp for 3 minutes to obtain an alkali-induced thickening hydrogel.
[0133] Summary: Based on Example 4, this example obtains the highest viscosity and the lowest hysteresis energy by adjusting the pH value of the solution to 11, which significantly improves the comprehensive performance of the hydrogel.
[0134] Summary:
[0135] Through the above five embodiments, the present invention gradually improves the adhesion performance of the hydrogel and controls the hysteresis energy by adjusting the pH value of the solution. Each embodiment is further optimized on the basis of the previous one, and the versatility and wide application potential of the hydrogel are achieved by accurately controlling the pH value range.
[0136] Experimental design:
[0137] Purpose:
[0138] The hydrogel preparation method used in the present invention was verified by experiments to explore whether it can achieve a multifunctional hydrogel with adjustable interfacial viscosity and low hysteresis by adjusting the pH value of the mixed solution before polymerization. When the pH value was adjusted from 4 to 11, the viscosity increased by 3.44 times, and the maximum viscosity was 15.48 kPa. When the pH value changed from 6.5 to 12, the hysteresis energy decreased by 2.22 times, and the minimum hysteresis energy was only 1.91 kJ·m -3 .
[0139] Experimental Materials:
[0140] Acrylamide
[0141] Methylcellulose
[0142] Deionized water
[0143] Silk protein
[0144] Photoinitiator 2959
[0145] Crosslinking agent N,N'-methylenebisacrylamide
[0146] Sodium hydroxide solution (2mol / L, 4mol / L, 6mol / L)
[0147] Hydrochloric acid solution (0.1mol / L, 1mol / L, 2mol / L)
[0148] pH Meter
[0149] UV lamp (70-150W)
[0150] Transparent flat bottom container
[0151] Viscometer
[0152] Hysteresis Energy Test Device
[0153] Experimental steps:
[0154] Experimental preparation:
[0155] Prepare all experimental materials and ensure their purity meets the experimental requirements.
[0156] Calibrate pH meters, viscometers and hysteresis energy test devices.
[0157] Hydrogel preparation:
[0158] S1: 4 g acrylamide and 0.4 g methylcellulose were dissolved in 14 mL deionized water and stirred at 60 °C for 30 min.
[0159] S2: Slowly pour 1.0 g of silk fibroin into the rapidly stirred mixed solution and set aside.
[0160] S3: 0.04 g of photoinitiator 2959 and 0.03 g of cross-linking agent N,N'-methylenebisacrylamide were added to the above mixed solution and magnetically stirred for 10 minutes.
[0161] S4:
[0162] S4.1: Divide the solution obtained in step S3 into several portions, each of which is approximately 1.5 mL.
[0163] S4.2: Prepare sodium hydroxide solution and hydrochloric acid solution of different concentrations.
[0164] S4.3: Add sodium hydroxide or hydrochloric acid solution dropwise to a portion of the solution in step S4.1, stirring while adding, until the desired pH value (respectively 1, 2, 3, 4, 5, 6, 6.5, 7, 8, 9, 10, 11, 12) is reached.
[0165] S4.4: Record the solution at each pH condition.
[0166] S5: The solutions in step S4 were placed under a 100 W ultraviolet lamp for 3 minutes to obtain alkali-induced thickening hydrogels at different pH values.
[0167] Experimental measurements:
[0168] The viscosity and hysteresis energy of the hydrogels prepared at different pH values were measured.
[0169] Record and organize data.
[0170] Experimental results:
[0171] The experimental results are organized into a table, see Table 1, recording the viscosity and hysteresis energy data at different pH values.
[0172] Table 1:
[0173]
[0174] Experimental summary:
[0175] Through the above experiments, the following conclusions are verified:
[0176] Viscosity regulation: When the pH value was adjusted from 4 to 11, the viscosity increased significantly, from 4.50 kPa to 15.48 kPa, a 3.44-fold increase. This shows that the viscosity of the hydrogel can be adjusted by adjusting the pH value.
[0177] Hysteresis energy reduction: When the pH value was adjusted from 6.5 to 12, the hysteresis energy decreased by 2.22 times, from 4.24 kJ·m -3 Reduced to 1.88 kJ / m^3, the minimum hysteresis energy is 1.91 kJ·m -3 This verifies that low hysteresis of the hydrogel can be achieved by adjusting the pH value.
[0178] Multifunctional application: The experimental results verified the new strategy of alkali-induced viscosity increase and low hysteresis proposed in this invention. By changing the pH value of the prepolymer solution, a hydrogel with adjustable adhesion and low hysteresis was successfully prepared. The application of this hydrogel in solid electrolyte solves the problem of strong adhesion and on-demand debonding between the hydrogel electrolyte and the electrode sheet.
[0179] Experimental design:
[0180] Purpose:
[0181] By comparing with multiple traditional technologies, it is verified whether the hydrogel preparation method of the present invention has the following advantages:
[0182] Alkali-induced viscosity increase, low hysteresis;
[0183] Adjustable adhesion and on-demand debonding;
[0184] Ensure long-term stability and availability;
[0185] Highly elastic hydrogels for improved output efficiency.
[0186] Experimental Materials:
[0187] Hydrogel prepared by the method of the present invention (using prepolymer solutions with different pH values)
[0188] Traditional hydrogel samples (two common preparation methods)
[0189] Traditional hydrogel A (prepared at fixed pH)
[0190] Conventional hydrogel B (without pH adjustment)
[0191] Acrylamide:
[0192] Methylcellulose
[0193] Deionized water
[0194] Silk protein
[0195] Photoinitiator 2959
[0196] Crosslinking agent N,N'-methylenebisacrylamide
[0197] Sodium hydroxide solution (2mol / L, 4mol / L, 6mol / L)
[0198] pH Meter
[0199] UV lamp (70-150W)
[0200] Transparent flat bottom container
[0201] Viscometer
[0202] Hysteresis Energy Test Device
[0203] Tensile testing machine
[0204] Experimental steps:
[0205] Experimental preparation:
[0206] Prepare all experimental materials and ensure their purity meets the experimental requirements.
[0207] Calibrate all testing equipment including pH meters, viscometers, hysteresis energy testers and tensile testers.
[0208] Hydrogel preparation:
[0209] The method of the present invention prepares hydrogel:
[0210] S1: 4 g acrylamide and 0.4 g methylcellulose were dissolved in 14 mL deionized water and stirred at 60 °C for 30 min.
[0211] S2: Slowly pour 1.0 g of silk fibroin into the rapidly stirred mixed solution and set aside.
[0212] S3: 0.04 g of photoinitiator 2959 and 0.03 g of cross-linking agent N,N'-methylenebisacrylamide were added to the above mixed solution and magnetically stirred for 10 minutes.
[0213] S4:
[0214] S4.1: Divide the solution obtained in step S3 into several portions, each of which is approximately 1.5 mL.
[0215] S4.2: Prepare sodium hydroxide or hydrochloric acid solutions of varying concentrations.
[0216] S4.3: Add sodium hydroxide or hydrochloric acid solution dropwise to a portion of the solution in step S4.1, stirring while adding, until the desired pH value (4, 5, 6, 7, 8, 9, 10, 11, respectively) is reached.
[0217] S4.4: Record the solution at each pH condition.
[0218] S5: The solutions in step S4 were placed under a 100 W ultraviolet lamp for 3 minutes to obtain alkali-induced thickening hydrogels at different pH values.
[0219] Traditional hydrogel A: prepared at a fixed pH value (pH=7).
[0220] Conventional hydrogel B: prepared by conventional method without pH adjustment.
[0221] Experimental measurements:
[0222] The viscosity, hysteresis energy, and elasticity of all hydrogel samples were measured.
[0223] Record and organize data.
[0224] Table 2:
[0225]
[0226] Experimental summary:
[0227] Viscosity control: The viscosity of the hydrogel sample of the present invention was increased from 4.50 kPa to 15.48 kPa by adjusting the pH value of the prepolymer solution, achieving a 3.44-fold increase in viscosity. In comparison, the viscosities of the conventional hydrogels A and B were 9.50 kPa and 6.00 kPa, respectively, and the viscosity control capability was relatively weak.
[0228] Hysteresis energy reduction: When the pH value is adjusted from 6.5 to 12, the hysteresis energy of the sample of the present invention is reduced from 4.24 kJ·m -3 Reduced to 1.91 kJ·m -3 , which was reduced by 2.22 times. The hysteresis energy of traditional hydrogels A and B was 3.50 kJ·m -3 and 4.00kJ / m^3, the hysteresis energy control effect is not good.
[0229] High elasticity: The hydrogel samples of the present invention exhibit high elasticity (2.00-2.50MPa) at high pH values (9-11), which is significantly higher than traditional hydrogels A and B (1.20MPa and 1.00MPa), verifying that the hydrogel synthesized by increasing the pH value of the prepolymer solution has high elasticity, solving the problem of unstable output efficiency of traditional solid electrolytes.
[0230] Multifunctional application: The new strategy of alkali-induced viscosity increase and low hysteresis proposed in this invention successfully achieves adjustable adhesion and on-demand debonding of the prepared hydrogel by adjusting the pH value of the prepolymer solution. It is suitable for solid electrolytes and solves the problems of strong adhesion and on-demand debonding between the hydrogel electrolyte and the electrode sheet. In contrast, traditional hydrogels perform poorly in these aspects.
[0231] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing an alkali-induced thickening hydrogel, characterized in that: The following steps are involved: S1. Dissolve methyl cellulose and acrylamide in deionized water and stir at 40-70°C for 20-50 minutes; S2. Slowly pour the silk protein into the rapidly stirred mixed solution and set aside; S3, adding the photoinitiator and the cross-linking agent to the mixed solution, and stirring magnetically for 5-20 minutes; S4, adding different sodium hydroxide or hydrochloric acid solutions dropwise into the solution in step 3, stirring evenly, measuring the pH value of the solution with a pH meter, and recording; S5. Rapidly place the solution in step S4 under a 70-150W ultraviolet lamp for 2-5 minutes to obtain an alkali-induced thickening hydrogel.
2. The method for preparing an alkali-induced thickening hydrogel according to claim 1, characterized in that: In the step S1, the methyl cellulose and acrylamide include the following components by weight ratio: 2-6 g acrylamide and 0.2-0.6 g methyl cellulose.
3. The method for preparing an alkali-induced thickening hydrogel according to claim 1, characterized in that: In the step S1, the amount of deionized water is 12-16 ml.
4. The method for preparing an alkali-induced thickening hydrogel according to claim 1, characterized in that: In the step S2, the silk protein comprises the following components by weight: 0.7-1.5 g of silk protein.
5. The method for preparing an alkali-induced thickening hydrogel according to claim 1, characterized in that: In the step S3, the photoinitiator and the crosslinking agent include the following components by weight ratio: 0.02-0.06 g of photoinitiator and 0.01-0.05 g of crosslinking agent.
6. The method for preparing an alkali-induced thickening hydrogel according to claim 1, characterized in that: In the step S4, the concentration of the sodium hydroxide or hydrochloric acid solution is 2-6 mol / L.
7. The method for preparing an alkali-induced thickening hydrogel according to claim 1, characterized in that: The photoinitiator in the step S3 is 2959, and the cross-linking agent in the step S3 is N,N'-methylenebisacrylamide.
8. The method for preparing an alkali-induced thickening hydrogel according to claim 1, characterized in that: The S4 step specifically includes the following steps: S4.
1. Divide the solution obtained in step S3 into several portions, each of which is about 1-2 mL; S4.
2. Prepare sodium hydroxide or hydrochloric acid solutions of different concentrations; S4.3, adding a sodium hydroxide or hydrochloric acid solution of a certain concentration dropwise to a portion of the solution of step S4.1, stirring while adding dropwise, until the desired pH value is reached, and measuring and recording the pH value of the solution using a pH meter while adding dropwise; S4.4, by adjusting the pH value of the mixed solution, when the pH value is between 4 and 11, the viscosity of the hydrogel changes accordingly; when the pH value is between 6.5 and 12, the hysteresis energy changes accordingly; S4.5, repeating steps S4.3 and S4.4, treating different portions of the solution in step S4.1 for each concentration of sodium hydroxide or hydrochloric acid solution, until the pH values of all solutions are measured and recorded; S4.
6. Set all treated solutions aside and let stand for 8-10 minutes; S4.
7. Use a pH meter to measure and record the pH value of each solution again; S4.