Rubber plate for waist-protecting sitting chair as well as preparation method and application of rubber plate

By using composite glass fiber filler and composite odor adsorbent in the waist-protecting seating chair glue plate, the mechanical properties of polypropylene resin are improved and the odor problem is reduced, the strength and odor problems of polypropylene resin glue plate are solved, and the use is improved Comfort and safety.

CN118994786AActive Publication Date: 2024-11-22GUANGZHOU LIUQUAN BRAND MANAGEMENT SERVICE CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411303024.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-11-22
Estimated Expiration
2044-09-19

AI Technical Summary

Technical Problem

The waist-protecting seating chair glue plate made of polypropylene resin is limited due to its high hardness, poor elasticity, and insufficient strength and support capacity. At the same time, the modified polypropylene resin has a high volatile organic substance content. It is easy to release harmful odors and affects the user experience.

Method used

65 to 95 parts by weight of polypropylene resin, 5 to 18 parts by weight of metallocene polyolefin elastomer, 10 to 30 parts by weight of composite glass fiber filler, 3 to 8 parts by weight of PP-g-MAH compatibilizer, 1 to 6 parts by weight of The combination of a composite odor absorber, 1 to 9 parts by weight of color masterbing, 0.4 to 1 part by weight of antioxidant, and 0.3 to 1.5 parts by weight of lubricant, improves the mechanics of the material through the use of composite glass fiber filler and composite odor adsorbent Performance and odor reduction.

Benefits of technology

It effectively enhances the strength and toughness of the rubber plate for lumbar protection seats, reduces the generation and release of irritating odors, and improves the comfort and safety of use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994786A_ABST
    Figure CN118994786A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of high polymer materials, in particular to a rubber plate for a waist-protecting sitting posture chair and a preparation method and application thereof, and the rubber plate for the waist-protecting sitting posture chair comprises the following raw materials: polypropylene resin, a metallocene polyolefin elastomer, a composite glass fiber filler, a PP-g-MAH compatilizer, a composite odor absorbent, a color master batch, an antioxidant and a lubricant. According to the rubber plate, by adding the composite glass fiber filler, the mechanical property of the polypropylene composite material can be improved, and then the strength and toughness of the rubber plate for the waist-protecting sitting chair are enhanced; by adding the composite odor adsorbent, odor molecules generated in the polypropylene composite material can be effectively adsorbed and deodorized, the low-odor polypropylene composite material can be obtained, and the product can be applied to sofas, office chairs, beds and automobiles and can be used for correcting sitting postures of adults, children, students, pregnant women, drivers and old people.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and more specifically to a rubber sheet for a waist-protecting sitting chair and a preparation method and application thereof. Background Art

[0002] The seat and back of the lumbar support chair are usually made of polymer materials, such as polypropylene resin and thermoplastic elastomer. Among them, polypropylene resin is not only easy to process, but also can be processed and designed into a complex shape of the back structure through various processes such as injection molding and blow molding to meet the needs of lumbar protection design. At the same time, it has good chemical stability and heat resistance, which helps to extend the service life of the lumbar support chair and reduce deformation or damage caused by chemical corrosion or high temperature environment. However, the plastic sheet of the lumbar support chair made of polypropylene resin is also prone to problems such as the high hardness, poor elasticity, relatively weak strength and supporting capacity of the polypropylene resin material, resulting in certain limitations in the comfort and load-bearing capacity of the plastic sheet of the lumbar support chair made of polypropylene resin, which reduces the load-bearing stability and comfort of the lumbar support chair in daily use.

[0003] In order to increase the application demand of polypropylene resin in lumbar support sitting chairs, polypropylene resin is usually blended with other functional plastics, mineral filling materials or external additives to modify the polypropylene resin. However, affected by the raw materials of polypropylene resin, the components of external additives and the processing technology, the content of volatile organic matter in the modified polypropylene resin is often higher, and it is more likely to release harmful volatile organic compounds. After the modified polypropylene resin is processed into a plastic sheet for lumbar support sitting chairs, the plastic sheet for lumbar support sitting chairs has a strong odor, which threatens human health and affects the user experience of the lumbar support sitting chair. In order to solve the odor problem of modified polypropylene resin, the odor of modified polypropylene resin is currently mainly reduced by using low-odor additives and adsorbents. However, low-odor additives cannot completely avoid the generation of odor. For example, PP-g-MAH compatibilizer is a low-odor compatibilizer, but since free MAH monomers are easily left in the PP-g-MAH compatibilizer, the PP-g-MAH compatibilizer is easy to release a pungent odor after addition. Ordinary physical adsorbents, such as activated carbon, molecular sieves, etc., can adsorb odors, but the adsorption capacity of physical adsorption is limited, and there are problems of incomplete adsorption or large addition amounts. Summary of the invention

[0004] In view of the deficiencies in the prior art, the present invention provides a rubber sheet for a waist-protecting sitting chair and a preparation method and application thereof.

[0005] A plastic sheet for a waist-protecting sitting chair, comprising the following raw materials: 65-95 parts by weight of polypropylene resin, 5-18 parts by weight of metallocene polyolefin elastomer, 10-30 parts by weight of composite glass fiber filler, 3-8 parts by weight of PP-g-MAH compatibilizer, 1-6 parts by weight of composite odor absorbent, 1-9 parts by weight of masterbatch, 0.4-1 parts by weight of antioxidant and 0.3-1.5 parts by weight of lubricant; The raw materials of the composite glass fiber filler include: 60 to 110 parts by weight of an amination nano boron nitride dispersion and 12 to 30 parts by weight of pretreated glass fibers, wherein the amination nano boron nitride dispersion is prepared by mixing amination nano boron nitride with deionized water in a weight ratio of (5 to 18): (30 to 50), and the pretreated glass fibers are obtained by alkalizing the glass fibers, modifying them with a titanate coupling agent, filtering, washing and drying them; Aminated nano boron nitride is obtained by modifying nano boron nitride through amino modification; The raw materials of the composite odor absorbent include: pretreated activated carbon and a cerium nitrate solution with a concentration of 0.1 mol / L, wherein the solid-liquid mass ratio of the pretreated activated carbon to the cerium nitrate solution is (1-5): (20-50), wherein the pretreated activated carbon is obtained by washing the activated carbon with deionized water, filtering and drying.

[0006] A method for preparing a rubber sheet for a waist-protecting sitting chair comprises the following steps: S1: pretreatment of glass fiber, adding glass fiber to sodium hydroxide solution for alkalization treatment, filtering, washing and drying to obtain surface roughened glass fiber, then adding the surface roughened glass fiber to titanate coupling agent for modification treatment, filtering, washing and drying to obtain pretreated glass fiber; S2: Preparation of composite glass fiber filler, using urea to modify nano boron nitride by amination to obtain amination nano boron nitride, mixing the amination nano boron nitride with deionized water to prepare an amination nano boron nitride dispersion, stirring the amination nano boron nitride dispersion with pretreated glass fiber to react, filtering, taking precipitation, and drying to obtain a composite glass fiber filler; S3: Preparation of composite odor absorbent, washing the activated carbon with deionized water, filtering and drying to obtain pretreated activated carbon, immersing the pretreated activated carbon in a cerium nitrate solution for a period of time, and after the immersion, rotary evaporation, drying and roasting to obtain a composite odor absorbent; S4: Preparation of a polypropylene composite material, comprising mixing 65 to 95 parts by weight of a polypropylene resin, 5 to 18 parts by weight of a metallocene polyolefin elastomer, 10 to 30 parts by weight of a composite glass fiber filler, 3 to 8 parts by weight of a PP-g-MAH compatibilizer, 1 to 6 parts by weight of a composite odor absorbent, 1 to 9 parts by weight of a masterbatch, 0.4 to 1 parts by weight of an antioxidant, and 0.3 to 1.5 parts by weight of a lubricant in a high-speed mixer to obtain a mixed material, and then melt-blending the mixed material to obtain a polypropylene composite material; S5: The rubber sheet for the lumbar support sitting chair is processed and formed, and the polypropylene composite material is extruded from a twin-screw extruder into a mold, and the rubber sheet for the lumbar support sitting chair is obtained through cooling, shaping, cutting and trimming.

[0007] Furthermore, step S1 of glass fiber pretreatment processing specifically includes the following steps: S1.1: Add glass fiber to a sodium hydroxide solution with a concentration of 0.3-1 mol / L, wherein the length of the single fiber of the glass fiber is 40-70 μm, the diameter is 10-20 μm, and the solid-liquid mass ratio of the glass fiber to the sodium hydroxide solution is (1-5):(10-20), and ultrasonic treatment is performed at 60-90°C for 15-30 min; S1.2: Then, the treated glass fiber is filtered out, washed with deionized water for 2 to 5 times, and dried at 50 to 60° C. for 2 to 4 hours to obtain a glass fiber with a roughened surface; S1.3: The surface roughened glass fiber is completely immersed in the titanate coupling agent for 30 to 50 minutes, and then filtered, washed and dried to obtain the pretreated glass fiber.

[0008] Furthermore, step S2 of preparing the composite glass fiber filler specifically comprises the following steps: S2.1: Add nano boron nitride, urea, deionized water and steel balls with a diameter of 5 mm into a ball mill, the weight ratio of nano boron nitride, urea, deionized water and steel balls is (1-8): (60-100): (60-130): (50-100), and ball mill at 800-1000 r / min for 2-6 hours. After the ball milling is completed, a reaction mixture is obtained; S2.2: The reaction mixture is centrifuged at 1000-1200 r / min for 15-20 min, the upper suspension is collected, the upper suspension is centrifuged at 4500-5000 r / min for 20-30 min, the lower precipitate is taken, and the lower precipitate is dried and ground to obtain amino-modified nano-boron nitride; S2.3: Mix the amino-treated nano-boron nitride and deionized water in a weight ratio of (5-18): (30-50), and perform ultrasonic treatment for 10-20 minutes to obtain an amino-treated nano-boron nitride dispersion; S2.4: Take 60-110 parts by weight of amino-modified nano-boron nitride dispersion and 12-30 parts by weight of pretreated glass fiber and add them into a reaction container, stir and react at 40-60°C for 3-5 hours. After the reaction is completed, filter and collect the precipitate. After drying the precipitate, a composite glass fiber filler is prepared.

[0009] Furthermore, step S3 of preparing the composite odor absorbent specifically comprises the following steps: S3.1: completely immersing the activated carbon in deionized water and ultrasonically treating it for 10 to 15 minutes to remove surface impurities, and then filtering and drying to obtain pretreated activated carbon, wherein the particle size of the activated carbon is 50 to 200 μm; S3.2: Immerse the pretreated activated carbon in a 0.1 mol / L cerium nitrate solution, wherein the solid-liquid mass ratio of the pretreated activated carbon to the cerium nitrate solution is (1-5): (20-50), and immerse at 40-60°C for 3-5 hours. After the immersion, perform rotary evaporation at 60-65°C for 10-20 minutes, and then dry at 90-110°C for 20-40 minutes, and then calcine at 350-450°C in a nitrogen atmosphere for 3-5 hours to obtain a composite odor adsorbent.

[0010] Furthermore, the metallocene polyolefin elastomer is an ethylene-octene copolymer, and its density is 0.86-0.88 g / cm 3 , the melt index is 5-10g / 10min.

[0011] Furthermore, the antioxidant is at least one of a thioester antioxidant, a phosphite antioxidant or a hindered phenol antioxidant.

[0012] Furthermore, the lubricant is at least one of a stearic acid lubricant, a stearate lubricant or an amide lubricant.

[0013] Furthermore, the extrusion temperature of the polypropylene composite material from the twin-screw extruder is 180 to 220° C., the pressure is 12 to 18 MPa, and the vacuum degree is -0.1 to -0.6 MPa.

[0014] The invention discloses an application of a plastic sheet for a waist-protecting sitting chair. The plastic sheet for the waist-protecting sitting chair is used as a seat and a backrest of the waist-protecting sitting chair and is used on an office chair, a car seat or a sofa.

[0015] The present invention has the following advantages: 1. The present invention utilizes urea to perform amino modification on nano boron nitride, so that the amino groups on the urea are grafted onto the surface of the nano boron nitride to prepare amino nano boron nitride. Subsequently, the amino nano boron nitride is mixed with the pretreated glass fiber for reaction, and the amino nano boron nitride and the glass fiber are grafted and polymerized to form a composite glass fiber filler. The generated composite glass fiber filler is used as a filler for a polypropylene composite material. With the help of the high strength and high modulus characteristics of the glass fiber, the strength and toughness of the polypropylene composite material can be effectively enhanced. At the same time, the amino nano boron nitride grafted onto the surface of the glass fiber can further enhance the overall strength of the composite glass fiber filler through the interface reinforcement effect, and enhance the mechanical properties of the polypropylene composite material, thereby enhancing the strength and toughness of the rubber plate for the lumbar support sitting chair.

[0016] 2. In the present invention, the composite glass fiber filler can not only improve the mechanical properties of the polypropylene composite material through the synergistic effect of the amino nano-boron nitride and the glass fiber, but also, in the preparation process of the polypropylene composite material, the amino group on the surface of the amino nano-boron nitride interacts with the carboxyl group on the free MAH monomer, so that the free MAH monomer generated in the PP-g-MAH compatibilizer can be adsorbed and fixed in the composite glass fiber filler, thereby achieving the purpose of reducing the odor of the polypropylene composite material, which is beneficial to reduce the pungent odor of the rubber sheet for lumbar support sitting chair after the polypropylene composite material is prepared into the rubber sheet for lumbar support sitting chair.

[0017] 3. The composite odor adsorbent of the present invention is composed of activated carbon and nano-cerium oxide. Nano-cerium oxide crystals are filled on the surface of the activated carbon by utilizing the principle of physical adsorption and chemical bonding, so that the activated carbon and nano-cerium oxide can cooperate with each other to effectively adsorb and deodorize the odor molecules generated in the polypropylene composite material. The activated carbon in the composite odor adsorbent has a porous structure and a large specific surface area, so that the activated carbon provides a large number of pores and surface areas for capturing and fixing odor molecules. When the odor molecules adsorbed by the activated carbon come into contact with the nano-cerium oxide loaded on the surface of the activated carbon, the active sites on the surface of the nano-cerium oxide can chemically react with the functional groups in the odor molecules and form chemical bonds, which further adsorbs and fixes the odor molecules, thereby facilitating the acquisition of a low-odor polypropylene composite material and improving the odor of the rubber sheet for the lumbar support chair.

[0018] 4. In the present invention, metallocene polyolefin elastomer is added to the polypropylene resin as an impact modifier. The metallocene polyolefin elastomer, due to its good polypropylene compatibility and special semi-crystalline structure, gives the polypropylene composite material good flexibility and elasticity. After the polypropylene composite material is prepared into a rubber sheet for a lumbar support sitting chair, the toughness effect of the rubber sheet for a lumbar support sitting chair can be further improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The present invention is a flow chart of a method for preparing a rubber sheet for a waist protection posture chair in an embodiment of the present invention.

[0020] Figure 2 This is a structural diagram showing the rubber sheet for the lumbar support posture chair prepared in an embodiment of the present invention.

[0021] Figure 3 This is a structural display diagram from another angle of the rubber plate for the lumbar protection sitting chair prepared in an embodiment of the present invention. DETAILED DESCRIPTION

[0022] In order to enable those skilled in the art to better understand the technical solutions of the present invention, the present invention is further described through the following implementation modes. It should be understood that the following implementation modes are only used to illustrate the present invention, but not to limit the present invention. Example 1

[0023] A method for preparing a rubber sheet for a waist-protecting sitting chair, such as Figure 1 As shown, the specific steps include: S1: Glass fiber pretreatment processing, S1.1: Add glass fiber with a monofilament length of 50 μm and a diameter of 20 μm into a sodium hydroxide solution with a concentration of 1 mol / L, and the solid-liquid mass ratio of the glass fiber to the sodium hydroxide solution is 1:10, and ultrasonically treat for 30 min at 90°C; S1.2: Subsequently, the treated glass fiber is filtered out, washed with deionized water for 5 times, and dried at 60° C. for 2 h to obtain a glass fiber with a roughened surface; S1.3: completely immersing the surface roughened glass fiber in a titanate coupling agent for 50 minutes, and then filtering, washing and drying to obtain a pretreated glass fiber; S2: Preparation of composite glass fiber filler, S2.1: Add nano boron nitride, urea, deionized water and steel balls with a diameter of 5 mm into a ball mill, the weight ratio of nano boron nitride, urea, deionized water and steel balls is 7:100:130:60, and ball mill at 1000 r / min for 6 h. After the ball milling is completed, a reaction mixture is obtained; S2.2: The reaction mixture is centrifuged at 1200 r / min for 20 min, the upper suspension is collected, the upper suspension is centrifuged at 5000 r / min for 30 min, the lower precipitate is taken, and the lower precipitate is dried and ground to obtain amino-modified nano-boron nitride; S2.3: Mix the amino-treated nano-boron nitride and deionized water in a weight ratio of 12:50, and perform ultrasonic treatment for 20 minutes to obtain an amino-treated nano-boron nitride dispersion; S2.4: 110 parts by weight of amination-modified nano-boron nitride dispersion and 30 parts by weight of pretreated glass fiber are added to a reaction vessel, stirred and reacted at 50° C. for 5 h. After the reaction is completed, the precipitate is filtered and dried to obtain a composite glass fiber filler. S3: Preparation of composite odor absorbent, S3.1: Activated carbon with a particle size of 80 μm is completely immersed in deionized water and ultrasonically treated for 15 min to remove surface impurities, and then filtered and dried to obtain pretreated activated carbon; S3.2: The pretreated activated carbon was immersed in a 0.1 mol / L cerium nitrate solution, the solid-liquid mass ratio of the pretreated activated carbon to the cerium nitrate solution was 1:10, and the mixture was immersed at 60°C for 5 hours. After the immersion, the mixture was rotary evaporated at 65°C for 10 minutes, and then dried at 90°C for 40 minutes. Then, the mixture was calcined at 400°C in a nitrogen atmosphere for 5 hours to obtain a composite odor adsorbent. S4: Preparation of polypropylene composite materials, 95 parts by weight of polypropylene resin, 14 parts by weight of ethylene-octene copolymer, 30 parts by weight of composite glass fiber filler, 8 parts by weight of PP-g-MAH compatibilizer, 6 parts by weight of composite odor absorbent, 6 parts by weight of masterbatch, 1 part by weight of antioxidant DSTP and 1 part by weight of calcium stearate are mixed at high speed in a high-speed mixer to obtain a mixed material, and then the mixed material is melt-blended to obtain a polypropylene composite material, wherein the density of the ethylene-octene copolymer is 0.86 g / cm 3 , melt index is 6g / 10min; S5: Waist support sitting chair is made of plastic sheet. The polypropylene composite material is extruded from a twin-screw extruder into a mold at an extrusion temperature of 220°C, a pressure of 15MPa, and a vacuum degree of -0.6MPa. After cooling, shaping, cutting, and trimming, a rubber sheet for a waist-protecting sitting chair is obtained. The processed and molded structure of the rubber sheet for the waist-protecting sitting chair is as follows: Figure 2-3 shown. Example 2

[0024] A method for preparing a rubber sheet for a waist-protecting sitting chair, such as Figure 1 As shown, the specific steps include: S1: Glass fiber pretreatment processing, S1.1: Add glass fiber with a monofilament length of 50 μm and a diameter of 20 μm into a sodium hydroxide solution with a concentration of 1 mol / L, and the solid-liquid mass ratio of the glass fiber to the sodium hydroxide solution is 1:10, and ultrasonically treat for 15 min at 60°C; S1.2: Subsequently, the treated glass fiber is filtered out, washed with deionized water for 3 times, and dried at 50° C. for 4 h to obtain a glass fiber with a roughened surface; S1.3: The surface roughened glass fiber is completely immersed in a titanate coupling agent for 30 minutes, and then filtered, washed and dried to obtain a pretreated glass fiber; S2: Preparation of composite glass fiber filler, S2.1: Add nano-boron nitride, urea, deionized water and steel balls with a diameter of 5 mm into a ball mill, the weight ratio of nano-boron nitride, urea, deionized water and steel balls is 7:100:130:60, and ball mill at 800 r / min for 3 h. After the ball milling is completed, a reaction mixture is obtained; S2.2: The reaction mixture was centrifuged at 1000 r / min for 15 min, the upper suspension was collected, the upper suspension was centrifuged at 4500 r / min for 20 min, the lower precipitate was taken, and the lower precipitate was dried and ground to obtain amino-modified nano-boron nitride; S2.3: Mix the amino-treated nano-boron nitride and deionized water in a weight ratio of 12:50, and perform ultrasonic treatment for 10 minutes to obtain an amino-treated nano-boron nitride dispersion; S2.4: 110 parts by weight of amination-modified nano-boron nitride dispersion and 30 parts by weight of pretreated glass fiber are added to a reaction vessel, and stirred at 40°C for 6 hours. After the reaction is completed, the precipitate is filtered and dried to obtain a composite glass fiber filler. S3: Preparation of composite odor absorbent, S3.1: Activated carbon with a particle size of 80 μm is completely immersed in deionized water and subjected to ultrasonic treatment for 10 min to remove surface impurities, and then filtered and dried to obtain pretreated activated carbon; S3.2: The pretreated activated carbon was immersed in a 0.1 mol / L cerium nitrate solution, the solid-liquid mass ratio of the pretreated activated carbon to the cerium nitrate solution was 1:10, and the mixture was immersed at 40°C for 3 hours. After the immersion, the mixture was rotary evaporated at 60°C for 20 minutes, and then dried at 100°C for 20 minutes. Then, the mixture was calcined at 450°C in a nitrogen atmosphere for 3 hours to obtain a composite odor adsorbent. S4: Preparation of polypropylene composite materials, 95 parts by weight of polypropylene resin, 14 parts by weight of ethylene-octene copolymer, 30 parts by weight of composite glass fiber filler, 8 parts by weight of PP-g-MAH compatibilizer, 6 parts by weight of composite odor absorbent, 6 parts by weight of masterbatch, 1 part by weight of antioxidant DSTP and 1 part by weight of calcium stearate are mixed at high speed in a high-speed mixer to obtain a mixed material, and then the mixed material is melt-blended to obtain a polypropylene composite material, wherein the density of the ethylene-octene copolymer is 0.86 g / cm 3 , melt index is 6g / 10min; S5: Waist support sitting chair is made of plastic sheet. The polypropylene composite material is extruded from a twin-screw extruder into a mold at an extrusion temperature of 180°C, a pressure of 12MPa, and a vacuum degree of -0.3MPa. After cooling, shaping, cutting, and trimming, a rubber sheet for a waist-protecting sitting chair is obtained. The processed and molded structure of the rubber sheet for the waist-protecting sitting chair is as follows: Figure 2-3 shown. Example 3

[0025] A method for preparing a rubber sheet for a waist-protecting sitting chair, such as Figure 1 As shown, the specific steps include: S1: Glass fiber pretreatment processing, S1.1: Add glass fiber with a monofilament length of 50 μm and a diameter of 20 μm into a sodium hydroxide solution with a concentration of 1 mol / L, and the solid-liquid mass ratio of the glass fiber to the sodium hydroxide solution is 1:4, and ultrasonically treat for 30 min at 90°C; S1.2: Subsequently, the treated glass fiber is filtered out, washed with deionized water for 5 times, and dried at 60° C. for 2 h to obtain a glass fiber with a roughened surface; S1.3: completely immersing the surface roughened glass fiber in a titanate coupling agent for 50 minutes, and then filtering, washing and drying to obtain a pretreated glass fiber; S2: Preparation of composite glass fiber filler, S2.1: Add nano-boron nitride, urea, deionized water and steel balls with a diameter of 5 mm into a ball mill, the weight ratio of nano-boron nitride, urea, deionized water and steel balls is 1:60:60:50, and ball mill at 800 r / min for 3 h. After the ball milling is completed, a reaction mixture is obtained; S2.2: The reaction mixture was centrifuged at 1000 r / min for 15 min, the upper suspension was collected, the upper suspension was centrifuged at 4500 r / min for 20 min, the lower precipitate was taken, and the lower precipitate was dried and ground to obtain amino-modified nano-boron nitride; S2.3: Mix the amino-treated nano-boron nitride and deionized water in a weight ratio of 5:30, and perform ultrasonic treatment for 10 minutes to obtain an amino-treated nano-boron nitride dispersion; S2.4: 60 parts by weight of amination-modified nano-boron nitride dispersion and 12 parts by weight of pretreated glass fiber are added to a reaction vessel, and stirred at 40°C for 6 hours. After the reaction is completed, the precipitate is filtered and dried to obtain a composite glass fiber filler. S3: Preparation of composite odor absorbent, S3.1: Activated carbon with a particle size of 80 μm is completely immersed in deionized water and ultrasonically treated for 15 min to remove surface impurities, and then filtered and dried to obtain pretreated activated carbon; S3.2: The pretreated activated carbon was immersed in a cerium nitrate solution with a concentration of 0.1 mol / L, the solid-liquid mass ratio of the pretreated activated carbon to the cerium nitrate solution was 1:20, and the mixture was immersed at 60°C for 5 hours. After the immersion, the mixture was rotary evaporated at 65°C for 10 minutes, and then dried at 90°C for 40 minutes. Then, the mixture was calcined at 400°C in a nitrogen atmosphere for 5 hours to obtain a composite odor adsorbent. S4: Preparation of polypropylene composite materials, 65 parts by weight of polypropylene resin, 5 parts by weight of ethylene-octene copolymer, 10 parts by weight of composite glass fiber filler, 3 parts by weight of PP-g-MAH compatibilizer, 2 parts by weight of composite odor absorbent, 2 parts by weight of masterbatch, 0.4 parts by weight of antioxidant DSTP and 0.8 parts by weight of calcium stearate are mixed at high speed in a high-speed mixer to obtain a mixed material, and then the mixed material is melt-blended to obtain a polypropylene composite material, wherein the density of the ethylene-octene copolymer is 0.86 g / cm 3 , melt index is 6g / 10min; S5: Waist support sitting chair is made of plastic sheet. The polypropylene composite material is extruded from a twin-screw extruder into a mold at an extrusion temperature of 220°C, a pressure of 15MPa, and a vacuum degree of -0.6MPa. After cooling, shaping, cutting, and trimming, a rubber sheet for a waist-protecting sitting chair is obtained. The processed and molded structure of the rubber sheet for the waist-protecting sitting chair is as follows: Figure 2-3 shown.

[0026] Comparative Example 1 Compared with Example 1, the difference of Comparative Example 1 is that steps S2.1-S2.2 are removed, and the amino-treated nano-boron nitride in step S2.3 is replaced by nano-boron nitride. After preparing the nano-boron nitride dispersion, the nano-boron nitride dispersion is mixed with the pretreated glass fiber to obtain a composite glass fiber filler. The other steps remain unchanged to prepare a polypropylene composite material, which is then processed into a rubber sheet for a lumbar protection sitting chair, which is recorded as Comparative Example 1.

[0027] Comparative Example 2 Compared with Example 1, the difference of Comparative Example 2 is that the composite glass fiber filler in step S4 is replaced with an equal weight portion of glass fiber, and the other steps remain unchanged to prepare a polypropylene composite material, which is then processed into a rubber sheet for a lumbar protection sitting chair, recorded as Comparative Example 2.

[0028] Comparative Example 3 Compared with Example 1, the difference of Comparative Example 3 is that the composite glass fiber filler in step S4 is replaced by an equal weight portion of amino-treated nano-boron nitride, and the other steps remain unchanged to prepare a polypropylene composite material, which is then processed into a rubber sheet for a lumbar protection sitting chair, which is recorded as Comparative Example 3.

[0029] Comparative Example 4 Compared with Example 1, the difference of Comparative Example 4 is that the composite odor absorbent in step S4 is removed, and the other steps remain unchanged to prepare a polypropylene composite material, which is then processed into a rubber sheet for a lumbar protection sitting chair, which is recorded as Comparative Example 4.

[0030] Comparative Example 5 Compared with Example 1, the difference of Comparative Example 5 is that the composite odor absorber in step S4 is replaced by the pretreated activated carbon in step S3.1, and the other steps remain unchanged to prepare a polypropylene composite material, which is then processed into a rubber sheet for a lumbar protection sitting chair, which is recorded as Comparative Example 5.

[0031] Comparative Example 6 Compared with Example 1, the difference of Comparative Example 6 is that the composite odor absorbent in step S4 is replaced by an equal weight portion of nano cerium oxide powder, and the other steps remain unchanged to prepare a polypropylene composite material, which is then processed into a rubber sheet for a lumbar protection sitting chair, which is recorded as Comparative Example 6.

[0032] Comparative Example 7 Compared with Example 1, the difference of Comparative Example 7 is that the ethylene-octene copolymer in step S4 is removed, and the other steps remain unchanged to prepare a polypropylene composite material, which is then processed into a rubber sheet for a lumbar support sitting chair, which is recorded as Comparative Example 7.

[0033] Mechanical properties test The polypropylene composite materials obtained in Examples 1-3 and Comparative Examples 1-3 and 7 were extruded into test samples of corresponding sizes. The tensile performance test was carried out according to the test standard of ISO527, the size of the test sample was 150*10*4mm, and the tensile speed was 50mm / min; the bending performance test was carried out according to the test standard of ISO178, the size of the test sample was 80*10*4mm, and the bending speed was 2mm / min; the impact strength performance test was carried out according to the test standard of ISO180, and the size of the test sample was 80*10*4mm. The mechanical properties test results are shown in Table 1.

[0034] Table 1:

[0035] As can be seen from Table 1, the polypropylene composite materials prepared in Examples 1-3, whether in terms of tensile strength, flexural strength, flexural modulus or impact strength, the test results are all better than those of Comparative Examples 1-3 and Comparative Example 7, indicating that the addition of composite glass fiber filler and ethylene-octene copolymer can effectively improve the mechanical properties of the polypropylene composite materials, improve the deformation strength and impact toughness of the polypropylene composite materials, and thus help improve the strength and toughness of the rubber sheet for the lumbar support chair.

[0036] Smell test The odor test was conducted according to the test method of PV3900-2000. Specifically, the rubber sheets for waist-protecting sitting chairs prepared in Examples 1-3 and Comparative Examples 1-6 were placed in a dry environment at a temperature of 80°C for 2 hours. Then, 5 testers were asked to judge and score each rubber sheet for waist-protecting sitting chair by smell, and the average of the judgement scores was taken as the final odor level result value (the judgment standard of the odor level: no odor or not easy to feel is level 1, odor but no irritating odor is level 2, obvious odor but no irritating odor is level 3, irritating odor is level 4, obvious irritating odor is level 5, and unbearable odor is level 6); the volatile organic matter (TVOC) content of the rubber sheets for waist-protecting sitting chairs prepared in Examples 1-3 and Comparative Examples 1-6 was conducted according to the test standard of VDA277-1995. The odor test results are shown in Table 2.

[0037] Table 2:

[0038] As shown in Table 2, the plastic sheets for waist-protecting sitting chairs made of the polypropylene composite materials prepared in Examples 1-3 have TVOC contents of less than 12 μgC / g and have no obvious or irritating odor. However, the polypropylene composite materials prepared in Comparative Examples 1-2 use a composite glass fiber filler composed of glass fiber and nano-boron nitride or glass fiber as a filler, and do not add an amination nano-boron nitride component. Therefore, the plastic sheets for waist-protecting sitting chairs prepared therefrom have a certain irritating odor, indicating that the amination nano-boron nitride component of the composite glass fiber filler in Examples 1-3 can play a role in irritating odor molecules. It has a certain adsorption and removal effect, reducing the generation and release of irritating odors; and although the plastic sheets for waist protection sitting chairs made of polypropylene composite materials obtained in Comparative Examples 4-6 do not have irritating odors, they all have relatively obvious odors. It can also be seen from the test results of TVOC content that in Comparative Examples 4-6, when no composite odor adsorbent is added or only activated carbon or only nano-cerium oxide is added, the TVOC content in the polypropylene composite materials is relatively high, indicating that the addition and use of composite odor adsorbents can effectively reduce the odor of the polypropylene composite materials, thereby improving the odor of the processed and formed plastic sheets for waist protection sitting chairs.

[0039] It should be understood that those skilled in the art can make improvements or changes based on the above description, and all such improvements and changes should fall within the scope of protection of the appended claims of the present invention. Parts not described in detail in this specification belong to the prior art known to those skilled in the art.

Claims

1. A rubber sheet for a waist-protecting sitting chair, characterized in that: Including the following raw materials: 65-95 parts by weight of polypropylene resin, 5-18 parts by weight of metallocene polyolefin elastomer, 10-30 parts by weight of composite glass fiber filler, 3-8 parts by weight of PP-g-MAH compatibilizer, 1-6 parts by weight of composite odor absorbent, 1-9 parts by weight of masterbatch, 0.4-1 parts by weight of antioxidant and 0.3-1.5 parts by weight of lubricant; The raw materials of the composite glass fiber filler include: 60 to 110 parts by weight of an amination nano boron nitride dispersion and 12 to 30 parts by weight of pretreated glass fibers, wherein the amination nano boron nitride dispersion is prepared by mixing amination nano boron nitride with deionized water in a weight ratio of (5 to 18): (30 to 50), and the pretreated glass fibers are obtained by alkalizing the glass fibers, modifying them with a titanate coupling agent, filtering, washing and drying them; Aminated nano boron nitride is obtained by modifying nano boron nitride through amino modification; The raw materials of the composite odor absorbent include: pretreated activated carbon and a cerium nitrate solution with a concentration of 0.1 mol / L, wherein the solid-liquid mass ratio of the pretreated activated carbon to the cerium nitrate solution is (1-5): (20-50), wherein the pretreated activated carbon is obtained by washing the activated carbon with deionized water, filtering and drying.

2. A method for preparing the rubber sheet for waist-protecting sitting chair according to claim 1, characterized in that: The steps include: S1: pretreatment of glass fiber, adding glass fiber to sodium hydroxide solution for alkalization treatment, filtering, washing and drying to obtain surface roughened glass fiber, then adding the surface roughened glass fiber to titanate coupling agent for modification treatment, filtering, washing and drying to obtain pretreated glass fiber; S2: Preparation of composite glass fiber filler, using urea to modify nano boron nitride by amination to obtain amination nano boron nitride, mixing the amination nano boron nitride with deionized water to prepare an amination nano boron nitride dispersion, stirring the amination nano boron nitride dispersion with pretreated glass fiber to react, filtering, taking precipitation, and drying to obtain a composite glass fiber filler; S3: Preparation of composite odor absorbent, washing the activated carbon with deionized water, filtering and drying to obtain pretreated activated carbon, immersing the pretreated activated carbon in a cerium nitrate solution for a period of time, and after the immersion, rotary evaporation, drying and roasting to obtain a composite odor absorbent; S4: Preparation of a polypropylene composite material, comprising mixing 65 to 95 parts by weight of a polypropylene resin, 5 to 18 parts by weight of a metallocene polyolefin elastomer, 10 to 30 parts by weight of a composite glass fiber filler, 3 to 8 parts by weight of a PP-g-MAH compatibilizer, 1 to 6 parts by weight of a composite odor absorbent, 1 to 9 parts by weight of a masterbatch, 0.4 to 1 parts by weight of an antioxidant, and 0.3 to 1.5 parts by weight of a lubricant in a high-speed mixer to obtain a mixed material, and then melt-blending the mixed material to obtain a polypropylene composite material; S5: The rubber sheet for the lumbar support sitting chair is processed and formed, and the polypropylene composite material is extruded from a twin-screw extruder into a mold, and the rubber sheet for the lumbar support sitting chair is obtained through cooling, shaping, cutting and trimming.

3. The method for preparing the rubber sheet for waist-protecting sitting chair according to claim 2, characterized in that: Step S1: pre-treatment of glass fiber, specifically including the following steps: S1.1: Add glass fiber to a sodium hydroxide solution with a concentration of 0.3-1 mol / L, wherein the length of the single fiber of the glass fiber is 40-70 μm, the diameter is 10-20 μm, and the solid-liquid mass ratio of the glass fiber to the sodium hydroxide solution is (1-5):(10-20), and ultrasonic treatment is performed at 60-90°C for 15-30 min; S1.2: Then, the treated glass fiber is filtered out, washed with deionized water for 2 to 5 times, and dried at 50 to 60° C. for 2 to 4 hours to obtain a glass fiber with a roughened surface; S1.3: The surface roughened glass fiber is completely immersed in the titanate coupling agent for 30 to 50 minutes, and then filtered, washed and dried to obtain the pretreated glass fiber.

4. The method for preparing the rubber sheet for waist-protecting sitting chair according to claim 3, characterized in that: Step S2: preparing the composite glass fiber filler, specifically comprising the following steps: S2.1: Add nano boron nitride, urea, deionized water and steel balls with a diameter of 5 mm into a ball mill, the weight ratio of nano boron nitride, urea, deionized water and steel balls is (1-8): (60-100): (60-130): (50-100), and ball mill at 800-1000 r / min for 2-6 hours. After the ball milling is completed, a reaction mixture is obtained; S2.2: The reaction mixture is centrifuged at 1000-1200 r / min for 15-20 min, the upper suspension is collected, the upper suspension is centrifuged at 4500-5000 r / min for 20-30 min, the lower precipitate is taken, and the lower precipitate is dried and ground to obtain amino-modified nano-boron nitride; S2.3: Mix the amino-treated nano-boron nitride and deionized water in a weight ratio of (5-18): (30-50), and perform ultrasonic treatment for 10-20 minutes to obtain an amino-treated nano-boron nitride dispersion; S2.4: Take 60-110 parts by weight of amino-modified nano-boron nitride dispersion and 12-30 parts by weight of pretreated glass fiber and add them into a reaction container, stir and react at 40-60°C for 3-5 hours. After the reaction is completed, filter and collect the precipitate. After drying the precipitate, a composite glass fiber filler is prepared.

5. The method for preparing the rubber sheet for waist-protecting sitting chair according to claim 4, characterized in that: Step S3: preparing the composite odor absorbent, specifically comprising the following steps: S3.1: completely immersing the activated carbon in deionized water and ultrasonically treating it for 10 to 15 minutes to remove surface impurities, and then filtering and drying to obtain pretreated activated carbon, wherein the particle size of the activated carbon is 50 to 200 μm; S3.2: Immerse the pretreated activated carbon in a 0.1 mol / L cerium nitrate solution, wherein the solid-liquid mass ratio of the pretreated activated carbon to the cerium nitrate solution is (1-5): (20-50), and immerse at 40-60°C for 3-5 hours. After the immersion, perform rotary evaporation at 60-65°C for 10-20 minutes, and then dry at 90-110°C for 20-40 minutes, and then calcine at 350-450°C in a nitrogen atmosphere for 3-5 hours to obtain a composite odor adsorbent.

6. The method for preparing the rubber sheet for waist-protecting sitting chair according to claim 2, characterized in that: Metallocene polyolefin elastomer is an ethylene-octene copolymer with a density of 0.86-0.88 g / cm 3 , the melt index is 5-10g / 10min.

7. The method for preparing the rubber sheet for waist-protecting sitting chair according to claim 6, characterized in that: The antioxidant is at least one of a thioester antioxidant, a phosphite antioxidant or a hindered phenol antioxidant.

8. The method for preparing the rubber sheet for waist-protecting sitting chair according to claim 7, characterized in that: The lubricant is at least one of a stearic acid lubricant, a stearate lubricant or an amide lubricant.

9. The method for preparing the rubber sheet for waist-protecting sitting chair according to claim 2, characterized in that: The extrusion temperature of the polypropylene composite material extruded from the twin-screw extruder is 180-220° C., the pressure is 12-18 MPa, and the vacuum degree is -0.1--0.6 MPa.

10. An application of the rubber sheet for waist-protecting sitting chair according to claim 1, characterized in that: The lumbar support posture chair uses a plastic sheet as the seat and back of the lumbar support posture chair and is used on office chairs, car seats or sofas.

Citation Information

Patent Citations

  • Polypropylene composite material and preparation method and application thereof

    CN103374180A

  • Low-odor polypropylene composition as well as preparation method and application thereof

    CN113248829A

  • Low-odor polypropylene master batch as well as preparation method and application thereof

    CN115873346A

  • Fiber-Reinforced Propylene Composition Having Ultralow Emissions

    US20240132707A1