High-strength plant fiber reinforced polypropylene composite material and preparation method thereof

By performing surface modification treatment on plant fibers and combining with the melt plasticization and extrusion process of polypropylene resin, the problem of poor compatibility between plant fibers and polypropylene resin is solved, the mechanical properties of composite materials are significantly improved, and high strength is achieved and high toughness plant fiber reinforced polypropylene composite.

CN118994794AInactive Publication Date: 2024-11-22ANQING HUITONG NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411265285.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Poor compatibility between plant fibers and polypropylene resins leads to the formation of voids and defects in the reinforced composite materials, resulting in poor mechanical properties of composite materials, especially when exhibiting brittleness at high fiber content, making it difficult to obtain materials with excellent mechanical properties.

Method used

The surface modification of plant fibers by using tetrafluoroborate ionic liquid, crosslinking sensitizer and coupling agent is performed to form a modifier diluent for impregnation and drying, and combined with ultraviolet irradiation, the plant fibers and polypropylene resin are improved by improving plant fibers and polypropylene resins. Compatibility and melt plasticization and extrusion granulation in a twin-screw extruder to prepare high-strength plant fiber reinforced polypropylene composites.

Benefits of technology

It significantly improves the enhancement effect of plant fibers on polypropylene, imparts higher mechanical properties to the composite material, enhances its tensile, bending and impact properties, avoids the disadvantages of material bridge building, and improves the mechanical properties of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005036949850000121
    Figure BDA0005036949850000121
Patent Text Reader

Abstract

The invention discloses a high-strength plant fiber reinforced polypropylene composite material and a preparation method thereof, and belongs to the field of polypropylene composite materials. The composite material comprises the following raw materials in parts by mass: 44.5-91 parts of polypropylene, 5-40 parts of modified plant fibers, 0-10 parts of a flexibilizer, 1-5 parts of a compatilizer and 0.5-3 parts of a processing aid, the modified plant fibers are prepared by performing surface modification on plant fibers by adopting tetrafluoroborate ionic liquid, a cross-linking sensitizer and a coupling agent. A comprehensive system of tetrafluoroborate ionic liquid, a cross-linking sensitizer and a coupling agent is used for carrying out surface modification on plant fibers, and ultraviolet lamp irradiation cross-linking curing is matched, so that the surface hydrophobicity effect of the plant fibers is greatly improved, and the characteristic that polypropylene is a hydrophobic non-polar material is matched; the compatibility between the plant fibers and the polypropylene resin is improved; and after the surface-modified plant fibers are added into the polypropylene resin, the reinforcing effect of the plant fibers on polypropylene is improved, and the composite material is endowed with higher mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polypropylene composite materials, and particularly relates to a high-strength plant fiber reinforced polypropylene composite material and a preparation method thereof. Background Art

[0002] Polypropylene (PP) is widely used in the fields of automobiles, home appliances, electronic appliances, power tools, medical equipment, and construction due to its advantages such as low density, acid and alkali resistance, easy processing, excellent comprehensive performance, and high cost performance. In order to further improve its mechanical properties, heat resistance, dimensional stability and other characteristics during the application process, it is usually selected to be reinforced and filled with other reinforcing fillers such as glass fiber, while also reducing material costs. However, since polypropylene is extracted from petroleum, it is a non-renewable resource; in addition, it is not easy to degrade after being discarded, which will cause pressure and damage to the natural ecological environment. All of the above have led to an increasing demand for biodegradable, non-petroleum-based renewable resources. Plant fiber is the most abundant renewable resource in nature. It has a high strength due to its huge hydrogen bond network structure. It is a reinforcing filler for many polymer materials. It plays an irreplaceable role in solving energy and environmental problems, and is in line with the current development theme of carbon neutrality.

[0003] Since the plant fiber surface contains a large number of hydroxyl groups and has strong hydrophilicity, while the hydrophobic polypropylene resin lacks groups that can react with hydroxyl groups, the compatibility between the plant fiber and the polypropylene resin is very poor. Furthermore, when the plant fiber is used to reinforce the polypropylene resin to prepare a composite material, it is easy to form gaps and defects on the interface, resulting in poor mechanical properties of the composite material. In particular, when the plant fiber content is high, the composite material shows obvious brittleness, and it is difficult to obtain a composite material with excellent mechanical properties.

[0004] Therefore, developing a plant fiber reinforced polypropylene composite material with high mechanical properties has excellent market application value prospects. Summary of the invention

[0005] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a high-strength plant fiber reinforced polypropylene composite material and a preparation method thereof, which solves the problems in the prior art.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A plant fiber reinforced polypropylene composite material comprises the following raw materials in parts by weight: 44.5 to 91 parts of polypropylene, 5 to 40 parts of modified plant fiber, 0 to 10 parts of a toughening agent, 1 to 5 parts of a compatibilizer, and 0.5 to 3 parts of a processing aid;

[0008] The modified plant fiber is prepared by surface modification of the plant fiber using tetrafluoroborate ionic liquid, a cross-linking sensitizer and a coupling agent.

[0009] Furthermore, the polypropylene is one or more of homopolypropylene, propylene-ethylene block copolymer, propylene-ethylene random copolymer, and propylene-1-butene random block.

[0010] Furthermore, the compatibilizer is at least one of PP, POE, SEBS, and SEPS grafted with maleic anhydride;

[0011] The toughening agent is at least one of POE, LLDPE, HDPE and SEBS;

[0012] The processing aid is at least one of an antioxidant, a weathering agent, a lubricant, and a toner.

[0013] Furthermore, the modified plant fiber preparation process includes:

[0014] Step 1: prepare a modifier dilution solution by mixing tetrafluoroborate ionic liquid, a cross-linking sensitizer, a coupling agent and a diluent;

[0015] Step 2: soaking and stirring the plant fiber with the modifier dilution;

[0016] Step 3: Take out the impregnated plant fiber, dry it, and expose it to ultraviolet light to obtain surface-modified plant fiber.

[0017] Furthermore, in step 1, the mass ratio of tetrafluoroborate ionic liquid, cross-linking sensitizer, coupling agent and diluent is (5-40): (1-5): (1-5): (50-93);

[0018] In the step 2, the mass ratio of the plant fiber to the modifier dilution is 1:3.

[0019] Further, the tetrafluoroborate ionic liquid is at least one of tetrafluoroborate ionic liquids containing vinyl imidazole, acryl imidazole, acrylonitrile imidazole, styryl imidazole, and epoxy imidazole;

[0020] The cross-linking sensitizer is one or more of trimethallyl isocyanate, triallyl isocyanurate, and tris(2-hydroxyethyl)isocyanurate triacrylate, which have high boiling point and low volatility.

[0021] The coupling agent is at least one of a silane coupling agent, a titanate coupling agent, and an aluminate coupling agent.

[0022] Furthermore, the diluent is at least one of water, methanol, ethanol, propanol, butanone and toluene.

[0023] A method for preparing a plant fiber reinforced polypropylene composite material comprises the following steps:

[0024] S1, preparing a modifier diluent by mixing tetrafluoroborate ionic liquid, a cross-linking sensitizer, a coupling agent, and a diluent in a mass ratio of (5-40):(1-5):(1-5):(50-93); impregnating plant fiber with the modifier diluent in a mass ratio of 1:3 and stirring; taking out the impregnated plant fiber, drying it, and irradiating it under ultraviolet light to obtain a surface-modified plant fiber;

[0025] S2, premixing polypropylene, toughening agent, compatibilizer and processing aid in a high-speed mixer to obtain a premix;

[0026] S3, placing the premix at the main material feeding port of the twin-screw extruder and adding the modified plant fiber from the side feeding port, melting and plasticizing in the twin-screw extruder and extruding into granules.

[0027] Furthermore, the temperatures of zones one to ten of the twin-screw extruder are 160°C, 210°C, 210°C, 210°C, 200°C, 200°C, 200°C, 200°C, 210°C, respectively; and the side feeding port of the twin-screw extruder is located in zone six.

[0028] Application of the above-mentioned plant fiber reinforced polypropylene composite material in the preparation of automobile parts.

[0029] Beneficial effects of the present invention:

[0030] 1. The present invention uses a comprehensive system of tetrafluoroborate ionic liquid, a cross-linking sensitizer, and a coupling agent to modify the surface of plant fibers; wherein the tetrafluoroborate ionic liquid is weakly acidic, and can play a good neutralizing role with the weak alkalinity of the plant fiber surface, eliminate the surface polarity of the plant fiber, and enhance the compatibility of the plant fiber with the polypropylene resin;

[0031] 2. Under the irradiation of ultraviolet light, the cross-linking sensitizer undergoes a cross-linking reaction with the hydroxyl groups on the surface of the plant fiber and the active functional groups in the tetrafluoroborate ionic liquid, which not only changes the fluffy state of the plant fiber surface, but also facilitates avoiding the disadvantages of bridging during material feeding in practical applications.

[0032] 3. After adding the surface-modified plant fibers to the polypropylene resin, the reinforcing effect of the plant fibers on the polypropylene can be increased, giving the composite material a higher mechanical performance advantage. DETAILED DESCRIPTION

[0033] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solution of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] A high-strength plant fiber reinforced polypropylene composite material, comprising the following raw materials in parts by weight: 44.5-91 parts of polypropylene, 5-40 parts of modified plant fiber, 0-10 parts of toughening agent, 1-5 parts of compatibilizer, and 0.5-3 parts of processing aid;

[0035] The polypropylene is one or more of homopolypropylene, propylene-ethylene block copolymer, propylene-ethylene random copolymer and propylene-1-butene random block.

[0036] The compatibilizer is at least one of PP, POE, SEBS and SEPS grafted maleic anhydride.

[0037] The toughening agent is at least one of POE, LLDPE, HDPE and SEBS.

[0038] At least one of the processing aids antioxidant, weathering agent, lubricant, and color powder.

[0039] The modified plant fiber preparation process is as follows:

[0040] Step 1, prepare a modifier dilution solution by mixing tetrafluoroborate ionic liquid, a cross-linking sensitizer, a coupling agent, and a diluent in a mass ratio of (5-40): (1-5): (1-5): (50-93);

[0041] Step 2, soaking the plant fiber and the modifier dilution in a mass ratio of 1:3 and stirring for 5 to 10 minutes;

[0042] Step 3, taking out the impregnated plant fiber and drying it at 50-80° C., and irradiating it under ultraviolet light for 2-4 hours to obtain surface-modified plant fiber.

[0043] The tetrafluoroborate ionic liquid is at least one of tetrafluoroborate ionic liquids containing vinyl imidazole, acryl imidazole, acrylonitrile imidazole, styryl imidazole and epoxy imidazole.

[0044] The cross-linking sensitizer is one or more of trimethallyl isocyanate, triallyl isocyanurate, and tris(2-hydroxyethyl)isocyanurate triacrylate, which have high boiling point and low volatility.

[0045] The coupling agent is at least one of a silane coupling agent, a titanate coupling agent, and an aluminate coupling agent. The diluent of the modifier dilution is at least one of water, methanol, ethanol, propanol, butanone, and toluene.

[0046] The following examples are used to illustrate the preparation process of the polypropylene composite material, and the parts in the examples and comparative examples are all parts by mass; the raw materials and reagents used in the examples are conventionally purchased raw materials and reagents, as follows:

[0047] Polypropylene, copolymer polypropylene, grade K7227H, Wuhan Petrochemical;

[0048] Plant fiber, average fiber length 2mm, from Yuyao Xindegao;

[0049] Compatibilizer, PP-g-MAH, brand CMG5701, Jiayirong;

[0050] Toughener, POE, brand LC565, LG Chemical;

[0051] Propylimidazolium tetrafluoroborate, McCarthy's reagent;

[0052] Cross-linking sensitizer: triallyl isocyanurate (TAIC), Fang Ruida;

[0053] Coupling agent, silane coupling agent, KH550, Xinwang Chemical;

[0054] Other processing aids are commercially available conventional additives, as follows:

[0055] Antioxidant 1010, BASF;

[0056] Antioxidant 168, BASF;

[0057] Light stabilizer, 3808PP5, cyanotera;

[0058] Lubricant calcium stearate, brand BZPP301, Chongqing Baozhuan New Material Technology Co., Ltd.;

[0059] Lubricant silicone masterbatch, brand CV500, Dongguan Hanwei Technology Co., Ltd.;

[0060] Black mother, 2718, Cabot.

[0061] Example 1

[0062] S1. Preparation of modified plant fiber: prepare a modifier diluent by mixing tetrafluoroborate ionic liquid, a cross-linking sensitizer, a coupling agent and a diluent in a mass ratio of 5:1:1:93; immerse the plant fiber in the modifier diluent in a mass ratio of 1:3 and stir for 5 minutes; take out the immersed plant fiber and dry it at 50°C, and expose it under ultraviolet light for 2 hours to obtain surface modified plant fiber.

[0063] S2, premix 44.5 parts of polypropylene, 10 parts of toughening agent, 5 parts of compatibilizer, 10100.2 parts of antioxidant and 1680.3 parts of antioxidant in a high mixer to obtain a premix; add the premix to the main material feeding port of a twin-screw extruder, add 40 parts of modified plant fiber from the side feeding port, melt and plasticize in the twin-screw extruder, extrude and granulate to obtain a high-strength plant fiber reinforced polypropylene composite material;

[0064] Among them, the temperatures of zones 1 to 10 of the twin-screw extruder are: 160°C, 210°C, 210°C, 210°C, 200°C, 200°C, 200°C, 200°C, 210°C respectively; the side feeding port of the twin-screw extruder is located in zone 6.

[0065] Example 2

[0066] S1. Preparation of modified plant fiber: prepare a modifier diluent by mixing tetrafluoroborate ionic liquid, a cross-linking sensitizer, a coupling agent and a diluent in a mass ratio of 10:2:4:84; immerse the plant fiber in the modifier diluent in a mass ratio of 1:3 and stir for 5 minutes; take out the immersed plant fiber and dry it at 60°C, and expose it under ultraviolet light for 3 hours to obtain surface modified plant fiber.

[0067] S2, premix 56 parts of polypropylene, 8 parts of toughening agent, 4 parts of compatibilizer, 0.2 parts of antioxidant 1010, 0.3 parts of antioxidant 168, 0.2 parts of lubricant calcium stearate, 0.3 parts of lubricant silicone masterbatch, and 1 part of black masterbatch in a high-speed mixer to obtain a premix; add the premix to the main material feeding port of a twin-screw extruder, add 30 parts of modified plant fiber from the side feeding port, melt and plasticize in a twin-screw extruder, and extrude and granulate to obtain a high-strength plant fiber reinforced polypropylene composite material;

[0068] The temperatures of zones 1 to 10 of the twin-screw extruder are respectively 160° C., 210° C., 210° C., 210° C., 200° C., 200° C., 200° C., 200° C., 200° C., 210° C. The side feed port of the twin-screw extruder is located in zone 6.

[0069] Example 3

[0070] S1. Preparation of modified plant fiber: prepare a modifier diluent by mixing tetrafluoroborate ionic liquid, a cross-linking sensitizer, a coupling agent and a diluent in a mass ratio of 20:3:3:74; impregnate the plant fiber with the modifier diluent in a mass ratio of 1:3 and stir for 10 minutes; take out the impregnated plant fiber, dry it at 70°C, and expose it to ultraviolet light for 4 hours to obtain surface-modified plant fiber.

[0071] S2, premix 69.2 parts of polypropylene, 6 parts of toughening agent, 3 parts of compatibilizer, 0.2 parts of antioxidant 1010, 0.3 parts of antioxidant 168, 0.3 parts of lubricant calcium stearate, and 1 part of black masterbatch in a high mixer to obtain a premix; add the premix to the main material feeding port of a twin-screw extruder, add 20 parts of modified plant fiber from the side feeding port, melt and plasticize in the twin-screw extruder, and extrude and granulate to obtain a high-strength plant fiber reinforced polypropylene composite material;

[0072] The temperatures of zones 1 to 10 of the twin-screw extruder are respectively 160° C., 210° C., 210° C., 210° C., 200° C., 200° C., 200° C., 200° C., 200° C., 210° C. The side feed port of the twin-screw extruder is located in zone 6.

[0073] Example 4

[0074] S1. Preparation of modified plant fiber: prepare a modifier diluent by mixing tetrafluoroborate ionic liquid, a cross-linking sensitizer, a coupling agent and a diluent in a mass ratio of 30:4:2:64; impregnate the plant fiber with the modifier diluent in a mass ratio of 1:3 and stir for 10 minutes; take out the impregnated plant fiber, dry it at 80°C, and expose it to ultraviolet light for 4 hours to obtain surface-modified plant fiber.

[0075] S2, 81 parts of polypropylene, 4 parts of toughening agent, 2 parts of compatibilizer, 0.2 parts of antioxidant 1010, 0.3 parts of antioxidant 168, 0.2 parts of lubricant calcium stearate, 1 part of lubricant silicone masterbatch, 0.3 parts of light stabilizer, 1 part of black masterbatch are premixed in a high-speed mixer to obtain a premix; the premix is ​​placed in the main material feeding port of a twin-screw extruder and added, 10 parts of modified plant fiber are added from the side feeding port, melt-plasticized in a twin-screw extruder, and extruded and granulated to obtain a high-strength plant fiber reinforced polypropylene composite material;

[0076] The temperatures of zones 1 to 10 of the twin-screw extruder are respectively 160° C., 210° C., 210° C., 210° C., 200° C., 200° C., 200° C., 200° C., 200° C., 210° C. The side feed port of the twin-screw extruder is located in zone 6.

[0077] Example 5

[0078] S1. Preparation of modified plant fiber: prepare a modifier diluent by mixing tetrafluoroborate ionic liquid, a cross-linking sensitizer, a coupling agent and a diluent in a mass ratio of 40:5:5:50; impregnate the plant fiber with the modifier diluent in a mass ratio of 1:3 and stir for 10 minutes; take out the impregnated plant fiber, dry it at 80°C, and expose it to ultraviolet light for 4 hours to obtain surface-modified plant fiber.

[0079] S2, 91 parts of polypropylene, 1 part of compatibilizer, 0.2 parts of antioxidant 1010, 0.3 parts of antioxidant 168, 0.2 parts of lubricant calcium stearate, 1 part of lubricant silicone masterbatch, 0.3 parts of light stabilizer, and 1 part of black masterbatch are premixed in a high-speed mixer to obtain a premix; the premix is ​​placed in the main material feeding port of a twin-screw extruder and added, 5 parts of modified plant fiber are added from the side feeding port, melt-plasticized in a twin-screw extruder, and extruded and granulated to obtain a high-strength plant fiber reinforced polypropylene composite material;

[0080] The temperatures of zones 1 to 10 of the twin-screw extruder are respectively 160° C., 210° C., 210° C., 210° C., 200° C., 200° C., 200° C., 200° C., 210° C. The side feed port of the twin-screw extruder is located in zone 6.

[0081] Comparative Example 1

[0082] 69.2 parts of polypropylene, 6 parts of toughening agent, 3 parts of compatibilizer, 10100.2 parts of antioxidant, 1680.3 parts of antioxidant, 0.3 parts of lubricant calcium stearate and 1 part of black masterbatch are premixed uniformly in a high-speed mixer to obtain a premix; the premix is ​​placed in a main material feeding port of a twin-screw extruder and added, 20 parts of unmodified plant fiber are added from a side feeding port, melt-plasticized in a twin-screw extruder, and extruded and granulated to obtain a plant fiber reinforced polypropylene composite material;

[0083] The temperatures of zones 1 to 10 of the twin-screw extruder are respectively 160° C., 210° C., 210° C., 210° C., 200° C., 200° C., 200° C., 200° C., 210° C. The side feed port of the twin-screw extruder is located in zone 6.

[0084] Comparative Example 2

[0085] S1. Preparation of modified plant fiber: prepare a modifier diluent by mixing a cross-linking sensitizer, a coupling agent and a diluent in a mass ratio of 3:3:94; immerse the plant fiber in the modifier diluent in a mass ratio of 1:3 and stir for 10 minutes; take out the immersed plant fiber and dry it at 70°C, and expose it to ultraviolet light for 4 hours to obtain a surface-treated plant fiber.

[0086] S2, premix 69.2 parts of polypropylene, 6 parts of toughening agent, 3 parts of compatibilizer, 0.2 parts of antioxidant 1010, 0.3 parts of antioxidant 168, 0.3 parts of lubricant calcium stearate, and 1 part of black masterbatch in a high mixer to obtain a premix; add the premix to the main material feeding port of a twin-screw extruder, add 20 parts of surface-treated plant fiber from the side feeding port, melt and plasticize in the twin-screw extruder, and extrude and granulate to obtain a high-strength plant fiber reinforced polypropylene composite material;

[0087] The temperatures of zones 1 to 10 of the twin-screw extruder are respectively 160° C., 210° C., 210° C., 210° C., 200° C., 200° C., 200° C., 200° C., 210° C. The side feed port of the twin-screw extruder is located in zone 6.

[0088] Comparative Example 3

[0089] S1. Preparation of modified plant fiber: prepare a modifier diluent by mixing tetrafluoroborate ionic liquid, coupling agent and diluent in a mass ratio of 20:3:77; impregnate the plant fiber with the modifier diluent in a mass ratio of 1:3 and stir for 10 minutes; take out the impregnated plant fiber, dry it at 70°C, and expose it to ultraviolet light for 4 hours to obtain surface-treated plant fiber.

[0090] S2, premix 69.2 parts of polypropylene, 6 parts of toughening agent, 3 parts of compatibilizer, 0.2 parts of antioxidant 1010, 0.3 parts of antioxidant 168, 0.3 parts of lubricant calcium stearate, and 1 part of black masterbatch in a high mixer to obtain a premix; add the premix to the main material feeding port of a twin-screw extruder, add 20 parts of surface-treated plant fiber from the side feeding port, melt and plasticize in the twin-screw extruder, and extrude and granulate to obtain a high-strength plant fiber reinforced polypropylene composite material;

[0091] The temperatures of zones 1 to 10 of the twin-screw extruder are respectively 160° C., 210° C., 210° C., 210° C., 200° C., 200° C., 200° C., 200° C., 210° C. The side feed port of the twin-screw extruder is located in zone 6.

[0092] Comparative Example 4

[0093] S1. Preparation of modified plant fiber: prepare a modifier diluent by mixing tetrafluoroborate ionic liquid, a cross-linking sensitizer and a diluent in a mass ratio of 20:3:77; impregnate the plant fiber with the modifier diluent in a mass ratio of 1:3 and stir for 10 minutes; take out the impregnated plant fiber, dry it at 70°C, and expose it to ultraviolet light for 4 hours to obtain a surface-treated plant fiber.

[0094] S2, premix 69.2 parts of polypropylene, 6 parts of toughening agent, 3 parts of compatibilizer, 0.2 parts of antioxidant 1010, 0.3 parts of antioxidant 168, 0.3 parts of lubricant calcium stearate, and 1 part of black masterbatch in a high mixer to obtain a premix; add the premix to the main material feeding port of a twin-screw extruder, add 20 parts of modified plant fiber from the side feeding port, melt and plasticize in the twin-screw extruder, and extrude and granulate to obtain a high-strength plant fiber reinforced polypropylene composite material;

[0095] The temperatures of zones 1 to 10 of the twin-screw extruder are respectively 160° C., 210° C., 210° C., 210° C., 200° C., 200° C., 200° C., 200° C., 210° C. The side feed port of the twin-screw extruder is located in zone 6.

[0096] Comparative Example 5

[0097] S1. Preparation of modified plant fiber: prepare a modifier diluent by mixing tetrafluoroborate ionic liquid, a cross-linking sensitizer, a coupling agent and a diluent in a mass ratio of 20:3:3:74; impregnate the plant fiber with the modifier diluent in a mass ratio of 1:3 and stir for 10 minutes; take out the impregnated plant fiber and dry it at 70°C to obtain a surface-treated plant fiber.

[0098] S2, premix 69.2 parts of polypropylene, 6 parts of toughening agent, 3 parts of compatibilizer, 0.2 parts of antioxidant 1010, 0.3 parts of antioxidant 168, 0.3 parts of lubricant calcium stearate, and 1 part of black masterbatch in a high mixer to obtain a premix; add the premix to the main material feeding port of a twin-screw extruder, add 20 parts of modified plant fiber from the side feeding port, melt and plasticize in the twin-screw extruder, and extrude and granulate to obtain a high-strength plant fiber reinforced polypropylene composite material;

[0099] The temperatures of zones 1 to 10 of the twin-screw extruder are respectively 160° C., 210° C., 210° C., 210° C., 200° C., 200° C., 200° C., 200° C., 210° C. The side feed port of the twin-screw extruder is located in zone 6.

[0100] Experimental testing

[0101] The plant fiber reinforced polypropylene composite materials obtained in Examples 1 to 5 and Comparative Examples 1 to 5 were tested for tensile strength, flexural strength, flexural modulus and notched impact strength. It is worth noting that these tests are test methods familiar to those skilled in the art, and the specific test methods are not described in detail here. The test results are shown in Table 1 below:

[0102] Table 1 Test results of polypropylene composite materials obtained from Examples 1 to 5 and Comparative Examples 1 to 5

[0103]

[0104] From the results in Table 1, it can be seen that the plant fiber reinforced polypropylene composite material prepared by the method of the present invention has good tensile properties, bending properties and impact properties; in the polypropylene resin system with added surface modified plant fibers, the composite material exhibits good mechanical properties.

[0105] It can be seen from Example 3 and Comparative Example 1 that when the plant fiber is not surface-modified, its mechanical properties show a significant downward trend. It can be seen from Example 3 and Comparative Examples 2, 3, and 4 that when the plant fiber is surface-treated, the lack of any of the tetrafluoroborate ionic liquid, cross-linking sensitizer, and coupling agent will have a certain impact on the final composite material. It can be seen from Example 3 and Comparative Example 5 that if the surface-treated plant fiber is not irradiated with ultraviolet light, a good cross-linking reaction cannot be generated on the surface of the plant fiber, thereby enhancing the surface modification effect of the plant fiber, which will also have a certain impact on the mechanical properties of the final composite material.

[0106] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0107] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.

Claims

1. A plant fiber reinforced polypropylene composite material, characterized in that: The invention comprises the following raw materials in parts by weight: 44.5 to 91 parts of polypropylene, 5 to 40 parts of modified plant fiber, 0 to 10 parts of toughening agent, 1 to 5 parts of compatibilizer, and 0.5 to 3 parts of processing aid; The modified plant fiber is prepared by surface modification of the plant fiber using tetrafluoroborate ionic liquid, a cross-linking sensitizer and a coupling agent.

2. The plant fiber reinforced polypropylene composite material according to claim 1, characterized in that: The polypropylene is one or more of homopolymer polypropylene, propylene-ethylene block copolymer, propylene-ethylene random copolymer and propylene-1-butene random block.

3. The plant fiber reinforced polypropylene composite material according to claim 1, characterized in that: The compatibilizer is at least one of PP, POE, SEBS, and SEPS grafted maleic anhydride; The toughening agent is at least one of POE, LLDPE, HDPE and SEBS; The processing aid is at least one of an antioxidant, a weathering agent, a lubricant, and a toner.

4. The plant fiber reinforced polypropylene composite material according to claim 1, characterized in that: The modified plant fiber preparation process comprises: Step 1: prepare a modifier dilution solution by mixing tetrafluoroborate ionic liquid, a cross-linking sensitizer, a coupling agent and a diluent; Step 2: soaking and stirring the plant fiber with the modifier dilution; Step 3: Take out the impregnated plant fiber, dry it, and expose it to ultraviolet light to obtain surface-modified plant fiber.

5. The plant fiber reinforced polypropylene composite material according to claim 4, characterized in that: In the step 1, the mass ratio of tetrafluoroborate ionic liquid, cross-linking sensitizer, coupling agent and diluent is (5-40): (1-5): (1-5): (50-93); In the step 2, the mass ratio of the plant fiber to the modifier dilution is 1:

3.

6. The plant fiber reinforced polypropylene composite material according to claim 1 or 4, characterized in that: The tetrafluoroborate ionic liquid is at least one of tetrafluoroborate ionic liquids containing vinyl imidazole, acryl imidazole, acrylonitrile imidazole, styryl imidazole, and epoxy imidazole; The cross-linking sensitizer is one or more of trimethallyl isocyanate, triallyl isocyanurate, and tris(2-hydroxyethyl)isocyanurate triacrylate, which have high boiling point and low volatility. The coupling agent is at least one of a silane coupling agent, a titanate coupling agent, and an aluminate coupling agent.

7. The plant fiber reinforced polypropylene composite material according to claim 4, characterized in that: The diluent is at least one of water, methanol, ethanol, propanol, butanone and toluene.

8. A method for preparing a plant fiber reinforced polypropylene composite material, characterized in that: The following steps are involved: S1, preparing a modifier diluent by mixing tetrafluoroborate ionic liquid, a cross-linking sensitizer, a coupling agent, and a diluent in a mass ratio of (5-40):(1-5):(1-5):(50-93); impregnating plant fiber with the modifier diluent in a mass ratio of 1:3 and stirring; taking out the impregnated plant fiber, drying it, and irradiating it under ultraviolet light to obtain a surface-modified plant fiber; S2, premixing polypropylene, toughening agent, compatibilizer and processing aid in a high-speed mixer to obtain a premix; S3, placing the premix at the main material feeding port of the twin-screw extruder and adding the modified plant fiber from the side feeding port, melting and plasticizing in the twin-screw extruder and extruding into granules.

9. The method for preparing a plant fiber reinforced polypropylene composite material according to claim 8, characterized in that: The temperatures of zones 1 to 10 of the twin-screw extruder are 160°C, 210°C, 210°C, 210°C, 200°C, 200°C, 200°C, 200°C, 210°C respectively; the side feeding port of the twin-screw extruder is located in zone 6.

10. Use of the plant fiber reinforced polypropylene composite material according to any one of claims 1 to 7 in the preparation of automobile parts.