Flame-retardant impact-resistant PVC (polyvinyl chloride) cable sheath material

By using combined materials such as gel-type PVC resin and ultrafine composite filler in PVC cable sheath, the limitations of flame retardancy and strength performance in the prior art are solved, and higher flame retardancy and strength performance are achieved. Improves the overall performance and environmental protection of the material.

CN118994816APending Publication Date: 2024-11-22ANHUI SIHUI CABLE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411279842.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The flame retardant and strength properties of existing PVC cable sheaths have limitations. Excessive addition of flame retardant will affect the mechanical properties of PVC resin, making it difficult to improve flame retardant and strength at the same time.

Method used

Using gel-type PVC resin, ultra-fine composite filler and phosphorus-based flame retardant, it forms a powerful cohesion and adhesion electrostatic effect through components such as polyethyleneimine, acrylic acid and polyvinylpyrrolidone to enhance the flame retardant of PVC resin. Performance and mechanical properties, and improve the compatibility and flame retardant properties of materials through materials such as magnesium, diceite and polar adenosine triphosphate.

Benefits of technology

It significantly improves the flame retardant and strength properties of PVC cable sheath material, enhances its wear resistance and tensile strength, and improves the uniformity and environmental protection of the material.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a flame-retardant impact-resistant PVC (polyvinyl chloride) cable sheath material, which relates to the technical field of cables and comprises the following raw materials in parts by weight: 80 parts of gel type PVC resin, 20-25 parts of plasticizer, 3-6 parts of stabilizer, 2-6 parts of superfine composite filler, 8-10 parts of flame retardant, 2-5 parts of stearic acid and 2-5 parts of calcium carbonate. The preparation method of the gel type PVC resin comprises the following steps: uniformly dispersing polyethyleneimine and acrylic acid in deionized water to obtain a solution A; uniformly dispersing polyvinylpyrrolidone and acrylic acid in deionized water to obtain a solution B, and uniformly mixing the solution A and the solution B to obtain gel slurry; adding PVC (polyvinyl chloride) resin into the gel slurry, and uniformly mixing under UV (ultraviolet) irradiation to obtain gel type PVC resin; the flame-retardant impact-resistant PVC cable sheath material disclosed by the invention has good flame retardance, strength performance and wear resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cables, and in particular to a flame-retardant and impact-resistant PVC cable sheath material. Background Art

[0002] Cable sheath material is an important component of the outer layer of the cable. Its main function is to protect the internal control structure of the cable from damage by mechanical equipment and provide waterproof, flame retardant, fire resistant and corrosion resistant properties. There are many types of cable sheath materials, among which PVC cable sheath material is a common sheath material.

[0003] In the existing PVC cable sheath material, the main raw material is PVC resin, and flame retardants or other additives are added thereto to improve the flame retardancy and strength properties of the PVC cable sheath material. However, since excessive addition of flame retardants will inevitably affect the mechanical properties of PVC resin, the flame retardant often needs to be controlled within a certain range, so its flame retardancy will be subject to certain limitations. At the same time, the strength of the PVC cable sheath material determines the service life of the cable. Therefore, on the basis of improving the flame retardancy, its strength also needs to be further improved. Summary of the invention

[0004] The purpose of the present invention is to provide a flame retardant and impact resistant PVC cable sheath material to solve the following technical problems:

[0005] How to improve the flame retardancy and strength performance of PVC cable sheath materials

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] The invention discloses a flame retardant and impact resistant PVC cable sheath material, comprising the following raw materials in parts by weight: 80 parts of gel-type PVC resin, 20-25 parts of plasticizer, 3-6 parts of stabilizer, 2-6 parts of ultrafine composite filler, 8-10 parts of flame retardant, 2-5 parts of stearic acid, and 2-5 parts of calcium carbonate;

[0008] The preparation method of the flame-retardant and impact-resistant PVC cable sheath material is as follows: adding the above raw materials into a mixer, mixing at 120° C. for 30 minutes, and then transferring to an extruder for extrusion granulation to obtain the flame-retardant and impact-resistant PVC cable sheath material.

[0009] Further, the preparation method of the gel-type PVC resin is:

[0010] S11: uniformly dispersing polyethyleneimine and acrylic acid in deionized water to obtain a solution A; uniformly dispersing polyvinyl pyrrolidone and acrylic acid in deionized water to obtain a solution B; and uniformly mixing the solution A and the solution B to obtain a gel slurry;

[0011] S12: adding PVC resin to the gel slurry, and mixing them evenly under UV irradiation to allow the gel slurry and the PVC resin to fully react, thereby obtaining a gel-type PVC resin;

[0012] In the above preparation process, when the polyethyleneimine in solution A reacts with acrylic acid, the polyelectrolyte with opposite charges has a large amount of anions -COO - and cation -NH 3+ The groups can form strong cohesive and adhesive electrostatic effects. Therefore, when mixed with PVC resin, it can achieve strong adhesion with PVC resin, improve compatibility and bonding strength, and enhance the mechanical properties of PVC resin;

[0013] The polyvinyl pyrrolidone and acrylic acid in solution B can quickly absorb water molecules under wetting conditions to form hydrophilic gel aggregates. Therefore, after mixing with PVC resin, the friction coefficient and hydrophilicity of the PVC resin can be reduced, and a hydrogel layer can be formed on the surface of the PVC resin to enhance the flame retardant and wear resistance of the PVC resin.

[0014] Preferably, in step 1, the mass ratio of polyethyleneimine to acrylic acid in solution A is 1:(0.8-1.2);

[0015] Preferably, in step 1, the mass ratio of polyvinyl pyrrolidone to acrylic acid in solution B is 1:(1.8-2.2);

[0016] Preferably, in step 1, the mass ratio of the solute in solution A to that in solution B is 1:(1-2);

[0017] Preferably, in step 2, the mass ratio of the PVC resin to the solute in the gel slurry is 5:(1-2).

[0018] Furthermore, the preparation method of the ultrafine composite filler is:

[0019] S21: grinding brucite, dickite, and polar adenosine triphosphate disodium into nanometer-level powders respectively, and then putting them into a high-speed mixer together, and mixing them evenly at 30-40° C. to obtain a mixed material;

[0020] S22: dissolving chlorinated polyethylene in an aromatic hydrocarbon solvent to form a chlorinated polyethylene solution, adding the chlorinated polyethylene solution into the mixed material and stirring evenly to obtain a mixed slurry;

[0021] S23: Atomize the mixed slurry into tiny droplets, quickly dry them into particles in hot air above 150° C., and grind the particles to 4-10 μm to obtain ultrafine composite fillers.

[0022] In the above preparation process, brucite and dickite are combined with polar adenosine triphosphate. Chlorinated polyethylene and polar adenosine triphosphate contain saturated carbon chain structures, which can achieve good compatibility. At the same time, -C l in chlorinated polyethylene and -C l in PVC resin are both highly polar groups, which can enhance the interaction between the two and improve compatibility. Therefore, chlorinated polyethylene can serve as a bridge between polar adenosine triphosphate and PVC resin, so that brucite and dickite on polar adenosine triphosphate can be evenly dispersed in PVC resin, thereby improving the uniformity of the material.

[0023] At the same time, brucite and dickite not only have good flame retardant properties, but also have a certain hardness. Therefore, dispersing them into PVC resin can also improve the mechanical properties of PVC resin. Polar adenosine triphosphate contains phosphate molecules, which can have a flame retardant effect, and polar adenosine triphosphate, as a biomaterial, has better environmental protection.

[0024] Wherein, the mass ratio of brucite, dickite, polar disodium adenosine triphosphate and chlorinated polyethylene is 3:(1-2):(2-4):(2-3);

[0025] Preferably, the aromatic hydrocarbon solvent is toluene, xylene or styrene.

[0026] Further, the preparation method of polar adenosine triphosphate disodium is:

[0027] Prepare disodium adenosine triphosphate and γ-aminopropyltriethoxysilane in a mass ratio of 2:(1-2), dissolve disodium adenosine triphosphate in ethanol and perform ultrasonic dispersion to form a uniform suspension, slowly drop γ-aminopropyltriethoxysilane into the suspension and stir evenly, then react at 40-60°C for 8-10h, filter the reaction product, and vacuum dry to obtain polar disodium adenosine triphosphate.

[0028] In the above preparation process, adenosine disodium triphosphate reacts with γ-aminopropyltriethoxysilane, so that active groups and saturated carbon chain structures are introduced into the surface of adenosine disodium triphosphate, and its surface activity is greatly improved, which is conducive to a firm combination with brucite and dickite.

[0029] Preferably, the usage ratio of adenosine triphosphate disodium to ethanol is 1 g:(8-12) mL.

[0030] Furthermore, the plasticizer is a mixture of TOTM and soybean oil or a mixture of DOTP and DOP.

[0031] Furthermore, the stabilizer is a calcium-zinc composite heat stabilizer.

[0032] Furthermore, the flame retardant is a phosphorus-based flame retardant.

[0033] Beneficial effects of the present invention:

[0034] (1) The flame-retardant and impact-resistant PVC cable sheath material of the present invention contains a gel-type PVC resin, in which polyvinyl pyrrolidone and acrylic acid can rapidly absorb water molecules under wet conditions to form hydrophilic gel aggregates. Therefore, after mixing with the PVC resin, the friction coefficient and hydrophilicity of the PVC resin can be reduced, and a hydrogel layer can be formed on the surface of the PVC resin to enhance the flame retardant properties of the PVC resin.

[0035] (2) When polyethyleneimine and acrylic acid in gel-type PVC resin react, the oppositely charged polyelectrolyte has a large number of anions -COO - and cation -NH 3+ The groups can form strong cohesive and adhesive electrostatic effects, achieve strong adhesion with PVC resin, and improve the bonding strength, thereby stably fixing the hydrogel layer on the surface of PVC resin, thereby improving its wear resistance; at the same time, in the structure formed by polyethyleneimine and acrylic acid, their molecular chains are cross-linked to form a three-dimensional network structure, thereby further improving the strength.

[0036] (3) The flame-retardant and impact-resistant PVC cable sheath material of the present invention contains polar disodium adenosine triphosphate, wherein the disodium adenosine triphosphate reacts with γ-aminopropyltriethoxysilane, so that active groups and saturated carbon chain structures are introduced into the surface of the disodium adenosine triphosphate, and its surface activity is greatly improved, so it is conducive to a firm combination with brucite and dickite, and the compatibility with the PVC resin is greatly improved. On the one hand, the bonding strength between the materials is improved, and the tensile strength of the material is improved. On the other hand, the materials in the sheath material system are more evenly dispersed, which is conducive to improving the flame retardant performance. DETAILED DESCRIPTION

[0037] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] The experimental methods in the following examples, unless otherwise specified, are all conventional methods, and are performed according to the techniques or conditions described in the literature in the field or according to the product instructions. The materials, reagents, etc. used in the following examples, unless otherwise specified, can all be obtained from commercial channels.

[0039] Example 1

[0040] Preparation of polar adenosine triphosphate disodium:

[0041] Add 500 mL of ethanol to an ultrasonic disperser, then add 50 g of adenosine triphosphate disodium, ultrasonically disperse at 50 Hz for 1 hour to form a uniform suspension, transfer it to a stirring tank, then slowly drop γ-aminopropyltriethoxysilane into the suspension and stir evenly, adjust the temperature of the stirring tank to 50°C, stir at 300 rpm for 9 hours to allow it to react fully, use a funnel to filter the reaction product, place the filter material in a crucible, transfer the crucible to a vacuum drying oven, and dry it at 80°C for 6 hours to obtain polar adenosine triphosphate disodium.

[0042] Example 2

[0043] Preparation of ultrafine composite fillers:

[0044] 30 g of brucite, 15 g of dickite, and 30 g of polar adenosine triphosphate disodium prepared in Example 1 were ground into powders with a particle size of 30-50 nm using a planetary ball mill, and then put into a high-speed mixer together, stirred at 300 rpm for 20 min at 35 ° C, and then 300 mL of toluene was added thereto, and stirring was continued at 300 rpm for 40 min to obtain a mixed slurry, and the mixed slurry was added to a spray granulator, atomized into tiny droplets, and then quickly dried into particles in hot air at 180 ° C, and the particles were added to a planetary grinder and ground to 4-10 um to obtain an ultrafine composite filler.

[0045] Comparative Example 1

[0046] Preparation of ultrafine composite fillers:

[0047] Compared with Example 2, the only difference is that the polar disodium adenosine triphosphate prepared in Example 1 is replaced by disodium adenosine triphosphate, and other conditions are exactly the same, and finally an ultrafine composite filler is obtained.

[0048] Example 3

[0049] Preparation of gel-type PVC resin:

[0050] Add 15 g of polyethyleneimine and 15 g of acrylic acid to beaker 1, then add 100 mL of deionized water, and stir well to obtain solution A; add 15 g of polyvinyl pyrrolidone and 30 g of acrylic acid to beaker 2, then add 100 mL of deionized water, and stir well to obtain solution B. Add solution A and solution B to a stirring tank, mix at 300 rpm for 30 min to obtain a gel slurry, add 250 g of PVC resin to the gel slurry, set a UV lamp (200200-F, λ=365 nm) above the stirring tank, and stir at 500 rpm for 25 min to obtain a gel-type PVC resin.

[0051] Comparative Example 2

[0052] Preparation of gel-type PVC resin:

[0053] Add 10 g of polyethyleneimine and 10 g of acrylic acid into a beaker, then add 100 mL of deionized water, stir well to obtain solution A, transfer solution A into a stirring tank, add 67 g of PVC resin into the stirring tank, set a UV lamp (200200-F, λ=365 nm) above the stirring tank, stir at 500 rpm for 25 min to obtain a gel-type PVC resin.

[0054] Comparative Example 3

[0055] Preparation of gel-type PVC resin:

[0056] Add 10 g of polyvinyl pyrrolidone and 20 g of acrylic acid into a beaker, then add 100 mL of deionized water, stir well to obtain solution B, transfer solution B into a stirring tank, add 100 g of PVC resin into the stirring tank, set a UV lamp (200200-F, λ=365 nm) above the stirring tank, stir at 500 rpm for 25 min to obtain a gel-type PVC resin.

[0057] Example 4

[0058] Preparation of flame retardant and impact resistant PVC cable sheath material:

[0059] 80 g of the gel-type PVC resin prepared in Example 3, 16 g of DOTP, 4 g of DOP, 3 g of a calcium-zinc composite heat stabilizer (STA-505T), 2 g of the ultrafine composite filler prepared in Example 2, 8 g of a phosphate flame retardant (Fyro l 38), 2 g of stearic acid, and 2 g of calcium carbonate were added to a mixer, mixed at 120° C. for 30 min, and then transferred to a small granulator for extrusion granulation at 200° C. to obtain the flame-retardant and impact-resistant PVC cable sheath material of the present invention.

[0060] Example 5

[0061] Preparation of flame retardant and impact resistant PVC cable sheath material:

[0062] 80 g of the gel-type PVC resin prepared in Example 3, 18 g of DOTP, 5 g of DOP, 4 g of a calcium-zinc composite heat stabilizer (STA-505T), 4 g of the ultrafine composite filler prepared in Example 2, 9 g of a phosphate flame retardant (Fyro l 38), 3 g of stearic acid, and 3 g of calcium carbonate were added to a mixer, mixed at 120° C. for 35 min, and then transferred to a small granulator for extrusion granulation at 200° C. to obtain the flame-retardant and impact-resistant PVC cable sheath material of the present invention.

[0063] Example 6

[0064] Preparation of flame retardant and impact resistant PVC cable sheath material:

[0065] 80 g of the gel-type PVC resin prepared in Example 3, 20 g of DOTP, 5 g of DOP, 6 g of a calcium-zinc composite heat stabilizer (STA-505T), 6 g of the ultrafine composite filler prepared in Example 2, 10 g of a phosphate flame retardant (Fyro l 38), 5 g of stearic acid, and 5 g of calcium carbonate were added to a mixer, mixed at 120° C. for 40 min, and then transferred to a small granulator for extrusion granulation at 200° C. to obtain the flame-retardant and impact-resistant PVC cable sheath material of the present invention.

[0066] Comparative Example 4

[0067] Compared with Example 5, the only difference is that the gel-type PVC resin prepared in Example 3 is replaced by the gel-type PVC resin prepared in Comparative Example 2, and other conditions are exactly the same, and finally a PVC cable sheath material is prepared.

[0068] Comparative Example 5

[0069] Compared with Example 5, the only difference is that the gel-type PVC resin prepared in Example 3 is replaced by the gel-type PVC resin prepared in Comparative Example 3, and other conditions are exactly the same, and finally a PVC cable sheath material is prepared.

[0070] Comparative Example 6

[0071] Compared with Example 5, the only difference is that the ultrafine composite filler prepared in Example 2 is replaced by the ultrafine composite filler prepared in Comparative Example 1, and other conditions are exactly the same, and finally a PVC cable sheath material is prepared.

[0072] The performance tests were conducted on the PVC cable sheath materials obtained in Examples 4-6 and Comparative Examples 4-6. The test items and methods are as follows:

[0073] Limiting oxygen index (LOI) test: GB / T 2406.1—2008

[0074] Vertical burning (UL-94 grade) test: GB / T 2408—2008

[0075] Tensile strength test: GB / T 1040.3—2006

[0076] Wear resistance test (wear rate): GB / T 1689-2014

[0077] The test results are listed in Table 1. Table 1 is as follows:

[0078] Table 1

[0079] LOI / 100% UL-94 Rating Wear rate / 100% Tensile strength / MPa Example 4 30.6 V-0 0.11 40.2 Example 5 31.2 V-0 0.05 42.1 Example 6 30.1 V-0 0.09 41.3 Comparative Example 4 26.5 V-2 2.25 36.5 Comparative Example 5 24.2 V-1 1.95 36.9 Comparative Example 6 25.1 V-1 2.65 35.8

[0080] By analyzing the data in Table 1, it can be seen that the PVC cable sheath material prepared in Examples 4-6 has stronger flame retardancy and strength properties than that in Comparative Examples 4-6.

[0081] Specifically, compared with Comparative Example 4, the gel-type PVC resin used in Examples 4-6 contains solution B, which indicates that the addition of polyvinyl pyrrolidone and acrylic acid can improve the flame retardant properties and strength properties of the sheath material; compared with Comparative Example 5, the gel-type PVC resin used in Examples 4-6 contains solution A, which indicates that the addition of polyethyleneimine and acrylic acid can improve the flame retardant properties and strength properties of the sheath material; compared with Comparative Example 6, the disodium adenosine triphosphate in the ultrafine composite filler used in Examples 4-6 has been modified with γ-aminopropyltriethoxysilane, which indicates that the addition of polar disodium adenosine triphosphate can improve the flame retardant properties and strength properties of the sheath material.

[0082] The above is a detailed description of an embodiment of the present invention, but the content is only a preferred embodiment of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.

Claims

1. A flame retardant and impact resistant PVC cable sheath material, characterized in that: The raw materials include the following parts by weight: 80 parts of gel-type PVC resin, 20-25 parts of plasticizer, 3-6 parts of stabilizer, 2-6 parts of ultrafine composite filler, 8-10 parts of flame retardant, 2-5 parts of stearic acid, and 2-5 parts of calcium carbonate; Wherein, the preparation method of gel type PVC resin is: Step 1: uniformly dispersing polyethyleneimine and acrylic acid in deionized water to obtain solution A; uniformly dispersing polyvinyl pyrrolidone and acrylic acid in deionized water to obtain solution B; and uniformly mixing solution A and solution B to obtain a gel slurry; Step 2: Add PVC resin into the gel slurry and mix them evenly under UV irradiation to obtain gel-type PVC resin.

2. The flame retardant and impact resistant PVC cable sheath material according to claim 1, characterized in that: In step 1, the mass ratio of polyethyleneimine to acrylic acid in solution A is 1:(0.8-1.2); the mass ratio of polyvinyl pyrrolidone to acrylic acid in solution B is 1:(1.8-2.2); the mass ratio of solutes in solution A to solution B is 1:(1-2); in step 2, the mass ratio of PVC resin to solutes in gel slurry is 5:(1-2).

3. The flame retardant and impact resistant PVC cable sheath material according to claim 1, characterized in that: The ultrafine composite filler includes brucite, dickite, polar disodium adenosine triphosphate and chlorinated polyethylene in a mass ratio of 3:(1-2):(2-4):(2-3).

4. The flame retardant and impact resistant PVC cable sheath material according to claim 3, characterized in that: The preparation method of polar adenosine triphosphate disodium is as follows: Prepare disodium adenosine triphosphate and γ-aminopropyltriethoxysilane in a mass ratio of 2:(1-2), dissolve disodium adenosine triphosphate in ethanol and perform ultrasonic dispersion to form a uniform suspension, slowly drop γ-aminopropyltriethoxysilane into the suspension and stir evenly, then react at 40-60°C for 8-10h, filter the reaction product, and vacuum dry to obtain polar disodium adenosine triphosphate.

5. The flame retardant and impact resistant PVC cable sheath material according to claim 4, characterized in that: The dosage ratio of the adenosine triphosphate disodium to the ethanol is 1 g:(8-12) mL.

6. The flame retardant and impact resistant PVC cable sheath material according to claim 4, characterized in that: The preparation method of ultrafine composite filler is: Step 1: Grind brucite, dickite and polar adenosine triphosphate disodium into nanometer-level powders respectively, put them into a high-speed mixer together, mix them evenly at 30-40° C. to obtain a mixed material; Step 2: dissolving chlorinated polyethylene in an aromatic hydrocarbon solvent to form a chlorinated polyethylene solution, adding the chlorinated polyethylene solution into the mixed material and stirring evenly to obtain a mixed slurry; Step 3: Atomize the mixed slurry into tiny droplets, quickly dry them into particles in hot air above 150°C, and grind the particles to 4-10um to obtain ultrafine composite fillers.

7. The flame retardant and impact resistant PVC cable sheath material according to claim 6, characterized in that: The aromatic hydrocarbon solvent is toluene, xylene or styrene.

8. The flame retardant and impact resistant PVC cable sheath material according to claim 1, characterized in that: The plasticizer is a mixture of trioctyl trimellitate and soybean oil or a mixture of dioctyl terephthalate and dioctyl phthalate.

9. The flame retardant and impact resistant PVC cable sheath material according to claim 1, characterized in that: The stabilizer is a calcium-zinc composite heat stabilizer.

10. The flame retardant and impact resistant PVC cable sheath material according to claim 1, characterized in that: The flame retardant is a phosphorus-based flame retardant.