Anti-corrosion coating with high weather resistance and preparation method of anti-corrosion coating
By combining waterborne fluorocarbon resin emulsion and waterborne polyurethane emulsion, along with modified materials, the problems of insufficient weather resistance, corrosion resistance and adhesion stability of anti-corrosion coatings have been solved, resulting in a coating with high adhesion stability and excellent anti-corrosion effect, suitable for ships, bridges and other fields.
Patent Information
- Application Number
- CN202411264688.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-22
AI Technical Summary
Existing anti-corrosion coatings are insufficient in terms of weather resistance, corrosion resistance and adhesion stability, especially in applications such as ships and bridges, where they are difficult to resist corrosion from ultraviolet rays and seawater for extended periods.
By combining waterborne fluorocarbon resin emulsion and waterborne polyurethane emulsion, along with materials such as modified hydroxyapatite ultralong nanowires, triethyl citrate modified silica whiskers, polyethylene glycol modified alumina fibers, and silicone modified graphene, the coating's weather resistance, corrosion resistance, and adhesion stability are improved through crosslinking and plasticizing effects.
It achieves high adhesion stability, excellent anti-corrosion effect and weather resistance of coatings on ship steel plates, extends service life, improves the strength and flexibility of film layer, and resists the erosion of ultraviolet rays and seawater.
Smart Images

Figure BDA0005036795600000091
Abstract
Description
Technical Field
[0001] The present invention relates to the field of coatings, and more specifically, to an anticorrosive coating with strong weather resistance and a preparation method thereof. Background Art
[0002] Anti-corrosion coatings are special coatings generally used to protect metals, wood and other materials from corrosion. They are widely used in aviation, shipping, chemical industry, oil pipelines, steel structures, bridges, oil drilling platforms and other fields.
[0003] The anti-corrosion coatings used on the bottom plates of ships and the steel structures of bridges need to have strong anti-corrosion properties and high weather resistance, be able to resist ultraviolet corrosion for a long time, and have a long service life in seawater.
[0004] Commonly used coatings include acrylic resin coatings, fluorocarbon resin coatings, epoxy resin coatings, etc. Although acrylic resin coatings have good adhesion and easy construction, the weather resistance of the film formed by acrylic resin coatings is worse than that of the film formed by fluorocarbon resin coatings, and the corrosion resistance is also worse than that of the film formed by fluorocarbon resin coatings. Fluorocarbon resin coatings have worse adhesion on the substrate surface than acrylic resin coatings. Although epoxy resin coatings have good adhesion on the substrate surface, they have poor weather resistance and are easily affected by harsh environments such as ultraviolet rays, high temperature and low temperature, resulting in aging, fading, cracking and other problems.
[0005] Therefore, how to prepare a new anti-corrosion coating that has the advantages of strong weather resistance, good corrosion resistance and high adhesion stability is a problem to be solved. Summary of the invention
[0006] In order to prepare a new anti-corrosion coating that has the advantages of strong weather resistance, good corrosion resistance and high adhesion stability, the present application provides an anti-corrosion coating with strong weather resistance and a preparation method thereof.
[0007] In the first aspect, the present application provides an anti-corrosion coating with strong weather resistance, which adopts the following technical solution: A weather-resistant anticorrosive coating comprises the following raw materials in parts by weight: 80-100 parts of aqueous fluorocarbon resin emulsion, 20-30 parts of aqueous polyurethane emulsion, 5-10 parts of plasticizer, 10-20 parts of water, 10-20 parts of filler, 1-3 parts of defoamer, 1-3 parts of thickener, 0.5-2 parts of dispersant, 15-20 parts of curing agent, 1-2 parts of leveling agent and 1-3 parts of modified hydroxyapatite ultra-long nanowires.
[0008] By adopting the above technical scheme, the water-based fluorocarbon resin emulsion, the water-based polyurethane emulsion and the plasticizer are matched, and the good weather resistance and corrosion resistance of the water-based fluorocarbon resin emulsion are utilized to make the coating have the advantages of excellent anti-corrosion effect and strong weather resistance; the filler and the modified hydroxyapatite ultra-long nanowires are matched to play a filling and supporting effect inside the coating, and the modified hydroxyapatite ultra-long nanowires can connect the water-based fluorocarbon resin emulsion and the water-based polyurethane emulsion, thereby further improving the strength, anti-corrosion effect and weather resistance of the coating after film formation; the thickener and the water-based polyurethane emulsion can make the coating stably bonded to the ship steel plate substrate, and improve the adhesion stability of the coating on the steel plate; the dispersant, defoamer and leveling agent are matched to further improve the stability and strength of the film layer formed by the coating, extend the service life, and further improve the weather resistance, corrosion resistance and adhesion stability.
[0009] Preferably, the filler is composed of triethyl citrate modified silica whiskers, polyethylene glycol modified alumina fibers, and silicone modified graphene in a mass ratio of 1:1-2:0.5-2.
[0010] By adopting the above technical scheme, triethyl citrate modified silica whiskers, polyethylene glycol modified alumina fibers, and silicone modified graphene are matched, and the carboxyl group of triethyl citrate and the hydroxyl group of polyethylene glycol are utilized to facilitate crosslinking with aqueous fluorocarbon resin emulsions and aqueous polyurethane emulsions. The plasticizing effects of triethyl citrate and polyethylene glycol are combined to stably bond the silica whiskers and alumina fibers with the aqueous fluorocarbon resin emulsions and aqueous polyurethane emulsions in the coating, thereby improving the density of the film layer formed by the coating. The high strength of the silica whiskers and graphene is combined to improve the strength and wear resistance of the coating. The flexibility and large specific surface area of the alumina fibers and the single-layer flaky structure of the graphene are combined to enable the absorption of substances such as aqueous polyurethane emulsions, thereby further improving the flexibility of the film layer, thereby improving the weather resistance and corrosion resistance of the coating.
[0011] The hydrophobic base of triethyl citrate combined with the hydrophobic effect of silicone can further improve the hydrophobicity of the coating, while silica whiskers, alumina fibers and graphene serve as supporting structures to improve the structural density of the film layer formed by the coating, thereby further blocking moisture and enabling the film layer formed by the coating on the ship's steel plate to resist the erosion of seawater for a long time.
[0012] Preferably, the triethyl citrate modified silica whisker is prepared from triethyl citrate, sodium carboxymethyl cellulose solution and silica whisker in a mass ratio of 1:0.2-0.4:2-4.
[0013] By adopting the above technical scheme, triethyl citrate, sodium carboxymethyl cellulose solution and silica whiskers are matched, and the viscosity of the sodium carboxymethyl cellulose solution is utilized to facilitate the adhesion of triethyl citrate to the surface of the silica whiskers. The triethyl citrate on the surface of the silica whiskers has a good cross-linking effect with the water-based fluorocarbon resin coating and the water-based polyurethane coating, so as to improve the corrosion resistance and wear resistance of the finished coating, and have a longer service life on ships.
[0014] Preferably, the average length of the silica whiskers is 10-100 μm.
[0015] By adopting the above technical solution, the average length of the silica whiskers is limited, ensuring that the silica whiskers are evenly dispersed in the film layer formed by the anti-corrosion coating, thereby improving the strength, wear resistance and water impact resistance of the film layer.
[0016] Preferably, the polyethylene glycol-modified alumina fiber is prepared from a polyethylene glycol aqueous solution and alumina fiber in a mass ratio of 1:1-3.
[0017] By adopting the above technical scheme, the polyethylene glycol aqueous solution adheres to the surface of the alumina fiber, giving the alumina fiber surface hydroxyl groups, which facilitates cross-linking and bonding with the aqueous fluorocarbon resin emulsion and the aqueous polyurethane emulsion, thereby improving the bonding stability and distribution uniformity of the alumina fiber in the coating, thereby improving the strength, wear resistance and weather resistance of the film layer.
[0018] Preferably, the silicone-modified graphene is prepared by bonding graphene to a sodium carboxymethyl cellulose solution and then to a camphor extract, and finally loading the graphene with silicone glue, and the mass ratio of graphene, sodium carboxymethyl cellulose solution, camphor extract and silicone glue is 1:0.1-0.2:0.1-0.2:0.2-0.5.
[0019] By adopting the above technical scheme and utilizing the bonding effect of silicone adhesive, it is convenient to seal the camphor extract on the surface of graphene, and utilize the good smell of camphor extract to repel marine organisms, thereby reducing the contact between fish and the bottom steel plate of the ship. The film layer formed by silicone adhesive has a certain air permeability and a good hydrophobic effect, which can block the erosion of ocean water. Combined with the good wear resistance and impact resistance of graphene, the wear resistance, weather resistance and strength of the coating are further improved.
[0020] Preferably, the modified hydroxyapatite ultra-long nanowires are prepared from a polyvinyl alcohol solution and hydroxyapatite ultra-long nanowires in a mass ratio of 1:1-2.
[0021] By adopting the above technical scheme, the polyvinyl alcohol solution and the hydroxyapatite ultra-long nanowires are matched, and the viscosity of the polyvinyl alcohol solution is utilized to facilitate bonding to the surface of the hydroxyapatite ultra-long nanowires, and the hydroxyl groups of the polyvinyl alcohol are utilized to facilitate bonding with the aqueous fluorocarbon resin emulsion and the aqueous polyurethane emulsion, thereby improving the distribution uniformity and bonding stability of the hydroxyapatite ultra-long nanowires in the coating. The hydroxyapatite ultra-long nanowires utilize their large specific surface area to connect the aqueous fluorocarbon resin emulsion and the aqueous polyurethane emulsion, further improving the stability of the film layer formed by the coating, and combined with the flexibility of the hydroxyapatite ultra-long nanowires, the impact resistance and corrosion resistance of the film layer are improved.
[0022] Preferably, the plasticizer consists of methyl phthalate and chlorinated paraffin in a mass ratio of 1:0.1-0.4.
[0023] By adopting the above technical scheme, methyl phthalate and chlorinated paraffin are combined to improve the low-temperature resistance, flexibility and corrosion resistance of the coating, and the coating has good weather resistance and is not prone to cracking, blistering and other problems due to ultraviolet rays and seawater impact, thereby ensuring the weather resistance and wear resistance of the coating.
[0024] Preferably, the thickener is hydroxyethyl cellulose.
[0025] By adopting the above technical scheme, the better solubility of hydroxyethyl cellulose in water-based paint can be utilized to improve the viscosity of the paint, and combined with the amino group in the water-based polyurethane emulsion, the adhesion of the paint on the steel plate surface can be further improved, and the adhesion stability of the coating formed by the paint can be improved.
[0026] In a second aspect, the present application provides a method for preparing a weather-resistant anticorrosive coating, which adopts the following technical solution: A method for preparing a weather-resistant anticorrosive coating comprises the following steps: S1. Weigh the water-based fluorocarbon resin emulsion, the water-based polyurethane coating, and water, mix and stir evenly to obtain a primary mixture; S2, adding filler and modified hydroxyapatite ultra-long nanowires to the primary mixture, mixing and stirring evenly, and then adding plasticizer, thickener, defoamer, dispersant, and leveling agent, mixing and stirring evenly to obtain a mixture; S3. Add curing agent to the mixture, mix well, and obtain finished coating.
[0027] By adopting the above technical solution, the prepared coating has the advantages of strong weather resistance, good corrosion resistance and high adhesion stability.
[0028] In summary, this application has the following beneficial effects: 1. The water-based fluorocarbon resin emulsion, water-based polyurethane emulsion and plasticizer are matched, and the good weather resistance and corrosion resistance of the water-based fluorocarbon resin emulsion are utilized to make the coating have excellent anti-corrosion effect and strong weather resistance; the filler and modified hydroxyapatite ultra-long nanowires are matched to play a filling and supporting effect inside the coating, and the modified hydroxyapatite ultra-long nanowires can connect the water-based fluorocarbon resin emulsion and the water-based polyurethane emulsion, thereby further improving the strength, anti-corrosion effect and weather resistance of the coating after film formation; the thickener and water-based polyurethane emulsion can make the coating stably bonded to the ship steel plate substrate, and improve the adhesion stability of the coating on the steel plate; the dispersant, defoamer and leveling agent are matched to further improve the stability and strength of the film layer formed by the coating, extend the service life, and further improve the weather resistance, corrosion resistance and adhesion stability.
[0029] 2. Before coating, the surface of the steel plate substrate of the ship is generally polished and degreased to expose the surface polar groups. The amino groups in the polyurethane emulsion, the carboxyl groups in the triethyl citrate on the surface of the silica whisker, the hydroxyl groups of the polyethylene glycol on the surface of the alumina fiber, and the hydroxyl groups of the polyvinyl alcohol on the surface of the modified hydroxyapatite ultra-long nanowires can attract and connect with the hydroxyl or carboxyl groups on the surface of the steel plate polar groups, further improving the adhesion stability of the coating on the steel plate surface, improving the disadvantage of the poor adhesion of the fluorocarbon resin emulsion on the steel plate surface, and making the coating have the advantage of high adhesion stability.
[0030] 3. Triethyl citrate modified silica whiskers, polyethylene glycol modified alumina fibers, and silicone modified graphene are combined. The carboxyl group of triethyl citrate and the hydroxyl group of polyethylene glycol are used to facilitate cross-linking with water-based fluorocarbon resin emulsions and water-based polyurethane emulsions. The plasticizing effect of triethyl citrate and polyethylene glycol makes the silica whiskers and alumina fibers stably bonded with the water-based fluorocarbon resin emulsions and water-based polyurethane emulsions in the coating, thereby improving the density of the film layer formed by the coating. The high strength of silica whiskers and graphene improves the strength and wear resistance of the coating. The flexibility and large specific surface area of alumina fibers and the single-layer flaky structure of graphene can absorb substances such as water-based polyurethane emulsions, further improving the flexibility of the film layer, thereby improving the weather resistance and corrosion resistance of the coating. DETAILED DESCRIPTION
[0031] The present application is further described in detail below in conjunction with embodiments.
[0032] Preparation Example of Triethyl Citrate Modified Silica Whiskers The following raw materials are all commercially available.
[0033] Preparation Example 1: Triethyl citrate modified silica whiskers were prepared by the following method: 1 kg of triethyl citrate and 0.3 kg of sodium carboxymethyl cellulose solution were weighed, mixed and stirred evenly, then sprayed evenly on the surface of 3 kg of silicon dioxide whiskers, dried and dispersed until the silicon dioxide whiskers did not stick to each other and agglomerated, to obtain a finished product; the sodium carboxymethyl cellulose solution was a sodium carboxymethyl cellulose aqueous solution with a mass fraction of 1%, and the average length of the silicon dioxide whiskers was 40 μm and the average diameter was 10 nm.
[0034] Preparation Example 2: This preparation example differs from Preparation Example 1 in that: Weigh 1 kg of triethyl citrate and 0.2 kg of sodium carboxymethyl cellulose solution, mix and stir evenly, then spray evenly on the surface of 2 kg of silicon dioxide whiskers, dry and disperse until the silicon dioxide whiskers do not stick to each other and agglomerate to obtain a finished product; the average length of the silicon dioxide whiskers is 10 μm and the average diameter is 10 nm.
[0035] Preparation Example 3: This preparation example differs from Preparation Example 1 in that: 1 kg of triethyl citrate and 0.4 kg of sodium carboxymethyl cellulose solution were weighed and mixed and stirred evenly, and then sprayed evenly on the surface of 4 kg of silica whiskers, and dried and dispersed until the silica whiskers did not stick to each other and agglomerated to obtain a finished product; the average length of the silica whiskers was 100 μm and the average diameter was 20 nm.
[0036] Preparation example of polyethylene glycol modified alumina fiber Preparation Example 4: Polyethylene glycol-modified alumina fiber is prepared by the following method: Put polyethylene glycol in water and stir until it is completely dissolved to obtain a polyethylene glycol aqueous solution with a mass fraction of 10%; the polyethylene glycol is polyethylene glycol 8000; 1 kg of polyethylene glycol aqueous solution was uniformly sprayed onto the surface of 2 kg of alumina fibers, and the finished product was obtained after drying and dispersion until the alumina fibers were not adhered to each other and agglomerated; the average length of the alumina fibers was 40 μm and the average diameter was 10 nm.
[0037] Preparation Example 5: This preparation example differs from Preparation Example 4 in that: 1 kg of polyethylene glycol aqueous solution is uniformly sprayed onto the surface of 1 kg of alumina fibers, and the alumina fibers are dried and dispersed until they are no longer adhered to each other and agglomerated to obtain a finished product.
[0038] Preparation Example 6: This preparation example differs from Preparation Example 4 in that: 1 kg of polyethylene glycol aqueous solution was evenly sprayed onto the surface of 3 kg of alumina fibers, and the finished product was obtained after drying and dispersion until the alumina fibers were no longer adhered to each other and agglomerated.
[0039] Preparation example of silicone-modified graphene Among the following raw materials, camphor extract was purchased from Lanzhou Waterless Biotechnology Co., Ltd., 100 mesh; silicone glue was purchased from Shanghai Xiongmai Construction Technology Co., Ltd.; other raw materials and equipment were all commercially available.
[0040] Preparation Example 7: Silicone-modified graphene was prepared by the following method: 0.15 kg of sodium carboxymethyl cellulose solution is evenly sprayed on the surface of 1 kg of graphene, and then 0.15 kg of camphor extract is added, and the addition rate of the camphor extract is 120 g / min. During the addition process, the graphene is continuously stirred at a rotation speed of 120 r / min, and is dried and dispersed until the graphenes do not stick to each other and agglomerate. Then 0.35 kg of silicone glue is evenly sprayed on the surface, and is dried and dispersed until the graphenes do not stick to each other and agglomerate to obtain a finished product; the sodium carboxymethyl cellulose solution is a sodium carboxymethyl cellulose aqueous solution with a mass fraction of 1%.
[0041] Preparation Example 8: This preparation example differs from Preparation Example 7 in that: 0.1 kg of sodium carboxymethyl cellulose solution is evenly sprayed on the surface of 1 kg of graphene, and then 0.1 kg of camphor extract is added, and the addition rate of the camphor extract is 120 g / min. During the adding process, the graphene is continuously stirred at a speed of 120 r / min. After drying and dispersion until the graphenes do not stick to each other and agglomerate, 0.2 kg of silicone glue is evenly sprayed on the surface, and after drying and dispersion until the graphenes do not stick to each other and agglomerate, a finished product is obtained.
[0042] Preparation Example 9: This preparation example differs from Preparation Example 7 in that: 0.2 kg of sodium carboxymethyl cellulose solution is evenly sprayed on the surface of 1 kg of graphene, and then 0.2 kg of camphor extract is added, and the addition rate of the camphor extract is 120 g / min. During the adding process, the graphene is continuously stirred at a speed of 120 r / min. After drying and dispersion until the graphenes do not stick to each other and agglomerate, 0.5 kg of silicone glue is evenly sprayed on the surface, and after drying and dispersion until the graphenes do not stick to each other and agglomerate, a finished product is obtained.
[0043] Preparation example of modified hydroxyapatite ultra-long nanowires Among the following raw materials, the hydroxyapatite ultra-long nanowires were purchased from Suzhou Kaifa New Material Technology Co., Ltd.; other raw materials and equipment were commercially available.
[0044] Preparation Example 10: Modified hydroxyapatite ultra-long nanowires are prepared by the following method: 1 kg of polyvinyl alcohol solution was weighed and sprayed evenly on 1.5 kg of hydroxyapatite ultra-long nanowires, and the product was obtained by drying and dispersing until the hydroxyapatite ultra-long nanowires did not stick to each other and agglomerate; the polyvinyl alcohol solution was a polyvinyl alcohol aqueous solution with a mass fraction of 1%, and the average length of the hydroxyapatite ultra-long nanowires was 100 μm and the average diameter was 10 nm.
[0045] Preparation Example 11: This preparation example differs from Preparation Example 10 in that: 1 kg of polyvinyl alcohol solution was weighed and sprayed evenly on 1 kg of hydroxyapatite ultra-long nanowires, and the solution was dried and dispersed until the hydroxyapatite ultra-long nanowires did not stick to each other and agglomerated, thereby obtaining a finished product.
[0046] Preparation Example 12: This preparation example differs from Preparation Example 10 in that: 1 kg of polyvinyl alcohol solution was weighed and sprayed evenly on 2 kg of hydroxyapatite ultra-long nanowires, and the solution was dried and dispersed until the hydroxyapatite ultra-long nanowires did not stick to each other and agglomerated, thereby obtaining a finished product. Example
[0047] Among the following raw materials, the water-based fluorocarbon resin emulsion was purchased from Qiyuan (Guangdong) Pharmaceutical Chemical Co., Ltd.; the water-based polyurethane emulsion was purchased from Shandong Aokai Waterproof Material Co., Ltd., model 823; the leveling agent was purchased from Germany Digo TEG4100 from Guangzhou Haoliangda International Trade Co., Ltd.; other raw materials are all commonly available on the market.
[0048] Example 1: A weather-resistant anticorrosive coating: 90kg of aqueous fluorocarbon resin emulsion, 25kg of aqueous polyurethane emulsion, 8kg of plasticizer, 15kg of water, 15kg of filler, 2kg of defoamer, 2kg of thickener, 1kg of dispersant, 18kg of curing agent, 1.5kg of leveling agent, and 2kg of modified hydroxyapatite ultra-long nanowires; the plasticizer is composed of methyl phthalate and chlorinated paraffin in a mass ratio of 1:0.2; the filler is composed of citric acid glyceride modified silica whiskers prepared in Preparation Example 1, polyethylene glycol modified alumina fibers prepared in Preparation Example 4, and silicone modified graphene prepared in Preparation Example 7 in a mass ratio of 1:1:1; the defoamer is an organosilicon defoamer; the thickener is hydroxyethyl cellulose; the dispersant is sodium polyacrylate; the curing agent is hexamethylene diisocyanate; the modified hydroxyapatite ultra-long nanowires are the modified hydroxyapatite ultra-long nanowires prepared in Preparation Example 10; The preparation method is as follows: S1. Weigh the water-based fluorocarbon resin emulsion, the water-based polyurethane coating, and water, mix and stir evenly to obtain a primary mixture; S2, adding filler and modified hydroxyapatite ultra-long nanowires to the primary mixture, mixing and stirring evenly, and then adding plasticizer, thickener, defoamer, dispersant, and leveling agent, mixing and stirring evenly to obtain a mixture; S3. Add curing agent to the mixture, mix well, and obtain finished coating.
[0049] Embodiment 2: This embodiment differs from Embodiment 1 in that: 80kg of aqueous fluorocarbon resin emulsion, 20kg of aqueous polyurethane emulsion, 5kg of plasticizer, 10kg of water, 10kg of filler, 1kg of defoamer, 1kg of thickener, 0.5kg of dispersant, 15kg of curing agent, 1kg of leveling agent, and 1kg of modified hydroxyapatite ultra-long nanowires; the plasticizer consists of methyl phthalate and chlorinated paraffin in a mass ratio of 1:0.1; the filler consists of citric acid glyceride-modified silica whiskers prepared in Preparation Example 2, polyethylene glycol-modified alumina fibers prepared in Preparation Example 5, and silicone-modified graphene prepared in Preparation Example 8 in a mass ratio of 1:1:0.5; the defoamer is an organosilicon defoamer; the thickener is hydroxyethyl cellulose; the dispersant is sodium polyacrylate; the curing agent is hexamethylene diisocyanate; the modified hydroxyapatite ultra-long nanowires are the modified hydroxyapatite ultra-long nanowires prepared in Preparation Example 11.
[0050] Embodiment 3: This embodiment differs from Embodiment 1 in that: 100kg of aqueous fluorocarbon resin emulsion, 30kg of aqueous polyurethane emulsion, 10kg of plasticizer, 20kg of water, 20kg of filler, 3kg of defoamer, 3kg of thickener, 2kg of dispersant, 20kg of curing agent, 2kg of leveling agent, and 3kg of modified hydroxyapatite ultra-long nanowires; the plasticizer consists of methyl phthalate and chlorinated paraffin in a mass ratio of 1:0.4; the filler consists of citric acid glyceride-modified silica whiskers prepared in Preparation Example 3, polyethylene glycol-modified alumina fibers prepared in Preparation Example 6, and silicone-modified graphene prepared in Preparation Example 9 in a mass ratio of 1:2:2; the defoamer is an organosilicon defoamer; the thickener is hydroxyethyl cellulose; the dispersant is sodium polyacrylate; the curing agent is hexamethylene diisocyanate; the modified hydroxyapatite ultra-long nanowires are the modified hydroxyapatite ultra-long nanowires prepared in Preparation Example 12.
[0051] Embodiment 4: This embodiment differs from Embodiment 1 in that: The filler is silica whisker.
[0052] Embodiment 5: This embodiment differs from Embodiment 1 in that: In the filler, the triethyl citrate modified silica whiskers are replaced by the same mass of silica whiskers, the polyethylene glycol modified alumina fibers are replaced by the same mass of alumina fibers, and the silicone modified graphene is replaced by the same mass of graphene.
[0053] Comparative Example Comparative Example 1: The difference between this comparative example and Example 1 is that: No modified hydroxyapatite ultra-long nanowires were added to the raw materials.
[0054] Comparative Example 2: The difference between this embodiment and embodiment 1 is that: The modified hydroxyapatite ultra-long nanowires are replaced by silica whiskers of equal mass in the raw materials, and the average length of the silica whiskers is 100 μm and the average diameter is 10 nm.
[0055] Comparative Example 3: The difference between this embodiment and embodiment 1 is that: No water-based polyurethane emulsion and thickener are added to the raw materials.
[0056] Performance testing 1. Adhesion test The coatings were prepared by the methods of Examples 1-6 and Comparative Examples 1-3, respectively, and the adhesion level was tested by the circle method of GB / T1720, and the data were recorded.
[0057] 2. Weather resistance test The coatings were prepared by the methods of Examples 1-6 and Comparative Examples 1-2, respectively, and the weather resistance was tested according to GB / T1767 for 24 months, and then the grade was evaluated; The grade standards are as follows: the sum of the blistering area, the peeling area, the color and gloss loss area ≤1% is Grade 1; the sum of the blistering area, the peeling area, the color and gloss loss area 1%<X≤10% is Grade 2; the sum of the blistering area, the peeling area, the color and gloss loss area 10%<X≤30% is Grade 3; the sum of the blistering area, the peeling area, the color and gloss loss area 30%<X≤60% is Grade 4; the sum of the blistering area, the peeling area, the color and gloss loss area 60%<X is Grade 5.
[0058] 3. Corrosion resistance test The coatings were prepared by the methods of Examples 1-6 and Comparative Examples 1-2, and the neutral salt spray resistance was tested with reference to GB / T1771. After 2400 hours, the total blistering area and rusting area were calculated.
[0059] 4. Wear resistance test The coatings were prepared by the methods of Examples 1-3, 5 and Comparative Example 1, respectively, and polished at 1000 revolutions according to GB / T1770, and the abrasion mass was recorded.
[0060] 5. Flexibility test The coatings were prepared by the methods of Examples 1-6 and Comparative Examples 1-3, respectively, and the flexibility was tested with reference to GB / T1731, and the reticulation, cracks, and peeling areas were recorded.
[0061] For the above test items, except for the coating samples in the embodiments or comparative examples, the other conditions are the same and follow the single variable principle.
[0062] Table 1 Performance test table It can be seen from Examples 1-3 and Table 1 that the coating has the advantages of high adhesion, strong corrosion resistance, good weather resistance, good wear resistance and flexibility.
[0063] Combining Example 1 and Examples 4-5 and Table 1, it can be seen that the filler of Example 4 is silica whisker. Compared with Example 1, the coating prepared in Example 4 has worse adhesion and weather resistance than Example 1, the total of the blistering area and the rusting area of corrosion is greater than that of Example 1, and the total of the reticulation, crack and peeling area of flexibility is greater than that of Example 1; this indicates that triethyl citrate, polyethylene glycol-modified alumina fiber and silicone-modified graphene are combined, and the plasticizing effect of triethyl citrate and polyethylene glycol is utilized, combined with the flexibility of alumina fiber and silicone, to further improve the weather resistance and corrosion resistance of the finished coating, and the flexibility is better.
[0064] In the filler of Example 5, the triethyl citrate modified silica whiskers are replaced by the same mass of silica whiskers, the polyethylene glycol modified alumina fibers are replaced by the same mass of alumina fibers, and the silicone modified graphene is replaced by the same mass of graphene. Compared with Example 1, the coating prepared in Example 5 has worse adhesion and weather resistance than Example 1, the total blistering area and rusting area of corrosion are greater than those of Example 1, the wear mass is greater than that of Example 1, and the sum of the reticulation, crack and peeling areas of flexibility is greater than that of Example 1. This indicates that the combination of triethyl citrate, polyethylene glycol and silicone can improve the crosslinking effect of silica whiskers, alumina fibers, graphene and aqueous fluorocarbon resin emulsions and aqueous polyurethane emulsions, thereby improving the structural density of the film layer formed by the coating, while improving the strength and flexibility as well as the wear resistance, weather resistance and corrosion resistance.
[0065] Combining Example 1 and Comparative Examples 1-3 and Table 1, it can be seen that no modified hydroxyapatite ultra-long nanowires are added to the raw materials of Comparative Example 1. Compared with Example 1, the coating prepared in Comparative Example 1 has worse adhesion than Example 1, worse weather resistance than Example 1, the total of the blistering area and the rusting area of corrosion is greater than that of Example 1, the wear quality is greater than that of Example 1, and the flexible mesh, crack, and peeling area are greater than that of Example 1; it indicates that the addition of modified hydroxyapatite ultra-long nanowires and the use of polyvinyl alcohol to improve the connection effect of hydroxyapatite ultra-long nanowires with aqueous fluorocarbon resin emulsion, aqueous polyurethane emulsion and filler are improved, thereby improving the wear resistance, corrosion resistance and weather resistance of the coating.
[0066] In Comparative Example 2, the modified hydroxyapatite ultra-long nanowires are replaced with silica whiskers of equal mass in the raw materials. Compared with Example 1, the coating prepared in Comparative Example 2 has worse adhesion and weather resistance than Example 1, the total of the blistering area and the rusting area of corrosion is greater than that of Example 1, and the total of the reticulation, cracks, and peeling areas of flexibility is greater than that of Example 1; this indicates that silica whiskers have higher strength and poorer flexibility, while the hydroxyapatite ultra-long nanowires have certain flexibility due to their longer length, which can improve the flexibility of the finished coating; and the modified hydroxyapatite ultra-long nanowires can be well cross-linked and bonded with the aqueous fluorocarbon resin emulsion and the aqueous polyurethane emulsion, while the ordinary silica whiskers and the aqueous fluorocarbon resin emulsion and the aqueous polyurethane emulsion only rely on the viscosity of the emulsion, thereby improving the weather resistance and corrosion resistance of the finished coating.
[0067] No water-based polyurethane emulsion and thickener were added to the raw materials of Comparative Example 3. Compared with Example 1, the adhesion of the coating prepared in Comparative Example 3 was worse than that in Example 1, and the reticulation, cracks, and peeling area of flexibility were greater than those in Example 1. This indicates that the combination of water-based polyurethane emulsion and thickener can improve the adhesion of the coating on the surface of the steel plate substrate, and utilize the good flexibility of the water-based polyurethane emulsion to further improve the flexibility of the film layer formed by the finished coating.
[0068] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A weather-resistant anticorrosive coating, characterized in that: The invention comprises the following raw materials in parts by weight: 80-100 parts of aqueous fluorocarbon resin emulsion, 20-30 parts of aqueous polyurethane emulsion, 5-10 parts of plasticizer, 10-20 parts of water, 10-20 parts of filler, 1-3 parts of defoamer, 1-3 parts of thickener, 0.5-2 parts of dispersant, 15-20 parts of curing agent, 1-2 parts of leveling agent and 1-3 parts of modified hydroxyapatite ultra-long nanowires.
2. The anti-corrosion coating with strong weather resistance according to claim 1, characterized in that: The filler consists of triethyl citrate modified silica whiskers, polyethylene glycol modified alumina fibers and silicone modified graphene in a mass ratio of 1:1-2:0.5-2.
3. The weather-resistant anticorrosive coating according to claim 2, characterized in that: The triethyl citrate modified silicon dioxide whisker is prepared from triethyl citrate, sodium carboxymethyl cellulose solution and silicon dioxide whisker in a mass ratio of 1:0.2-0.4:2-4.
4. The weather-resistant anticorrosive coating according to claim 3, characterized in that: The average length of the silicon dioxide whiskers is 10-100 μm.
5. The weather-resistant anticorrosive coating according to claim 2, characterized in that: The polyethylene glycol-modified alumina fiber is prepared from a polyethylene glycol aqueous solution and alumina fiber in a mass ratio of 1:1-3.
6. The weather-resistant anticorrosive coating according to claim 2, characterized in that: The silicone-modified graphene is prepared by bonding graphene to a sodium carboxymethyl cellulose solution and then bonding to a camphor extract, and finally loading silicone glue. The mass ratio of graphene, sodium carboxymethyl cellulose solution, camphor extract and silicone glue is 1:0.1-0.2:0.1-0.2:0.2-0.
5.
7. The weather-resistant anticorrosive coating according to claim 1, characterized in that: The modified hydroxyapatite ultra-long nanowires are prepared from a polyvinyl alcohol solution and hydroxyapatite ultra-long nanowires in a mass ratio of 1:1-2.
8. The weather-resistant anticorrosive coating according to claim 1, characterized in that: The plasticizer consists of methyl phthalate and chlorinated paraffin in a mass ratio of 1:0.1-0.
4.
9. The weather-resistant anticorrosive coating according to claim 1, characterized in that: The thickener is hydroxyethyl cellulose.
10. The method for preparing a weather-resistant anticorrosive coating according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1. Weigh the water-based fluorocarbon resin emulsion, the water-based polyurethane coating, and water, mix and stir evenly to obtain a primary mixture; S2, adding filler and modified hydroxyapatite ultra-long nanowires to the primary mixture, mixing and stirring evenly, and then adding plasticizer, thickener, defoamer, dispersant, and leveling agent, mixing and stirring evenly to obtain a mixture; S3. Add curing agent to the mixture, mix well, and obtain finished coating.
Citation Information
Patent Citations
Hydroxyapatite ultralong nanowire composite inflaming retarding and damping paint
CN105969196A
Fluorocarbon coating and preparation method thereof and coating method
CN110229601A
Preparation method and application of graphene fluorocarbon coating
CN117363112A
Self-crosslinking exterior wall coating containing reinforced fibers and preparation method of self-crosslinking exterior wall coating
CN117965071A
Wear-resistant coating as well as preparation method and application thereof
CN118325448A
Cited By
Multifunctional coating based on acrylic resin and production process thereof
CN120484589A
Multifunctional acrylic resin-based coating and process for its production
CN120484589B