Thermal insulation coating and application thereof

By applying heat-insulating coatings containing components such as silicon-aluminum-based ceramic hollow microbeads on the main chamber of the single crystal furnace, the problem of poor thermal insulation effect of the single crystal furnace is solved, and more efficient energy is achieved Retention and improvement in single crystal silicon rod quality.

CN118995040APending Publication Date: 2024-11-22QINGHAI GOKIN SOLAR TECH CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411272808.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The thermal insulation effect of single crystal furnaces is poor, resulting in waste of energy and degradation of the quality of single crystal silicon rods.

Method used

Provide a heat-insulating coating, containing components such as silicon-aluminum-based ceramic hollow microbeads, silicon nitride, potassium hexatitate whiskers, nanotitanium dioxide and aluminum trioxide. Water is used as a dispersion medium to form high temperature resistance and heat insulation. , heat insulation coating with excellent characteristics such as waterproofing and weather resistance, is applied on the furnace body and the surface of graphite parts of the main chamber of the single crystal furnace.

Benefits of technology

It significantly improves the insulation performance of the single crystal furnace, reduces the power consumption of the equipment, extends the service life, and improves the quality of the single crystal silicon rod.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a thermal insulation coating and application thereof. The thermal insulation coating is prepared from the following components in parts by weight: 10 to 15 parts of silicon-aluminum-based ceramic hollow microspheres, 5 to 15 parts of silicon nitride, 5 to 15 parts of potassium hexatitanate whiskers, 5 to 15 parts of titanium dioxide, 5 to 15 parts of aluminum oxide, 30 to 40 parts of film-forming emulsion and 5 to 10 parts of water. According to the invention, water is used as a dispersion medium, meanwhile, the types and dosages of the added components are synergistically designed, and special silicon-aluminum-based ceramic hollow microspheres and potassium hexatitanate whiskers are added, so that the obtained heat-insulating coating can form a heat-insulating coating with excellent characteristics of high temperature resistance, heat insulation, water resistance, weather resistance and the like after being cured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of coating materials, and in particular to a thermal insulation coating and application thereof. Background Art

[0002] In the process of using a single crystal furnace to produce single crystal silicon rods by the Czochraiski (CZ) method, heat is mainly lost from the side of the furnace body of the main chamber of the single crystal furnace, accounting for about 36.89% of the heat loss of the entire furnace body. The large amount of heat loss requires the heater to provide higher power. At present, in the production process of single crystal silicon rods, high heating power and low thermal insulation performance of existing single crystal furnaces not only cause a large amount of energy waste, but also the long-term high-temperature baking of the crucible by the heater will increase the silicon monoxide volatilized from the crucible, thereby affecting the quality of the single crystal silicon rod.

[0003] At present, the main chamber of the single crystal furnace is mainly made of stainless steel. Its structure is double-layer stainless steel, and there is no effective coating inside, which cannot provide good protection for the heat lost from the inside of the thermal field. Pure water is also passed between the two layers of stainless steel for cooling. Generally, when the single crystal furnace is running normally, the water inlet temperature of the main chamber furnace is 27°C, and the water outlet temperature is 31°C. The large temperature difference will inevitably take away a lot of heat, causing energy waste and reducing product quality. The 4°C temperature difference between the water inlet and the water outlet also shows that the thermal insulation performance of the thermal field in the existing single crystal furnace equipment is insufficient. Therefore, it is possible to consider using a coating with good thermal insulation performance to brush the main chamber furnace body and internal graphite parts of the thermal field to improve its thermal insulation performance, reduce equipment power consumption and improve the quality of single crystal products.

[0004] Based on this, how to provide a thermal insulation coating material suitable for the inner surface of the main chamber of the single crystal furnace and the outer surface of the internal graphite parts so that it can meet high thermal insulation requirements after the coating is formed is one of the technical problems that technical personnel in this field need to solve. Summary of the invention

[0005] The main purpose of the present invention is to provide a thermal insulation coating and its application to solve the problem of poor thermal insulation effect of the single crystal furnace thermal field in the prior art.

[0006] In order to achieve the above-mentioned purpose, the present invention provides a thermal insulation coating on the one hand, which includes, by weight: 10 to 15 parts of silicon-aluminum-based ceramic hollow microspheres, 5 to 15 parts of silicon nitride, 5 to 15 parts of potassium hexatitanate whiskers, 5 to 15 parts of titanium dioxide, 5 to 15 parts of aluminum oxide, 30 to 40 parts of film-forming emulsion and 5 to 10 parts of water.

[0007] Furthermore, the compressive strength of the silicon-aluminum-based ceramic hollow microspheres is 4000kg / cm 2 ~7000kg / cm 2, the thermal conductivity is 0.03W / (m·K)~0.12W / (m·K).

[0008] Furthermore, the particle size of the silicon-aluminum-based ceramic hollow microspheres is 50 μm to 100 μm.

[0009] Furthermore, the particle size ratio of the silicon-aluminum-based ceramic hollow microspheres to that of silicon nitride is (3-5):1.

[0010] Furthermore, the film-forming emulsion is a mixed emulsion of an organic silicone resin emulsion and an acrylic emulsion, and the weight ratio of the organic silicone resin emulsion to the acrylic emulsion is (0.8-1.2):1.

[0011] Furthermore, the mass concentration of the silicone resin emulsion is 4wt% to 5wt%, and the mass concentration of the acrylic emulsion is 50wt% to 55wt%.

[0012] Furthermore, the particle size of titanium dioxide is 20 μm to 50 μm, and the particle size of aluminum oxide is 10 μm to 30 μm.

[0013] Furthermore, the thermal insulation coating also includes one or more of a rheological agent, a dispersant, a wetting agent, a coupling agent and a defoaming agent; preferably, by weight, the rheological agent, the dispersant, the wetting agent, the coupling agent and the defoaming agent are each independently 1.0 to 1.2 parts in the thermal insulation coating.

[0014] Further, the thermal insulation coating comprises, by weight: 10 parts of silicon-aluminum-based ceramic hollow microspheres, 15 parts of silicon nitride, 15 parts of potassium hexatitanate whiskers, 10 parts of titanium dioxide, 10 parts of aluminum trioxide, 15 parts of silicone resin emulsion, 15 parts of acrylic emulsion, 5 parts of water, 1 part of rheological agent, 1 part of dispersant, 1 part of wetting agent, 1 part of coupling agent and 1 part of defoaming agent; or, by weight, the thermal insulation coating comprises: 15 parts of silicon-aluminum-based ceramic hollow microspheres, 5 parts of silicon nitride, 5 parts of potassium hexatitanate whiskers, 15 parts of titanium dioxide, 5 parts of aluminum trioxide Aluminum, 15 parts of silicone resin emulsion, 15 parts of acrylic emulsion, 10 parts of water, 1 part of rheological agent, 1 part of dispersant, 1 part of wetting agent, 1 part of coupling agent and 1 part of defoaming agent; or, by weight, the thermal insulation coating includes: 10 parts of silicon-aluminum-based ceramic hollow microspheres, 10 parts of silicon nitride, 10 parts of potassium hexatitanate whiskers, 5 parts of titanium dioxide, 15 parts of aluminum trioxide, 15 parts of silicone resin emulsion, 15 parts of acrylic emulsion, 5 parts of water, 1 part of rheological agent, 1 part of dispersant, 1 part of wetting agent, 1 part of coupling agent and 1 part of defoaming agent.

[0015] Another aspect of the present invention provides an application of the above-mentioned thermal insulation coating as a coating material on the inner surface of the furnace body of the main chamber of the thermal field of the single crystal furnace and / or the outer surface of the internal graphite parts.

[0016] By applying the technical solution of the present invention, water is used as the dispersion medium, and the types and amounts of components added therein are collaboratively designed, wherein special silicon-aluminum-based ceramic hollow microspheres and potassium hexatitanate whiskers are added, so that the obtained thermal insulation coating can form a thermal insulation coating with excellent properties such as high temperature resistance, heat insulation, waterproofness, and weather resistance after curing. DETAILED DESCRIPTION

[0017] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.

[0018] As described in the background technology, the thermal field of the single crystal furnace in the prior art has the problem of poor thermal insulation effect. In order to solve the above technical problems, the present invention provides a thermal insulation coating, which includes, by weight: 10 to 15 parts of silicon-aluminum-based ceramic hollow microspheres, 5 to 15 parts of silicon nitride, 5 to 15 parts of potassium hexatitanate whiskers, 5 to 15 parts of titanium dioxide, 5 to 15 parts of aluminum oxide, 30 to 40 parts of film-forming emulsion and 5 to 10 parts of water.

[0019] The present invention uses water as a dispersion medium and a mixture of a silicone resin emulsion and an acrylic emulsion as a film-forming substance, and the types and amounts of the components added therein are collaboratively designed, so that the obtained thermal insulation coating can form a thermal insulation coating with excellent properties such as high temperature resistance, heat insulation, waterproofness, and weather resistance after curing. Specifically: The introduction of silicon-aluminum-based ceramic hollow microspheres can not only enhance the thermal insulation performance of the coating formed after the coating is cured, but also improve the lightweight and crack resistance of the coating. Silicon nitride not only enhances the high temperature resistance of the obtained coating, but also improves its wear resistance and corrosion resistance. The use of potassium hexatitanate whiskers improves the mechanical strength and thermal shock resistance of the coating obtained by curing the coating, and its role in the coating is similar to the reinforcing role of steel bars in concrete. Nano-titanium dioxide and aluminum oxide are used as additives, which can be used to simultaneously construct a thermal radiation shielding layer with excellent performance when the coating is cured to form a coating. The film-forming emulsion is used to form a stable dispersion system.

[0020] In addition to the inherent advantages of each component as mentioned above and the performance optimization results they bring to the thermal insulation coating, what is more important is that the above components can cooperate with each other, thus forming an organic whole formula to form a coating material with excellent performance after curing, especially excellent thermal insulation.

[0021] In several preferred embodiments, the inventors have selected the compressive strength of the silicon-aluminum-based ceramic hollow microspheres to be 4000 kg / cm 2 ~7000kg / cm 2, so as to significantly improve the mechanical strength and wear resistance of the coating obtained by curing the thermal insulation coating, making it less likely to break or wear when subjected to external forces, and improving its thermal stability and durability. At the same time, its thermal conductivity is preferably 0.03W / (m·K)~0.12W / (m·K), so as to more effectively prevent the transfer of heat inside the final coating, thereby improving its thermal insulation effect. The main components of silicon-aluminum-based ceramic hollow microspheres are Al2O3 and SiO2.

[0022] Furthermore, in order to balance the mechanical properties and thermal insulation properties of the cured coating, the inventors have optimized the particle size of silicon-aluminum-based ceramic hollow microspheres to 50μm to 100μm after a large number of experiments, thereby obtaining a thermal insulation coating with better wear resistance and thermal insulation properties after curing, while also having higher durability and longer service life.

[0023] In several preferred embodiments, in order to further optimize the structural uniformity and continuity of the cured coating and improve its thermal insulation performance, the inventors have selected the particle size ratio of silicon-aluminum-based ceramic hollow microspheres to silicon nitride to be (3-5):1 after a large number of experiments. This is because the particle size ratio of the two will first affect the pore structure of the coating. Under this particle size relationship, the pore structure in the cured coating is more uniform, which is conducive to improving the thermal insulation performance. At the same time, under this particle size relationship, the mechanical properties and thermal stability of the obtained coating are also higher.

[0024] With respect to the film-forming emulsion in the thermal insulation coating formula provided by the present invention, in order to further meet the use requirements of the cured coating under high temperature and harsh environment, the film-forming emulsion is preferably a mixed emulsion of silicone resin emulsion and acrylic emulsion, and the weight ratio of silicone resin emulsion to acrylic emulsion is (0.8-1.2):1. The introduction of silicone resin provides good heat resistance and weather resistance for the cured coating, while acrylic emulsion enhances the flexibility and wear resistance of the coating. The two are mixed in the above ratio, which can more significantly optimize the stability and adhesion of the thermal insulation coating after curing.

[0025] On the basis of the above, the inventors further preferred the mass concentration of silicone resin emulsion to be 4wt% to 5wt% and the mass concentration of acrylic emulsion to be 50wt% to 55wt% through a large number of experiments, so as to achieve better compatibility between the two and form a more stable film-forming emulsion with better film-forming properties and higher adhesion of the coating obtained after film formation and curing.

[0026] In the thermal insulation coating formula provided by the present invention, nano titanium dioxide and aluminum oxide cooperate with each other to simultaneously form a thermal radiation shielding layer when the coating is cured. The inventor further prefers that the particle size of titanium dioxide is 20μm to 50μm, and the particle size of aluminum oxide is 10μm to 30μm, so as to more effectively exert their excellent heat resistance and high refractive index, reduce the direct impact of high temperature on the cured coating, thereby reducing heat energy loss and improving the thermal insulation effect. At the same time, the above-mentioned particle size range can also better make the two evenly dispersed in the thermal insulation coating.

[0027] Furthermore, the thermal insulation coating also includes one or more of a rheological agent, a dispersant, a wetting agent, a coupling agent and a defoaming agent. The addition of the above-mentioned additives can not only improve the preparation efficiency of the thermal insulation coating, but also improve its curing and film-forming properties. In several preferred embodiments, in order to further improve the comprehensive performance of the coating obtained after curing, the rheological agent, dispersant, wetting agent, coupling agent and defoaming agent are preferably 1.0 to 1.2 parts by weight each in the thermal insulation coating. Among them, the dispersant includes but is not limited to silica sol, the wetting agent includes but is not limited to X405, the coupling agent includes but is not limited to KH550, and the defoaming agent includes but is not limited to DF601.

[0028] In several preferred embodiments, the thermal insulation coating comprises, by weight: 10 parts of silicon-aluminum-based ceramic hollow microspheres, 15 parts of silicon nitride, 15 parts of potassium hexatitanate whiskers, 10 parts of titanium dioxide, 10 parts of aluminum trioxide, 15 parts of silicone resin emulsion, 15 parts of acrylic emulsion, 5 parts of water, 1 part of rheological agent, 1 part of dispersant, 1 part of wetting agent, 1 part of coupling agent and 1 part of defoaming agent; or, by weight, the thermal insulation coating comprises: 15 parts of silicon-aluminum-based ceramic hollow microspheres, 5 parts of silicon nitride, 5 parts of potassium hexatitanate whiskers, 15 parts of titanium dioxide, 5 parts of Aluminum oxide, 15 parts of silicone resin emulsion, 15 parts of acrylic emulsion, 10 parts of water, 1 part of rheological agent, 1 part of dispersant, 1 part of wetting agent, 1 part of coupling agent and 1 part of defoaming agent; or, by weight, the thermal insulation coating includes: 10 parts of silicon-aluminum-based ceramic hollow microspheres, 10 parts of silicon nitride, 10 parts of potassium hexatitanate whiskers, 5 parts of titanium dioxide, 15 parts of aluminum oxide, 15 parts of silicone resin emulsion, 15 parts of acrylic emulsion, 5 parts of water, 1 part of rheological agent, 1 part of dispersant, 1 part of wetting agent, 1 part of coupling agent and 1 part of defoaming agent. After a large number of experiments, the inventor optimized the dosage of the components of the thermal insulation coating and obtained these three specific formulas. It was found that the thermal insulation coating prepared with these three formulas can form a coating with a smoother appearance, lower thermal conductivity, higher adhesion and water resistance, and superior mechanical strength after curing.

[0029] Another aspect of the present invention provides an application of the above-mentioned thermal insulation coating as a coating material on the inner surface of the furnace body of the main chamber of the thermal field of the single crystal furnace and / or the outer surface of the internal graphite parts. After the thermal insulation coating obtained by the present invention is cured to form a coating, the corresponding coating exhibits excellent comprehensive performance, namely higher heat resistance, mechanical properties, adhesion and water resistance. Therefore, when it is applied as a coating material to the inner surface of the furnace body of the main chamber of the thermal field of the single crystal furnace and / or the outer surface of the internal graphite parts and cured to form a coating, it can effectively isolate high temperature, reduce heat energy loss, and can also enhance the mechanical strength and thermal shock resistance of the furnace body and the internal graphite parts, and extend their service life.

[0030] Furthermore, it is preferred that after the thermal insulation coating is cured to form a coating, the thickness of the resulting coating is 0.8 to 1.0 mm, so as to overcome the problems of insufficient thermal insulation protection due to too thin a coating and internal stress concentration due to too thick a coating, and achieve better thermal insulation effects and mechanical performance.

[0031] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0032] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0033] Example 1

[0034] A thermal insulation coating material:

[0035] 10 parts of silicon-aluminum-based ceramic hollow microspheres, 15 parts of silicon nitride, 15 parts of potassium hexatitanate whiskers, 10 parts of titanium dioxide, 10 parts of aluminum oxide, 15 parts of silicone resin emulsion, 15 parts of acrylic emulsion, 5 parts of water, 1 part of rheological agent silica sol, 1 part of dispersant JF890, 1 part of wetting agent X405, 1 part of coupling agent KH550 and 1 part of defoaming agent DF601 are mixed in proportion to obtain a thermal insulation coating material.

[0036] Among them, the compressive strength of silicon-aluminum-based ceramic hollow microspheres is 5000kg / cm 2 , thermal conductivity is 0.038W / (m·K), and the particle size is 100μm; the particle size of silicon nitride is 20μm (that is, the ratio of the particle size of silicon-aluminum-based ceramic hollow microspheres to that of silicon nitride is 5:1); the microscopic morphology of potassium hexatitanate whiskers is columnar single crystals; the particle size of titanium dioxide is 20μm, and the particle size of aluminum oxide is 10μm; the mass concentration of silicone resin emulsion is 4wt%; the mass concentration of acrylic emulsion is 50wt%.

[0037] Example 2

[0038] A thermal insulation coating material:

[0039] 15 parts of silica-alumina-based ceramic hollow microspheres, 5 parts of silicon nitride, 5 parts of potassium hexatitanate whiskers, 15 parts of titanium dioxide, 5 parts of aluminum oxide, 15 parts of silicone resin emulsion, 15 parts of acrylic emulsion, 10 parts of water, 1 part of rheological agent silica sol, 1 part of dispersant JF890, 1 part of wetting agent X405, 1 part of coupling agent KH550 and 1 part of defoaming agent DF601 are mixed in proportion to obtain a thermal insulation coating material.

[0040] The physicochemical properties of each component are the same as those in Example 1.

[0041] Example 3

[0042] A thermal insulation coating material:

[0043] 10 parts of silicon-aluminum-based ceramic hollow microspheres, 10 parts of silicon nitride, 10 parts of potassium hexatitanate whiskers, 5 parts of titanium dioxide, 15 parts of aluminum oxide, 15 parts of silicone resin emulsion, 15 parts of acrylic emulsion, 5 parts of water, 1 part of rheological agent silica sol, 1 part of dispersant JF890, 1 part of wetting agent X405, 1 part of coupling agent KH550 and 1 part of defoaming agent DF601 are mixed in proportion to obtain a thermal insulation coating material.

[0044] The physicochemical properties of each component are the same as those in Example 1.

[0045] Example 4

[0046] A thermal insulation coating material:

[0047] The difference between this embodiment and embodiment 1 is that the physical and chemical properties of the silicon-aluminum-based ceramic hollow microspheres used are different, specifically: the compressive strength is 3000kg / cm 2 , thermal conductivity is 0.02W / (m·K), particle size is 40μm. (At this time, the particle size ratio of silicon aluminum-based ceramic hollow microspheres to silicon nitride is 2:1).

[0048] Example 5

[0049] A thermal insulation coating material:

[0050] The difference between this embodiment and embodiment 1 is that the physical and chemical properties of the silicon-aluminum-based ceramic hollow microspheres used are different, specifically: the compressive strength is 8000kg / cm 2 , thermal conductivity is 0.15W / (m·K), particle size is 120μm. (At this time, the particle size ratio of silicon aluminum-based ceramic hollow microspheres to silicon nitride is 6:1).

[0051] Example 6

[0052] A thermal insulation coating material:

[0053] The only difference between this embodiment and embodiment 1 is that the particle size of titanium dioxide used is changed to 15 μm; the particle size of aluminum oxide used is changed to 35 μm.

[0054] Example 7

[0055] A thermal insulation coating material:

[0056] The only difference between this embodiment and embodiment 1 is that the particle size of titanium dioxide used is changed to 55 μm; the particle size of aluminum oxide used is changed to 5 μm.

[0057] Example 8

[0058] A thermal insulation coating material:

[0059] The only difference between this embodiment and embodiment 1 is that the mass concentration of the silicone resin emulsion used is changed to 3wt%, and the amount thereof is changed to 12 parts; the mass concentration of the acrylic emulsion used is changed to 60wt%, and the amount thereof is changed to 24 parts.

[0060] Example 9

[0061] A thermal insulation coating material:

[0062] The only difference between this embodiment and embodiment 1 is that the mass concentration of the silicone resin emulsion used is changed to 6wt%, and the amount thereof is changed to 21.6 parts; the mass concentration of the acrylic emulsion used is changed to 45wt%, and the amount thereof is changed to 14.4 parts.

[0063] Comparative Example 1

[0064] A thermal insulation coating material:

[0065] 8 parts of silica-alumina-based ceramic hollow microspheres, 3 parts of silicon nitride, 3 parts of potassium hexatitanate whiskers, 18 parts of titanium dioxide, 18 parts of aluminum oxide, 23 parts of silicone resin emulsion, 24 parts of acrylic emulsion, 3 parts of water, 1 part of rheological agent silica sol, 1 part of dispersant JF890, 1 part of wetting agent X405, 1 part of coupling agent KH550 and 1 part of defoaming agent DF601 are mixed in proportion to obtain a thermal insulation coating material.

[0066] The physicochemical properties of each component are the same as those in Example 1.

[0067] Comparative Example 2

[0068] A thermal insulation coating material:

[0069] 18 parts of silica-alumina-based ceramic hollow microspheres, 18 parts of silicon nitride, 18 parts of potassium hexatitanate whiskers, 3 parts of titanium dioxide, 3 parts of aluminum oxide, 11 parts of silicone resin emulsion, 11 parts of acrylic emulsion, 18 parts of water, 1 part of rheological agent silica sol, 1 part of dispersant JF890, 1 part of wetting agent X405, 1 part of coupling agent KH550 and 1 part of defoaming agent DF601 are mixed in proportion to obtain a thermal insulation coating material.

[0070] The physicochemical properties of each component are the same as those in Example 1.

[0071] Test Method

[0072] Thermal conductivity: According to GB / T 3651-2008 metal high temperature thermal conductivity measurement method.

[0073] Compressive strength: According to GB / T 7314-2005 metal material room temperature compression test method.

[0074] Adhesion: According to QJ 990.14-1986.

[0075] The coating materials obtained in each embodiment and comparative example were applied to the surface of a graphite plate with a size of 50 mm×50 mm to form a thermal insulation coating sample with a thickness of 1 mm. The above tests were performed on each of the formed coating samples, and the obtained performance data are shown in Table 1.

[0076] Table 1

[0077] Coating appearance <![CDATA[Thermal conductivity / [W·(m·K) -1 > Compressive strength / kPa Adhesion / MPa Water resistance Example 1 smooth 0.029 115 0.61 No change Example 2 smooth 0.031 112 0.72 No change Example 3 smooth 0.034 116 0.83 No change Example 4 smooth 0.028 110 0.57 No change Example 5 smooth 0.030 102 0.55 No change Example 6 smooth 0.032 109 0.59 No change Example 7 smooth 0.031 108 0.54 No change Example 8 smooth 0.035 110 0.52 No change Example 9 smooth 0.030 106 0.58 No change Comparative Example 1 Cracking \ \ \ \ Comparative Example 2 Relatively flat 0.037 95 0.48 A small amount of foaming

[0078] From the above description, it can be seen that the above-mentioned embodiments of the present invention realize the preparation of a coating composition with excellent performance. After the coating is formed, the obtained coating has a smooth appearance, excellent mechanical properties, water resistance and adhesion, and good thermal insulation performance.

[0079] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those described herein, for example.

[0080] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A thermal insulation coating, characterized in that: The thermal insulation coating comprises, by weight: 10 to 15 parts of silicon-aluminum-based ceramic hollow microspheres, 5 to 15 parts of silicon nitride, 5 to 15 parts of potassium hexatitanate whiskers, 5 to 15 parts of titanium dioxide, 5 to 15 parts of aluminum oxide, 30 to 40 parts of film-forming emulsion and 5 to 10 parts of water.

2. The thermal insulation coating according to claim 1, characterized in that: The compressive strength of the silicon-aluminum-based ceramic hollow microspheres is 4000kg / cm 2 ~7000kg / cm 2 , the thermal conductivity is 0.03W / (m·K)~0.12W / (m·K).

3. The thermal insulation coating according to claim 1 or 2, characterized in that: The particle size of the silicon-aluminum-based ceramic hollow microspheres is 50 μm to 100 μm.

4. The thermal insulation coating according to any one of claims 1 to 3, characterized in that: The particle size ratio of the silicon-aluminum-based ceramic hollow microspheres to the silicon nitride is (3-5):

1.

5. The thermal insulation coating according to any one of claims 1 to 4, characterized in that: The film-forming emulsion is a mixed emulsion of an organic silicone resin emulsion and an acrylic emulsion, and the weight ratio of the organic silicone resin emulsion to the acrylic emulsion is (0.8-1.2):

1.

6. The thermal insulation coating according to any one of claims 1 to 5, characterized in that: The mass concentration of the silicone resin emulsion is 4wt% to 5wt%, and the mass concentration of the acrylic emulsion is 50wt% to 55wt%.

7. The thermal insulation coating according to any one of claims 1 to 6, characterized in that: The particle size of the titanium dioxide is 20 μm to 50 μm, and the particle size of the aluminum oxide is 10 μm to 30 μm.

8. The thermal insulation coating according to any one of claims 1 to 7, characterized in that: The thermal insulation coating also includes one or more of a rheological agent, a dispersant, a wetting agent, a coupling agent and a defoaming agent; Preferably, in parts by weight, the rheological agent, the dispersant, the wetting agent, the coupling agent and the defoaming agent are each independently 1.0 to 1.2 parts in the thermal insulation coating.

9. The thermal insulation coating according to claim 8, characterized in that: In parts by weight, the thermal insulation coating comprises: 10 parts of the silicon-aluminum-based ceramic hollow microspheres, 15 parts of the silicon nitride, 15 parts of the potassium hexatitanate whiskers, 10 parts of the titanium dioxide, 10 parts of the aluminum oxide, 15 parts of the silicone resin emulsion, 15 parts of the acrylic emulsion, 5 parts of the water, 1 part of the rheological agent, 1 part of the dispersant, 1 part of the wetting agent, 1 part of the coupling agent and 1 part of the defoaming agent; or, In parts by weight, the thermal insulation coating comprises: 15 parts of the silicon-aluminum-based ceramic hollow microspheres, 5 parts of the silicon nitride, 5 parts of the potassium hexatitanate whiskers, 15 parts of the titanium dioxide, 5 parts of the aluminum oxide, 15 parts of the silicone resin emulsion, 15 parts of the acrylic emulsion, 10 parts of the water, 1 part of the rheological agent, 1 part of the dispersant, 1 part of the wetting agent, 1 part of the coupling agent and 1 part of the defoaming agent; or, In parts by weight, the thermal insulation coating includes: 10 parts of the silicon-aluminum-based ceramic hollow microspheres, 10 parts of the silicon nitride, 10 parts of the potassium hexatitanate whiskers, 5 parts of the titanium dioxide, 15 parts of the aluminum oxide, 15 parts of the silicone resin emulsion, 15 parts of the acrylic emulsion, 5 parts of the water, 1 part of the rheological agent, 1 part of the dispersant, 1 part of the wetting agent, 1 part of the coupling agent and 1 part of the defoaming agent.

10. Use of the thermal insulation coating according to any one of claims 1 to 9 as a coating material on the inner surface of a furnace body in a main chamber of a thermal field of a single crystal furnace and / or the outer surface of an internal graphite part.

Citation Information

Patent Citations

  • Nanometer high temperature resistant thermal insulation and prevention coating

    CN104231917A

  • Nano high-temperature-resistant heat-insulating coating

    CN108715731A

  • High-temperature-resistant fiber nano coating

    CN116676040A

  • Total-effect gel heat insulation coating and preparation method thereof

    CN117363060A

  • Single crystal furnace electrode sheath coating and preparation method thereof

    CN117924977A