Fracturing temporary plugging material and preparation method thereof

By preparing carbonate polyoxyethylene block copolymer and composite temporary blocking components, the problems of poor high temperature resistance and difficulty in degradation of traditional fracturing materials in high-temperature deep carbonate reservoirs are solved, and more efficient temporary Blocking effect and environmental protection performance.

CN118995162APending Publication Date: 2024-11-22SICHUAN CHUANQING UNDERGROUND TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410890765.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The poor high temperature resistance and difficulty in degradation of traditional fracturing temporary plugging materials in high-temperature deep carbonate reservoirs are difficult to meet the needs of deep fracturing and pose potential risks to the formation environment.

Method used

Carbonate polyoxyethylene block copolymer is prepared by polyoxyethylene large monomer and carbonate components, and the composite temporary blocking components are prepared by polymerization by combining acrylamide, acrylic acid and sodium alginate to form good temperature resistance, Degradable and environmentally friendly fracturing temporary plugging material.

Benefits of technology

Improve the temperature resistance and degradability of temporary plugging materials, enhance their stability and performance in high-temperature and high-salt environments, achieve a tighter temporary plug layer and better sealing effect, and also have good environmental protection performance. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004927452210000091
    Figure BDA0004927452210000091
  • Figure BDA0004927452210000092
    Figure BDA0004927452210000092
Patent Text Reader

Abstract

The invention relates to the technical field of fracture temporary plugging materials, in particular to a fracture temporary plugging material and a preparation method thereof.The fracture temporary plugging material is prepared by mixing a carbonate polyoxyethylene block copolymer and a composite temporary plugging component, and the carbonate polyoxyethylene block copolymer contains polyoxyethylene chain segments, so that the fracture temporary plugging material is prepared; according to the present invention, with the introduction of the carbonate chain segment, the chemical stability and the thermal stability of the copolymer can be enhanced so as to improve the temperature resistance and the chemical corrosion resistance of the temporary plugging material; the carbonate polyoxyethylene block copolymer is added into preparation of the temporary plugging material, bridging and thickening effects can be achieved, a tighter temporary plugging layer is formed, permeation of liquid or gas is reduced, the copolymer can form a stable gel structure in water more easily due to the hydrophilicity of polyoxyethylene chain segments, and the temporary plugging material is more stable in performance. The carbonic ester polyoxyethylene block copolymer has good degradability, and can play a very good role in environmental protection.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of temporary fracturing plugging materials, and in particular to a temporary fracturing plugging material and a preparation method thereof. Background Art

[0002] In the field of global oil and gas exploration and development, fracturing technology, as a key means of increasing production, is widely used to improve the development efficiency of low-permeability oil and gas reservoirs, especially in carbonate reservoirs. This type of reservoir accounts for a significant proportion of global oil and gas reserves and is also widely distributed in my country. However, carbonate reservoirs usually have the characteristics of high temperature, high pressure and complex fracture networks, which makes traditional fracturing technology face many challenges.

[0003] Temporary plugging materials play a vital role in the fracturing process. Temporary plugging materials are mainly used to temporarily plug the formed cracks during the fracturing process, build up pressure, and force the fractured cracks to extend to the unfractured area, thereby increasing the fracture network and improving the oil and gas recovery rate. However, traditional temporary plugging materials have many limitations in their application in high-temperature deep carbonate reservoirs, such as poor high temperature resistance and weak pressure resistance, which cannot meet the needs of deep fracturing.

[0004] In addition, with the enhancement of environmental awareness and the promotion of the concept of sustainable development, higher requirements have been put forward for the environmental protection of fracturing materials. Traditional temporary plugging materials are often difficult to degrade, posing potential risks to the formation environment. Therefore, how to develop a fracturing temporary plugging material with good high temperature resistance and easy degradation has become a technical problem that needs to be solved urgently by technicians in this field. Summary of the invention

[0005] Technical issues solved

[0006] In view of the above-mentioned shortcomings of the prior art, the present invention provides a temporary fracturing plugging material and a preparation method thereof, which can effectively solve the problems of the temporary plugging material in the prior art having poor high temperature resistance and being difficult to degrade.

[0007] Technical Solution

[0008] To achieve the above objectives, the present invention is implemented through the following technical solutions:

[0009] A method for preparing a temporary fracturing plugging material, the method comprising the following steps:

[0010] S1.1, preparing a carbonate polyoxyethylene block copolymer using a polyoxyethylene macromonomer component and a carbonate component as raw materials;

[0011] S1.2, preparing a composite temporary plugging component by polymerization using acrylamide, acrylic acid and sodium alginate as raw materials;

[0012] S1.3, weigh 30-35 parts of carbonate polyoxyethylene block copolymer, 35-40 parts of composite temporary plugging component, 10-15 parts of starch, 0.2-0.3 parts of aluminum nitrate, 0.3-0.5 parts of light calcium carbonate and 15-18 parts of deionized water according to weight parts, mix and stir at a stirring speed of 300r / min for 10min, the obtained mixture is recorded as mixed component;

[0013] S1.4. The mixed components are kneaded and granulated into particles with a particle size of 3-5 mm, and the particles are placed in an oven at 70°C and dried to constant weight to obtain the temporary plugging material for fracturing.

[0014] Furthermore, in S1.1, the preparation steps of the polyoxyethylene macromonomer component are:

[0015] S2.1. Add 2 g of sodium sulfadiazine into a reaction kettle, add 25 mL of ethylene oxide and 10 mL of tetrahydrofuran under argon protection, seal the kettle, heat to 70 ° C, stir at 100 r / min for 24-48 h, then add 2 mL of methacryloyl chloride, seal the kettle, heat to 50 ° C, stir at 100 r / min for 12 h, and the result is recorded as the reaction system;

[0016] S2.2. Pour the reaction system into 200 mL of ether to produce a white precipitate. The filtered precipitate component is extracted three times with chloroform and poured into 200 mL of ether again for precipitation. The filtered solid product is placed in a vacuum drying oven at 38°C and dried for 12 hours to obtain the polyoxyethylene macromonomer component.

[0017] Furthermore, the carbonate component is prepared by mixing dimethyl carbonate and diethyl carbonate in an equal weight ratio.

[0018] Furthermore, in S1.1, the preparation steps of the carbonate polyoxyethylene block copolymer are:

[0019] S5.1. Weigh 3 g of polyoxyethylene macromonomer component and 5 g of carbonate component and disperse them in 30 mL of tetrahydrofuran. Pour the mixture into a flask and add 15 mg of azobisisobutyronitrile under argon protection. Heat the mixture in an oil bath to 60°C and stir at a stirring speed of 150 r / min for 14-18 h. Add 2 mL of reaction termination component and record the result as reaction component. The reaction termination component is prepared by mixing hydroquinone and dioxane solution at a solid-liquid ratio of 1:20 g / mL.

[0020] S5.2. Pour the reaction components into 200 mL of methanol for precipitation. After filtration, obtain a solid crude product. Pour the crude product into 200 mL of methanol to extract and remove unreacted monomers. After filtration again, dry in an oven at 65°C for 24 hours to obtain a carbonate polyoxyethylene block copolymer.

[0021] Furthermore, in S1.2, the preparation steps of the composite temporary plugging component are:

[0022] S7.1. According to the molar ratio of acrylamide to acrylic acid of 1:1, an aqueous solution of acrylamide having a calculated concentration of 1.4 mol / L and an aqueous solution of acrylic acid having a neutralization degree of 70% are measured and mixed, and the result is recorded as a monomer component;

[0023] S7.2. Add 6% sodium alginate by weight to the monomer component, stir at a stirring speed of 200 r / min for 10 minutes, heat to 75°C and introduce nitrogen for 30 minutes, add 10% potassium persulfate solution with a mass fraction of 3% of the monomer component at a dropping rate of 1 drop / s, continue the constant temperature reaction for 3 hours, place in an oven at 60°C to dry to constant weight, grind through a 200-mesh sieve, and the result is the composite temporary plugging component.

[0024] A fracturing temporary plugging material is prepared by a method for preparing a fracturing temporary plugging material.

[0025] Beneficial Effects

[0026] The present invention provides a temporary fracturing plugging material and a preparation method thereof. Compared with the prior art, the present invention has the following beneficial effects:

[0027] 1. The present invention first prepares a polyoxyethylene macromonomer component by a ring-opening polymerization method, and then generates a carbonate polyoxyethylene block copolymer by a polymerization reaction between the polyoxyethylene macromonomer component and dimethyl carbonate and diethyl carbonate. The carbonate polyoxyethylene block copolymer contains a polyoxyethylene chain segment and has good hydrophilicity and flexibility, thereby improving the fluidity and wettability of the temporary plugging material. The introduction of the carbonate chain segment can enhance the chemical stability and thermal stability of the copolymer, thereby improving the temperature resistance and chemical corrosion resistance of the temporary plugging material. Secondly, the carbonate polyoxyethylene block copolymer is added to the preparation of the temporary plugging material, which can play a bridging and thickening role, thereby forming a tighter temporary plugging layer and reducing the penetration of liquid or gas. The hydrophilicity of the polyoxyethylene chain segment can make the copolymer easier to form a stable gel structure in water, further enhancing the temporary plugging effect. Finally, the carbonate polyoxyethylene block copolymer has good degradability, is easy to degrade, and can play an excellent environmental protection role.

[0028] 2. The present invention uses acrylamide, acrylic acid and sodium alginate as raw materials to prepare a composite temporary plugging component by a polymerization method. Acrylamide and acrylic acid have different active groups and can undergo a variety of chemical reactions to generate polymers with diverse structures and excellent performance. The introduction of sodium alginate provides the system with additional hydrophilicity and adsorption capacity, so that the composite temporary plugging component can still maintain good stability and performance under high temperature and high salt environment. The particle size of the polymer microspheres synthesized by the polymerization reaction can be controlled by adjusting the reaction conditions. At the same time, the polymer microspheres have good deformability and can adapt to pores of different sizes and shapes, thereby achieving effective plugging of cracks and pores; secondly, the hydrophilic groups in the composite temporary plugging component give it excellent swelling ability, which can absorb a large amount of water or liquid, thereby increasing the volume and enhancing the plugging effect. At the same time, the polymer microspheres have good dispersion stability and are not prone to precipitation or agglomeration, which is conducive to maintaining good rolling and migration capabilities in the reservoir channel; finally, the performance of the temporary plugging material can be further improved by adding carbonate polyoxyethylene block copolymers. This copolymer has good flexibility and elasticity, which can enhance the adhesion between the temporary plugging material and the pore wall, and improve the durability and reliability of the plugging. DETAILED DESCRIPTION

[0029] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] The present invention will be further described below in conjunction with the embodiments.

[0031] Example 1

[0032] A preparation method of a temporary fracturing plugging material according to this embodiment comprises the following steps:

[0033] S1.1, preparing a carbonate polyoxyethylene block copolymer using a polyoxyethylene macromonomer component and a carbonate component as raw materials;

[0034] S1.2, preparing a composite temporary plugging component by polymerization using acrylamide, acrylic acid and sodium alginate as raw materials;

[0035] S1.3, weigh 30 parts of carbonate polyoxyethylene block copolymer, 35 parts of composite temporary plugging component, 10 parts of starch, 0.2 parts of aluminum nitrate, 0.3 parts of light calcium carbonate and 15 parts of deionized water according to weight, mix and stir at a stirring speed of 300 r / min for 10 minutes, and the result is recorded as a mixed component;

[0036] S1.4. The mixed components are kneaded and granulated into particles with a particle size of 3 mm, and the particles are placed in an oven at 70°C and dried to constant weight to obtain temporary plugging material for fracturing.

[0037] In S1.1, the steps for preparing the polyoxyethylene macromonomer component are:

[0038] S2.1. Add 2 g of sodium sulfadiazine into a reaction kettle, add 25 mL of ethylene oxide and 10 mL of tetrahydrofuran under argon protection, seal the kettle, heat to 70 ° C, stir at 100 r / min for 24 h, then add 2 mL of methacryloyl chloride, seal the kettle, heat to 50 ° C, stir at 100 r / min for 12 h, and the result is recorded as the reaction system;

[0039] S2.2. Pour the reaction system into 200 mL of ether to produce a white precipitate. The filtered precipitate component is extracted three times with chloroform and poured into 200 mL of ether again for precipitation. The filtered solid product is placed in a vacuum drying oven at 38°C and dried for 12 hours to obtain the polyoxyethylene macromonomer component.

[0040] The carbonate component is prepared by mixing dimethyl carbonate and diethyl carbonate in an equal weight ratio.

[0041] In S1.1, the preparation steps of the carbonate polyoxyethylene block copolymer are:

[0042] S5.1. Weigh 3 g of polyoxyethylene macromonomer component and 5 g of carbonate component and disperse them in 30 mL of tetrahydrofuran. Pour the mixture into a flask and add 15 mg of azobisisobutyronitrile under argon protection. Heat the mixture in an oil bath to 60°C and stir at a stirring speed of 150 r / min for 14 h. Add 2 mL of reaction termination component and record the result as reaction component. The reaction termination component is prepared by mixing hydroquinone and dioxane solution at a solid-liquid ratio of 1:20 g / mL.

[0043] S5.2. Pour the reaction components into 200 mL of methanol for precipitation. After filtration, obtain a solid crude product. Pour the crude product into 200 mL of methanol to extract and remove unreacted monomers. After filtration again, dry in an oven at 65°C for 24 hours to obtain a carbonate polyoxyethylene block copolymer.

[0044] In S1.2, the preparation steps of the composite temporary plugging component are:

[0045] S7.1. According to the molar ratio of acrylamide to acrylic acid of 1:1, an aqueous solution of acrylamide having a calculated concentration of 1.4 mol / L and an aqueous solution of acrylic acid having a neutralization degree of 70% are measured and mixed, and the result is recorded as a monomer component;

[0046] S7.2. Add 6% sodium alginate by weight to the monomer component, stir at a stirring speed of 200 r / min for 10 minutes, heat to 75°C and introduce nitrogen for 30 minutes, add 10% potassium persulfate solution with a mass fraction of 3% of the monomer component at a dropping rate of 1 drop / s, continue the constant temperature reaction for 3 hours, place in an oven at 60°C to dry to constant weight, grind through a 200-mesh sieve, and the result is the composite temporary plugging component.

[0047] A fracturing temporary plugging material is prepared by a method for preparing a fracturing temporary plugging material.

[0048] Example 2

[0049] A preparation method of a temporary fracturing plugging material according to this embodiment comprises the following steps:

[0050] S1.1, preparing a carbonate polyoxyethylene block copolymer using a polyoxyethylene macromonomer component and a carbonate component as raw materials;

[0051] S1.2, preparing a composite temporary plugging component by polymerization using acrylamide, acrylic acid and sodium alginate as raw materials;

[0052] S1.3, weigh 35 parts of carbonate polyoxyethylene block copolymer, 40 parts of composite temporary plugging component, 15 parts of starch, 0.3 parts of aluminum nitrate, 0.5 parts of light calcium carbonate and 18 parts of deionized water according to weight, mix and stir at a stirring speed of 300 r / min for 10 minutes, and the obtained mixture is recorded as a mixed component;

[0053] S1.4. The mixed components are kneaded and granulated into particles with a particle size of 5 mm, and the particles are placed in an oven at 70°C and dried to constant weight to obtain temporary fracturing plugging materials.

[0054] In S1.1, the steps for preparing the polyoxyethylene macromonomer component are:

[0055] S2.1. Add 2 g of sodium sulfadiazine into a reaction kettle, add 25 mL of ethylene oxide and 10 mL of tetrahydrofuran under argon protection, seal the kettle, heat to 70 ° C, stir at 100 r / min for 48 h, then add 2 mL of methacryloyl chloride, seal the kettle, heat to 50 ° C, stir at 100 r / min for 12 h, and the result is recorded as the reaction system;

[0056] S2.2. Pour the reaction system into 200 mL of ether to produce a white precipitate. The filtered precipitate component is extracted three times with chloroform and poured into 200 mL of ether again for precipitation. The filtered solid product is placed in a vacuum drying oven at 38°C and dried for 12 hours to obtain the polyoxyethylene macromonomer component.

[0057] The carbonate component is prepared by mixing dimethyl carbonate and diethyl carbonate in an equal weight ratio.

[0058] In S1.1, the preparation steps of the carbonate polyoxyethylene block copolymer are:

[0059] S5.1. Weigh 3 g of polyoxyethylene macromonomer component and 5 g of carbonate component and disperse them in 30 mL of tetrahydrofuran. Pour the mixture into a flask and add 15 mg of azobisisobutyronitrile under argon protection. Heat the mixture in an oil bath to 60°C and stir at a stirring speed of 150 r / min for 18 h. Add 2 mL of reaction termination component and record the result as reaction component. The reaction termination component is prepared by mixing hydroquinone and dioxane solution at a solid-liquid ratio of 1:20 g / mL.

[0060] S5.2. Pour the reaction components into 200 mL of methanol for precipitation. After filtration, obtain a solid crude product. Pour the crude product into 200 mL of methanol to extract and remove unreacted monomers. After filtration again, dry in an oven at 65°C for 24 hours to obtain a carbonate polyoxyethylene block copolymer.

[0061] In S1.2, the preparation steps of the composite temporary plugging component are:

[0062] S7.1. According to the molar ratio of acrylamide to acrylic acid of 1:1, an aqueous solution of acrylamide having a calculated concentration of 1.4 mol / L and an aqueous solution of acrylic acid having a neutralization degree of 70% are measured and mixed, and the result is recorded as a monomer component;

[0063] S7.2. Add 6% sodium alginate by weight to the monomer component, stir at a stirring speed of 200 r / min for 10 minutes, heat to 75°C and introduce nitrogen for 30 minutes, add 10% potassium persulfate solution with a mass fraction of 3% of the monomer component at a dropping rate of 1 drop / s, continue the constant temperature reaction for 3 hours, place in an oven at 60°C to dry to constant weight, grind through a 200-mesh sieve, and the result is the composite temporary plugging component.

[0064] A fracturing temporary plugging material is prepared by a method for preparing a fracturing temporary plugging material.

[0065] Example 3

[0066] A preparation method of a temporary fracturing plugging material according to this embodiment comprises the following steps:

[0067] S1.1, preparing a carbonate polyoxyethylene block copolymer using a polyoxyethylene macromonomer component and a carbonate component as raw materials;

[0068] S1.2, preparing a composite temporary plugging component by polymerization using acrylamide, acrylic acid and sodium alginate as raw materials;

[0069] S1.3, weigh 33 parts of carbonate polyoxyethylene block copolymer, 38 parts of composite temporary plugging component, 13 parts of starch, 0.2 parts of aluminum nitrate, 0.4 parts of light calcium carbonate and 17 parts of deionized water according to weight, mix and stir at a stirring speed of 300 r / min for 10 minutes, and the result is recorded as a mixed component;

[0070] S1.4. The mixed components are kneaded and granulated into particles with a particle size of 4 mm, and the particles are placed in an oven at 70°C and dried to constant weight to obtain temporary plugging material for fracturing.

[0071] In S1.1, the steps for preparing the polyoxyethylene macromonomer component are:

[0072] S2.1. Add 2 g of sulfadiazine sodium into a reaction kettle, add 25 mL of ethylene oxide and 10 mL of tetrahydrofuran under argon protection, seal the kettle, heat to 70 ° C, stir at 100 r / min for 36 h, then add 2 mL of methacryloyl chloride, seal the kettle, heat to 50 ° C, stir at 100 r / min for 12 h, and the result is recorded as the reaction system;

[0073] S2.2. Pour the reaction system into 200 mL of ether to produce a white precipitate. The filtered precipitate component is extracted three times with chloroform and poured into 200 mL of ether again for precipitation. The filtered solid product is placed in a vacuum drying oven at 38°C and dried for 12 hours to obtain the polyoxyethylene macromonomer component.

[0074] The carbonate component is prepared by mixing dimethyl carbonate and diethyl carbonate in an equal weight ratio.

[0075] In S1.1, the preparation steps of the carbonate polyoxyethylene block copolymer are:

[0076] S5.1. Weigh 3 g of polyoxyethylene macromonomer component and 5 g of carbonate component and disperse them in 30 mL of tetrahydrofuran. Pour the mixture into a flask and add 15 mg of azobisisobutyronitrile under argon protection. Heat the mixture in an oil bath to 60°C and stir at a stirring speed of 150 r / min for 16 h. Add 2 mL of reaction termination component and record the result as reaction component. The reaction termination component is prepared by mixing hydroquinone and dioxane solution at a solid-liquid ratio of 1:20 g / mL.

[0077] S5.2. Pour the reaction components into 200 mL of methanol for precipitation. After filtration, obtain a solid crude product. Pour the crude product into 200 mL of methanol to extract and remove unreacted monomers. After filtration again, dry in an oven at 65°C for 24 hours to obtain a carbonate polyoxyethylene block copolymer.

[0078] In S1.2, the preparation steps of the composite temporary plugging component are:

[0079] S7.1. According to the molar ratio of acrylamide to acrylic acid of 1:1, an aqueous solution of acrylamide having a calculated concentration of 1.4 mol / L and an aqueous solution of acrylic acid having a neutralization degree of 70% are measured and mixed, and the result is recorded as a monomer component;

[0080] S7.2. Add 6% sodium alginate by weight to the monomer component, stir at a stirring speed of 200 r / min for 10 minutes, heat to 75°C and introduce nitrogen for 30 minutes, add 10% potassium persulfate solution with a mass fraction of 3% of the monomer component at a dropping rate of 1 drop / s, continue the constant temperature reaction for 3 hours, place in an oven at 60°C to dry to constant weight, grind through a 200-mesh sieve, and the result is the composite temporary plugging component.

[0081] A fracturing temporary plugging material is prepared by a method for preparing a fracturing temporary plugging material.

[0082] Comparative Example 1

[0083] The fracturing temporary plugging material and the preparation method thereof provided in this comparative example are substantially the same as those in Example 1, with the main difference being that in this comparative example 1, the carbonate polyoxyethylene block copolymer in Example 1 is replaced by the composite temporary plugging component in Example 1.

[0084] Comparative Example 2

[0085] The fracturing temporary plugging material and the preparation method thereof provided in this comparative example are substantially the same as those in Example 1, with the main difference being that in this comparative example 2, the composite temporary plugging component in Example 1 is replaced with the carbonate polyoxyethylene block copolymer in Example 1.

[0086] Performance Testing

[0087] The temporary fracturing plugging materials in Examples 1-3 and Comparative Examples 1-2 are marked as Example 1, Example 2, Example 3, Comparative Example 1 and Comparative Example 2, respectively. Then, the performance of Examples 1-3 and Comparative Examples 1-2 is tested. The specific test items and test methods are as follows:

[0088] 1. Weigh 0.2g of the temporary plugging materials for fracturing in Examples 1-3 and Comparative Examples 1-2 as samples, recorded as m0, put the samples into a 200-mesh non-woven bag, seal the bag mouth, weigh and record as m1, add 50mL of distilled water at different temperatures into a 100mL beaker, immerse the non-woven bag containing the samples in the solution, take it out once every 30 minutes, use dry filter paper to absorb the distilled water adsorbed on the non-woven bag, weigh and record as m2. Measure in this way until the absorption and swelling equilibrium is reached, and calculate the water absorption rate of the temporary plugging agent. The calculation method of the water absorption rate is (m2-m1) / m0×100%, and the water absorption rate at different temperatures is calculated. The obtained data is recorded in Table 1;

[0089] 2. The temporary plugging materials for fracturing in Examples 1-3 and Comparative Examples 1-2 were respectively placed in beakers filled with an appropriate amount of clean water and heated in a water bath at 80° C. until the temporary plugging materials for fracturing completely became fluid, i.e., completely degraded. The time taken at this point was recorded, i.e., the complete degradation time of the temporary plugging agent. The obtained data are recorded in Table 2;

[0090] 3. The temporary plugging rates of the temporary plugging materials for fracturing in Example 1-3 and Comparative Example 1-2 were tested, and the obtained data are recorded in Table 2.

[0091] Table 1

[0092]

[0093] Table 2

[0094]

[0095]

[0096] The data in the above table show that the water absorption rates of the temporary plugging materials in Examples 1-3 at different temperatures are higher than those in Comparative Examples 1-2, indicating that the carbonate polyoxyethylene block copolymer and the composite temporary plugging component can achieve better temporary plugging effects than a single component, and the temporary plugging rate of the temporary plugging materials in the present invention is higher, and the degradation rate is faster, which can achieve better environmental protection effects. In summary, the temporary plugging materials prepared by the present invention have excellent market promotion value and excellent application prospects.

[0097] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.

[0098] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a temporary fracturing plugging material, characterized in that: The preparation method comprises the following steps: S1.1, preparing a carbonate polyoxyethylene block copolymer using a polyoxyethylene macromonomer component and a carbonate component as raw materials; S1.2, preparing a composite temporary plugging component by polymerization using acrylamide, acrylic acid and sodium alginate as raw materials; S1.3, weigh 30-35 parts of carbonate polyoxyethylene block copolymer, 35-40 parts of composite temporary plugging component, 10-15 parts of starch, 0.2-0.3 parts of aluminum nitrate, 0.3-0.5 parts of light calcium carbonate and 15-18 parts of deionized water according to weight parts, mix and disperse, and the obtained mixture is recorded as mixed component; S1.

4. The mixed components are kneaded and granulated to prepare granules, and the obtained granules after drying are the temporary plugging material for fracturing.

2. The method for preparing a temporary fracturing plugging material according to claim 1, characterized in that: In S1.1, the steps for preparing the polyoxyethylene macromonomer component are: S2.

1. Add 2 g of sulfadiazine sodium into a reaction kettle, add 25 mL of ethylene oxide and 10 mL of tetrahydrofuran under argon protection, seal and heat to 70°C and stir to react for 24-48 h, then add 2 mL of methacryloyl chloride, seal and heat to 50°C and stir to react for 12 h, the result is recorded as the reaction system; S2.

2. Pour the reaction system into 200 mL of ether to produce a white precipitate. The filtered precipitate component is extracted three times with chloroform and poured into 200 mL of ether again for precipitation. The solid product after filtration is dried to obtain the polyoxyethylene macromonomer component.

3. The method for preparing a temporary fracturing plugging material according to claim 2, characterized in that: In S2.1, the stirring speed of the stirring reaction is 100 r / min. In S2.2, the drying method is to place it in a vacuum drying oven at 38° C. and dry it for 12 hours.

4. The method for preparing a temporary fracturing plugging material according to claim 1, characterized in that: The carbonate component is prepared by mixing dimethyl carbonate and diethyl carbonate in an equal weight ratio.

5. The method for preparing a temporary fracturing plugging material according to claim 1, characterized in that: In S1.1, the preparation steps of the carbonate polyoxyethylene block copolymer are: S5.

1. Weigh 3 g of the polyoxyethylene macromonomer component and 5 g of the carbonate component and disperse them in 30 mL of tetrahydrofuran. Pour the mixture into a flask and add 15 mg of azobisisobutyronitrile under argon protection. Heat the mixture in an oil bath to 60°C and stir to react for 14-18 h. Add 2 mL of the reaction termination component and the result is recorded as the reaction component. S5.

2. Pour the reaction components into 200 mL of methanol for precipitation, and obtain a solid crude product after filtration. Pour the crude product into 200 mL of methanol to extract and remove unreacted monomers, and then filter again and dry to obtain a carbonate polyoxyethylene block copolymer.

6. The method for preparing a temporary fracturing plugging material according to claim 5, characterized in that: In S5.1, the stirring speed of the stirring reaction is 150 r / min, the reaction termination component is prepared by mixing hydroquinone and dioxane solution in a solid-liquid ratio of 1:20 g / mL, and in S5.2, the drying method is to place it in an oven at 65°C and dry it for 24 hours.

7. The method for preparing a temporary fracturing plugging material according to claim 1, characterized in that: In S1.2, the preparation steps of the composite temporary plugging component are: S7.

1. According to the molar ratio of acrylamide to acrylic acid of 1:1, an aqueous solution of acrylamide having a calculated concentration of 1.4 mol / L and an aqueous solution of acrylic acid having a neutralization degree of 70% are measured and mixed, and the result is recorded as a monomer component; S7.

2. Add 6% by weight of sodium alginate to the monomer component, stir evenly, heat to 75°C and introduce nitrogen for 30 minutes, dropwise add 3% by weight of potassium persulfate solution of the monomer component, continue the constant temperature reaction for 3 hours, then place in an oven at 60°C and dry to constant weight, grind through a 200-mesh sieve, and the obtained product is the composite temporary plugging component.

8. The method for preparing a temporary fracturing plugging material according to claim 7, characterized in that: In S7.2, the uniform stirring operation is to stir at a stirring speed of 200 r / min for 10 min, the mass fraction of the potassium persulfate solution is 10%, and the dropping rate is 1 drop / s.

9. The method for preparing a temporary fracturing plugging material according to claim 1, characterized in that: In S1.3, the mixing and dispersing method is to stir at a stirring speed of 300 r / min for 10 minutes. In S1.4, the particle size of the particles is 3-5 mm, and the drying method is to place them in an oven at 70° C. and dry them to constant weight.

10. A temporary fracturing plugging material, characterized in that: The material is prepared by the method for preparing a temporary fracturing plugging material according to any one of claims 1 to 9.